Modified large crystal USY zeolite for hydrocracking hydrocarbon oil

The FS-USY catalyst, formed by using ultra-stable Y-type zeolite substituted with zirconium, titanium, or hafnium, solves the problem of low efficiency of existing catalysts in heavy hydrocarbon oil processing, achieving higher hydrocarbon oil conversion rate and naphtha selectivity.

CN116507416BActive Publication Date: 2024-11-05SAUDI ARABIAN OIL CO +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080105098.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2020-10-30
Publication Date
2024-11-05
Estimated Expiration
2040-10-30

AI Technical Summary

Technical Problem

Existing hydrocracking catalysts are inefficient when processing heavy hydrocarbon oils, making it difficult to effectively decompose large molecules and improve the economic value of hydrocarbon oils.

Method used

Using zirconium, titanium or hafnium-substituted ultrastable Y-type zeolite (FS-USY) as a catalyst support, FS-USY zeolite with an average crystallite size of 5 μm to 50 μm is formed through a specific preparation method, and then combined with hydride metal components to form a highly efficient hydrocracking catalyst.

Benefits of technology

It improved the efficiency of the hydrocracking process, increased the conversion rate of hydrocarbon oil and the selectivity of naphtha, while reducing the yield of middle distillate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116507416B_ABST
    Figure CN116507416B_ABST
Patent Text Reader

Abstract

According to one or more embodiments of the present disclosure, the catalyst composition includes a catalyst support and at least one hydrogenation component arranged on the catalyst support. The catalyst support includes at least one USY zeolite having a framework substituted with titanium and / or zirconium and / or hafnium. The average crystallite size of the framework-substituted USY zeolite is 5 μm to 50 μm. A method for preparing and using such a catalyst in a hydrocracking process is also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. application serial number 17 / 038,074, filed on September 30, 2020, the entire contents of which are incorporated herein by reference. Technical Field

[0003] Embodiments of the present disclosure relate generally to the hydrocracking of hydrocarbon oils, and particularly to catalyst compositions for the hydrocracking of hydrocarbon oils, methods of making these catalyst compositions, and methods of using these catalyst compositions. Background Art

[0004] A large number of refineries commercially use the hydrocracking process to process a variety of hydrocarbon feeds that boil in the range of 370°C to 520°C in conventional hydrocracking units and boil at 520°C and above in residue hydrocracking units. In general, the hydrocracking process breaks down the molecules of the hydrocarbon feed into smaller, i.e., lighter molecules that have a higher average volatility and economic value. In addition, the hydrocracking process generally improves the quality of the hydrocarbon feedstock by increasing the hydrogen-to-carbon ratio and by removing organic sulfur and organic nitrogen compounds. The hydrocracking catalyst is a key feature of the hydrocracking process technology.

[0005] There are two types of catalysts used in hydrocracking: pretreatment catalysts and cracking catalysts. Pretreatment catalysts are designed to remove pollutants such as sulfur and nitrogen from heavy hydrocarbon oils. Cracking catalysts are designed to decompose low-value heavy molecules into high-value transportation fuels. Cracking catalysts are generally composed of active phase metals for hydrogenation, an amorphous support as a binder, and zeolites as cracking components. Active phase metals generally include nickel, molybdenum, and tungsten. Exemplary zeolites include ultrastable Y-type zeolites (USY zeolites). Summary of the invention

[0006] There is a continuing need for more efficient hydrocracking catalyst compositions. It has been discovered that a catalyst composition comprising at least one ultrastable Y-type (hereinafter referred to as "USY") zeolite framework substituted with titanium, zirconium, hafnium, or a combination of two or more thereof, and having an average crystallite size of 5 μm to 50 μm can greatly improve the effectiveness of the hydrocracking process.

[0007] According to one embodiment, the catalyst composition includes at least one hydrogenation metal component and a support. The support comprises a framework-substituted ultrastable Y-type (USY) zeolite substituted with zirconium atoms, titanium ions, or both zirconium atoms and titanium atoms. The average crystallite size of the framework-substituted USY zeolite is 5 μm to 50 μm.

[0008] According to one embodiment, a method for preparing a catalyst composition includes forming an ultrastable Y-type (USY) zeolite having an average crystallite size of 5 μm to 50 μm; heating the USY zeolite at a temperature of 500°C to 700°C; forming a suspension comprising the USY zeolite, the liquid / solid ratio of the suspension being 5 to 15; adding at least one inorganic acid, at least one organic acid, or a mixture of at least one inorganic acid and at least one organic acid to the suspension so that the pH of the suspension is less than or equal to 2; mixing a zirconium compound, a titanium compound, a hafnium compound, or a mixture of two or more thereof with the suspension having a pH less than or equal to 2; and adding a base so that the pH of the suspension is 6 to 8 to obtain a framework-substituted USY zeolite.

[0009] According to one embodiment, a method for hydrocracking a hydrocarbon oil comprises contacting the hydrocarbon oil with at least one catalyst composition and hydrogen in a reactor to hydrocracking the hydrocarbon oil. The catalyst composition comprises at least one hydrogenation metal component and a carrier. The carrier comprises a framework-substituted ultrastable Y-type (USY) zeolite substituted with zirconium atoms, titanium ions, or both zirconium atoms and titanium atoms. The average crystallite size of the framework-substituted USY zeolite is 5 μm to 50 μm.

[0010] Additional features and advantages of the embodiments described herein will be set forth in the detailed description which follows, and in part will be apparent to those skilled in the art from that description or may be learned by practicing the described embodiments, including the detailed description and claims provided below. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] The following detailed description of specific embodiments of the present disclosure may be best understood when read in conjunction with the following drawings, in which:

[0012] Figure 1 depicts a SEM image of a conventionally sized NaY zeolite at 10,000x magnification;

[0013] Figure 2 depicts a SEM image of a large crystal NaY zeolite at 10,000 times magnification according to one or more embodiments of the present disclosure;

[0014] Figure 3 depicts a SEM image of a conventionally sized NaY zeolite at 30,000x magnification;

[0015] Figure 4 depicts a SEM image of a large crystal NaY zeolite at 30,000 times magnification according to one or more embodiments of the present disclosure;

[0016] Figure 5The crystallite size distribution curves of conventional sized NaY zeolite and large crystal NaY zeolite are depicted;

[0017] Figure 6 depicts a graph of VGO feed conversion versus reactor temperature; and

[0018] Figure 7 Middle distillate (MD) and naphtha selectivity versus VGO feed conversion are plotted. DETAILED DESCRIPTION

[0019] In an embodiment, the catalyst composition includes a catalyst support and at least one hydrogenation component arranged on the catalyst support. The catalyst support includes at least one USY zeolite having a framework substituted with titanium and / or zirconium and / or hafnium (hereinafter referred to as "FS-USY zeolite"). The average crystallite size of the FS-USY zeolite is 5 μm to 50 μm. The embodiment will now be described in more detail.

[0020] As used herein, the term "hydrocarbon oil" or "hydrocarbon feedstock" refers to an oil-containing liquid consisting primarily of a mixture of hydrocarbon compounds. Hydrocarbon oils may include refined oils obtained from crude oil, synthetic crude oil, asphalt, oil sands, shale oil or kerosene. The term "refined oil" includes, but is not limited to, vacuum gas oil (VGO), deasphalted oil (DAO) obtained from a solvent deasphalting process, demetallized oil (DMO), light and / or heavy coker gas oils obtained from a coking process, cycle oils obtained from a fluidized catalytic cracking (FCC) process, and gas oils obtained from a visbreaking process.

[0021] As used herein, the term "hydrocarbon" refers to a chemical compound composed entirely of carbon and hydrogen atoms.

[0022] As used herein, the term "lattice constant" refers to the physical dimensions of a unit cell in a crystal lattice. The lattice constant can be determined by ASTM D 3942-03, entitled "Standard Test Method for Determination of the Unit Cell Dimension of a Faujasite-Type Zeolite," the entire contents of which are incorporated herein by reference.

[0023] As used herein, the term "specific surface area" refers to the total surface area per unit mass of zeolite. The specific surface area can be measured by ASTM D3663-03 entitled "Standard Test Method for Surface Area of ​​Catalysts and Catalyst Carriers", the entire contents of which are incorporated herein by reference. Alternatively, the Brunauer-Emmett-Teller ("BET") model can be used to measure the specific surface area. Alternatively, the specific surface area can be measured by ASTM D 4365-19 entitled "Standard Test Method for Determining Micropore Volume and Zeolite Area of ​​a Catalyst", the entire contents of which are incorporated herein by reference.

[0024] As used herein, the term "hydrogen / oil ratio" or "hydrogen-oil ratio" refers to a standard measure of the volumetric rate of hydrogen circulating through a reactor relative to the volume of feed. The hydrogen / oil ratio can be determined by comparing the flow rate of the hydrogen stream to the flow rate of the hydrocarbon feed using a standard flow meter.

[0025] As used herein, the term "liquid space velocity" or "LHSV" refers to the ratio of the liquid flow rate of the hydrocarbon feed to the volume or mass of the catalyst.

[0026] As used herein, the term "catalyst activity" or "catalytic activity" refers to the rate increase of the hydrocracking process due to the presence of the catalyst and can be approximated by the temperature at which the feed conversion reaches 50%. More active catalysts will have lower such temperatures.

[0027] In one aspect, the catalyst composition may include a catalyst support and at least one hydrogenation component. In embodiments, the catalyst composition may include 60 wt % to 99.99 wt % of a support. For example, the catalyst composition may include 65 wt % to 95 wt %, 60 wt % to 90 wt %, 65 wt % to 85 wt % or even 70 wt % to 80 wt % of a support. It should be understood that the catalyst composition may include a support amount in a range formed from any lower limit of such a range as described herein to any upper limit of such a range as described herein. In embodiments, the catalyst composition may include 0.01 wt % to 40 wt % of a hydrogenation component. For example, the catalyst composition may include 1 wt % to 40 wt %, 5 wt % to 35 wt %, 10 wt % to 30 wt % or even 15 wt % to 25 wt % of a hydrogenation component. It should be understood that the catalyst composition may include an amount of hydrogenation component in a range formed from any lower limit of such a range as described herein to any upper limit of such a range as described herein. Without intending to be bound by any particular theory, it is believed that when the amount of hydrogenation component in the catalyst composition is too large relative to the amount of support, the dispersion of the hydrogenation metal on the catalyst is not optimal. For example, when the catalyst composition includes more than 40% by weight of the hydrogenation component, the hydrogenation metal may agglomerate on the support.

[0028] The catalyst carrier may include at least one USY zeolite, which may have a framework substituted with titanium and / or zirconium and / or hafnium. In an embodiment, the catalyst carrier may include 0.1 wt % to 90 wt % of FS-USY zeolite. For example, the catalyst carrier may include 0.1 wt % to 85 wt %, 5 wt % to 80 wt %, 10 wt % to 75 wt %, 15 wt % to 70 wt %, 20 wt % to 65 wt %, 25 wt % to 60 wt %, 30 wt % to 55 wt %, 35 wt % to 50 wt %, or even 40 wt % to 45 wt % of FS-USY zeolite. It should be understood that the catalyst carrier may include an amount of FS-USY zeolite in a range formed from any lower limit of such a range described herein to any upper limit of such a range described herein. It is not intended to be bound by any particular theory, and it is believed that when the amount of zeolite in the catalyst carrier is higher than 90%, the formation of catalyst particles / extrudates is limited.

[0029] In an embodiment, the framework substitution can be accomplished by a post-modification process, wherein the zeolite undergoes dealumination and then inserts a transition metal, such as Ti and / or Zr and / or Hf. As a result, the zeolite having a framework substituted with titanium and / or zirconium and / or hafnium can have a greater silica to alumina molar ratio (hereinafter referred to as "SAR") relative to an unsubstituted zeolite. Without intending to be bound by any particular theory, it is believed that this post-modification produces mesopores, which, as used herein, refer to pores with a diameter of 2nm to 50nm, which give the zeolite the ability to accept macromolecules in the pores. In addition, this post-modification process is believed to increase the number of moderate acid sites while reducing the number of strong acid sites and enhancing the dispersion of hydrogenation metals on the catalyst surface.

[0030] In an embodiment, the post-modification of USY zeolite can be completed by the following process. Zeolite can be placed in the form of a liquid suspension so that the mass ratio of liquid to solid zeolite is 5 to 15. Mineral acid or organic acid can be added to the suspension so that the pH of the suspension is less than 2. At least one zirconium compound and / or at least one titanium compound and / or at least one hafnium compound are added to the acidic suspension, which are then mixed and neutralized to obtain a post-modified catalyst. An exemplary process for preparing a USY zeolite framework substituted with titanium and / or zirconium and / or hafnium is described in U.S. Patent No. 10,293,332, the entire contents of which are incorporated herein by reference. Framework substitution can be monitored, for example, by ultraviolet, visible and near-infrared spectrophotometry (UV-Vis-NIR or UV-vis), Fourier transform infrared spectroscopy (FT-IR) or nuclear magnetic resonance spectroscopy (NMR).

[0031] In embodiments, the USY zeolite may be independently substituted with 0.1 wt % to 5 wt % zirconium and / or 0.1 wt % to 5 wt % titanium and / or 0.1 wt % to 5 wt % hafnium calculated as oxide. That is, in embodiments, although at least one of zirconium, titanium and hafnium is included, one or more of zirconium, titanium and hafnium may not be included. For example, the USY zeolite may be substituted with only zirconium, only titanium, only hafnium, both zirconium and titanium, both zirconium and hafnium, both titanium and hafnium, or all three of zirconium, titanium and hafnium.

[0032] In embodiments where zirconium is present, the USY zeolite may include 0.1 wt % to 5 wt % zirconium, 0.5 wt % to 4.5 wt % zirconium, 0.5 wt % to 4 wt % zirconium, 0.5 wt % to 3.5 wt % zirconium, 0.5 wt % to 3 wt % zirconium, 0.5 wt % to 2.5 wt % zirconium, 0.5 wt % to 2 wt % zirconium, 0.5 wt % to 1.5 wt % zirconium, 0.5 wt % to 1 wt % zirconium, 1 wt % to 4 wt % zirconium, 1 wt % to 3.5 wt % zirconium, 1 wt % to 3 wt % zirconium, 1 wt % to 2.5 wt % zirconium, or even 1 wt % to 2 wt % zirconium.

[0033] In the same or different embodiments, the USY zeolite can be substituted with 0.5 wt % to 4.5 wt % titanium, 0.5 wt % to 4 wt % titanium, 0.5 wt % to 3.5 wt % titanium, 0.5 wt % to 3 wt % titanium, 0.5 wt % to 2.5 wt % titanium, 0.5 wt % to 2 wt % titanium, 0.5 wt % to 1.5 wt % titanium, 0.5 wt % to 1 wt % titanium, 1 wt % to 4 wt % titanium, 1 wt % to 3.5 wt % titanium, 1 wt % to 3 wt % titanium, 1 wt % to 2.5 wt % titanium, or even 1 wt % to 2 wt % titanium.

[0034] In the same or different embodiments, the USY zeolite can be substituted with 0.5 wt % to 4.5 wt % hafnium, 0.5 wt % to 4 wt % hafnium, 0.5 wt % to 3.5 wt % hafnium, 0.5 wt % to 3 wt % hafnium, 0.5 wt % to 2.5 wt % hafnium, 0.5 wt % to 2 wt % hafnium, 0.5 wt % to 1.5 wt % hafnium, 0.5 wt % to 1 wt % hafnium, 1 wt % to 4 wt % hafnium, 1 wt % to 3.5 wt % hafnium, 1 wt % to 3 wt % hafnium, 1 wt % to 2.5 wt % hafnium, or even 1 wt % to 2 wt % hafnium.

[0035] It should be understood that any amount of zirconium substitution described herein can be used in combination with any amount of titanium substitution described herein and any amount of hafnium substitution described herein, including 0 wt % of any one or both of zirconium, titanium, and hafnium. In addition, it should be understood that ranges of zirconium substitution or titanium substitution or hafnium substitution can be formed by any lower limit of such substitution described herein and any upper limit of such substitution described herein.

[0036] Without intending to be bound by any particular theory, it is believed that the addition of zirconium compounds and / or titanium compounds and / or hafnium compounds in an amount less than 0.1 wt % does not improve the solid acid properties of the zeolite. In contrast, the addition of zirconium compounds and / or titanium compounds and / or hafnium compounds in an amount exceeding 5 wt % does not further improve the activity of the zeolite and may result in an unnecessary increase in the cost of the resulting catalyst.

[0037] In embodiments, the lattice constant of the FS-USY zeolite may be from 2.42 nm to 2.45 nm. For example, the lattice constant of the FS-USY zeolite may be from 2.42 nm to 2.449 nm, 2.42 nm to 2.448 nm, 2.42 nm to 2.447 nm, 2.42 nm to 2.446 nm, 2.42 nm to 2.445 nm, 2.42 nm to 2.444 nm, 2.42 nm to 2.443 nm, 2.42 nm to 2.442 nm, 2.42 nm to 2.441 nm, 2.42 nm to 2.444 nm, 2.42 nm to 2.447 nm, 2.42 nm to 2.448 nm, 2.42 nm to 2.449 ... 45nm, 2.434nm to 2.45nm, or even 2.435nm to 2.45nm. It should be understood that the lattice constant of the FS-USY zeolite can be within a range formed from any lower limit of such lattice constant described herein to any upper limit of such lattice constant described herein.

[0038] Without intending to be bound by any particular theory, it is believed that the lattice constant of FS-USY zeolite less than 2.42 nm may result in a reduction in the activity of the resulting hydrocracking catalyst. This reduction is believed to be due to the high SiO2 content in the USY zeolite framework. 2 / Al 2 O 3 The molar ratio and a small amount of solid acid sites serve as the result of hydrocarbon decomposition active sites. On the contrary, due to the low heat resistance of FS-USY zeolite, the lattice constant of FS-USY zeolite exceeding 2.45 nm may cause the crystal structure of FS-USY zeolite to be destroyed during the hydrocracking reaction. The destruction of the crystal structure of FS-USY zeolite may result in a decrease in the activity of the finally formed hydrocracking catalyst composition.

[0039] In an embodiment, the specific surface area of ​​FS-USY zeolite may be 600 m 2 / g to 900m 2 / g. For example, the specific surface area of ​​FS-USY can be 600m 2 / g to 890m 2 / g、600m 2 / g to 880m 2 / g、600m 2 / g to 870m 2 / g、600m 2 / g to 860m 2 / g、600m 2 / g to 850m 2 / g、600m 2 / g to 840m 2 / g、600m 2 / g to 830m 2 / g、600m 2 / g to 820m 2 / g、600m 2 / g to 810m 2 / g、600m 2 / g to 800m 2 / g, 610m 2 / g to 900m 2 / g, 620m 2 / g to 900m 2 / g, 630m 2 / g to 900m 2 / g, 640m 2 / g to 900m 2 / g, 650m 2 / g to 900m 2 / g, 660m 2 / g to 900m 2 / g, 670m 2 / g to 900m 2 / g, 680m 2 / g to 900m 2 / g, 690m 2 / g to 900m 2 / g, or even 700m 2 / g to 900m 2 / g. It should be understood that the specific surface area of ​​FS-USY zeolite can be within a range formed from any lower limit of such specific surface area described herein to any upper limit of such specific surface area described herein. Without intending to be bound by any particular theory, it is believed that less than 600 m 2 A specific surface area of ​​FS-USY zeolite of less than 100 Å / g may result in a reduction in the number of available solid acid sites, thereby lowering the catalyst activity of the resulting hydrocracking catalyst composition to an unsatisfactory level.

[0040] In an embodiment, the catalyst composition comprising FS-USY zeolite may have a specific surface area of ​​200 m 2 / g to 450m 2 For example, the specific surface area of ​​the catalyst composition comprising FS-USY zeolite may be 210 m 2 / g to 450m 2 / g, 220m 2 / g to 450m 2 / g, 230m 2 / g to 450m 2 / g, 240m 2 / g to 450m 2 / g, 250m 2 / g to 450m 2 / g, 200m 2 / g to 440m 2 / g, 200m 2 / g to 430m 2 / g, 200m 2 / g to 420m 2 / g, 200m 2 / g to 410m 2 / g, or even 200m 2 / g to 400m 2 / g. It should be understood that the specific surface area of ​​the catalyst composition comprising FS-USY zeolite can be within a range formed from any lower limit of such specific surface area described herein to any upper limit of such specific surface area described herein. Without intending to be bound by any particular theory, it is believed that when the specific surface area is less than 200 m 2 / g, the hydrocracking rate decreases and the yield of middle distillates decreases. However, if the specific surface area exceeds 450m 2 / g, the hydrocracking rate may increase too high and the product selectivity may change unfavorably.

[0041] In an embodiment, the SiO of FS-USY zeolite 2 With Al 2 O 3 The molar ratio of SiO to zeolite may be 5 to 100. For example, the SiO 2 With Al 2 O 3The molar ratio of may be 5 to 99, 5 to 98, 5 to 97, 5 to 96, 5 to 95, 5 to 94, 5 to 93, 5 to 92, 5 to 91, 5 to 90, 5 to 89, 5 to 88, 5 to 87, 5 to 86, 5 to 85, 5 to 84, 5 to 83, 5 to 82, 5 to 81, 5 to 80, 5 to 79, 5 to 78, 5 to 77, 5 to 76, 5 to 75, 5 to 74, 5 to 73, 5 to 72, 5 to 71, 5 to 70 , 5 to 69, 5 to 68, 5 to 67, 5 to 66, 5 to 65, 5 to 64, 5 to 63, 5 to 62, 5 to 61, 5 to 60, 5 to 59, 5 to 58, 5 to 57, 5 to 56, 5 to 55, 5 to 54, 5 to 53, 5 to 52, 5 to 51, 5 to 50, 5 to 49, 5 to 48, 5 to 47, 5 to 46, 5 to 45, 5 to 44, 5 to 43, 5 to 42, 5 to 41, 5 to 40, 6 to 10 0, 7 to 100, 8 to 100, 9 to 100, 10 to 100, 11 to 100, 12 to 100, 13 to 100, 14 to 100, 15 to 100, 16 to 100, 17 to 100, 18 to 100, 19 to 100, 20 to 100, 21 to 100, 22 to 100, 23 to 100, 24 to 100, 25 to 100, 26 to 100, 27 to 100, 28 to 100, 29 100, 30 to 100, 31 to 100, 32 to 100, 33 to 100, 34 to 100, 35 to 100, 36 to 100, 37 to 100, 38 to 100, 39 to 100, 40 to 100, 41 to 100, 42 to 100, 43 to 100, 44 to 100, 45 to 100, 46 to 100, 47 to 100, 48 to 100, 49 to 100, or even 50 to 100. It should be understood that the SiO of FS-USY zeolite 2 With Al 2 O 3 The ratio can be within a range formed from any lower limit of such ratio described herein to any upper limit of such ratio described herein.

[0042] Without intending to be bound by any particular theory, it is believed that a FS-USY zeolite having a silica-alumina molar ratio of less than 5 may have highly acidic sites with very high acid strength, thus easily leading to reduced hydrogenation and hydrocracking activities of the final hydrocracking catalyst formed. In addition, a greater alumina content is associated with a lower stability of FS-USY. Conversely, a FS-USY zeolite having a silica-alumina ratio exceeding 100 may lead to reduced hydrocracking activity of the final prepared hydrocracking catalyst in a decomposition reactor because a small number of solid acid sites are effective for hydrocracking.

[0043] In an embodiment, a catalyst composition comprising FS-USY zeolite may include a or smaller. These diameters are The pore volume of the present invention can be 0.4ml / g to 0.75ml / g or smaller. For example, the pore volume can be 0.4ml / g to 0.74ml / g, 0.4ml / g to 0.73ml / g, 0.4ml / g to 0.72ml / g, 0.4ml / g to 0.71ml / g, 0.4ml / g to 0.7ml / g, 0.4ml / g to 0.69ml / g, 0.4ml / g to 0.68ml / g, 0.4ml / g to 0.67ml / g, 0.4ml / g to 0.66ml / g, 0.4ml / g to 0.65ml / g, 0.41 0.42 ml / g to 0.75 ml / g, 0.43 ml / g to 0.75 ml / g, 0.44 ml / g to 0.75 ml / g, 0.45 ml / g to 0.75 ml / g, 0.46 ml / g to 0.75 ml / g, 0.47 ml / g to 0.75 ml / g, 0.48 ml / g to 0.75 ml / g, 0.49 ml / g to 0.75 ml / g, or even 0.5 ml / g to 0.75 ml / g. It should be understood that the range of diameters is The pore volume of the pores of the catalyst composition of FS-USY zeolite or smaller can be within a range formed from any lower limit of such pore volume described herein to any upper limit of such pore volume described herein.

[0044] Without intending to be bound by any particular theory, it is believed that if the pore volume is less than 0.40 ml / g, the specific surface area is reduced. As a result, the activity of the hydrocracking catalyst and the yield of the middle distillate are reduced. On the contrary, if the pore volume exceeds 0.75 ml / g, the specific surface area is increased. As a result, the hydrocracking rate and product selectivity may be adversely changed.

[0045] In embodiments, the catalyst composition may include other additives. For example, in addition to the above-mentioned zeolite, the catalyst composition may also include one or more inorganic oxides. The inorganic oxide may be used as a granulating agent or a binder. Exemplary inorganic oxides include, but are not limited to, aluminum oxide, silicon dioxide, titanium dioxide, silicon dioxide-alumina, aluminum oxide-titania, aluminum oxide-zirconia, aluminum oxide-boria, phosphorus-alumina, silicon dioxide-alumina-boria, phosphorus-alumina-boria, phosphorus-alumina-silicon dioxide, silicon dioxide-alumina-titania and silicon dioxide-alumina-zirconia.

[0046] In embodiments, one or more inorganic oxides can be components of catalyst carriers. In embodiments with both FS-USY zeolite and inorganic oxide, the FS-USY zeolite present can account for 1 wt % to 90 wt %, 1 wt % to 85 wt %, 1 wt % to 80 wt %, 10 wt % to 75 wt %, 20 wt % to 70 wt % or even 30 wt % to 60 wt % of the carrier. In such embodiments, the inorganic oxide content can account for 99 wt % to 10 wt %, 99 wt % to 15 wt %, 99 wt % to 20 wt %, 90 wt % to 25 wt %, 80 wt % to 30 wt % or even 70 wt % to 40 wt % of the carrier. It should be understood that FS-USY zeolite can be present in the range formed from any one lower limit of this concentration as described herein to any one upper limit of this concentration as described herein. It should be further understood that inorganic oxide can be present in the range formed from any one lower limit of this concentration as described herein to any one upper limit of this concentration as described herein. Without intending to be bound by any particular theory, it is believed that if the inorganic oxide content drops below 10 wt%, the catalyst may not have sufficient mechanical strength. In addition, it is believed that if the zeolite content drops below 1 wt%, the catalyst may not have sufficient cracking capacity.

[0047] A zeolite sample will have a distribution of crystallite sizes with a peak concentration of one crystallite size. As used herein, the term "average crystallite size" refers to the most likely crystallite size in a zeolite sample. For example, as discussed more fully in the Examples below, Figure 5The crystallite size distribution of conventional sized FS-USY zeolites and large crystallite FS-USY zeolites is provided. Conventional sized FS-USY generally has an average crystallite size of about 2 μm, as shown in size distribution curve (a). However, as shown in size distribution curve (b), the average crystallite size of the FS-USY described herein may be 5 μm to 50 μm, 6 μm to 50 μm, 7 μm to 50 μm, 8 μm to 50 μm, 9 μm to 50 μm, 10 μm to 50 μm, 11 μm to 50 μm, 12 μm to 50 μm, 13 μm to 50 μm, 14 μm to 50 μm, 15 μm to 50 μm, 16 μm to 50 μm, 17 μm to 50 μm, 18 μm to 50 μm, 19 μm to 50 μm, 20 μm to 50 μm, 21 μm to 50 μm, 22 μm to 50 μm, 23 μm to 50 μm, 24 μm to 50 μm, 25 μm to 50 μm, 26 μm to 50 μm, 27 μm to 50 μm, 28 μm to 50 μm, 29 μm to 50 μm, 30 μm to 50 μm, 31 μm to 50 μm, 32 μm to 50 μm, 33 μm to 50 μm, 34 μm to 50 μm, 35 μm to 50 μm, 36 μm to 50 μm, 37 μm to 50 μm, 38 μm to 50 μm, 39 μm to 50 μm 6μm to 50μm, 17μm to 50μm, 18μm to 50μm, 19μm to 50μm, 20μm to 50μm, 21μm to 50μm, 22μm to 50μm, 23μm to 50μm, 24μm to 50μm, 25μm to 50μm, 26μm to 50μm, 27μm to 50μm, 28μm to 50μm, 29μm to 50μm, 30μm m to 50μm, 5μm to 49μm, 5μm to 48μm, 5μm to 47μm, 5μm to 46μm, 5μm to 45μm, 5μm to 44μm, 5μm to 43μm, 5 μm to 42μm, 5μm to 41μm, 5μm to 40μm, 5μm to 39μm, 5μm to 38μm, 5μm to 37μm, 5μm to 36μm, 5μm to 35μm, 1 to 16 μm. It should be understood that the average crystallite size can be within a range formed from any lower limit of such average crystallite size described herein to any upper limit of such average crystallite size described herein.

[0048] Without intending to be bound by any particular theory, it is believed that the larger average crystallite size zeolites used in the hydrocracking catalyst formulation can provide a more active catalyst and provide higher naphtha selectivity when compared to catalyst compositions using conventional size zeolites. Likewise, without intending to be bound by any particular theory, it is believed that the larger crystallite size allows the hydrocarbons to have a longer residence time in the super cages formed by the zeolite, which in turn allows for more intense cracking.

[0049] In an embodiment, the hydrogenation metal component may include known metal components used in conventional hydrocracking catalysts. Examples include, but are not limited to, metal components in Group 8 of the long periodic table (iron, cobalt, nickel, rhodium, palladium, silver, iridium, platinum or gold) and / or metal components in Group 6 (chromium, molybdenum or tungsten). For example, the hydrogenation metal component may include a metal component of the platinum group (platinum, rhodium, palladium, etc.) or a combination of molybdenum or tungsten in Group 6 and cobalt or nickel in Group 8.

[0050] In another aspect, a method of preparing a catalyst composition may include forming a USY zeolite having an average crystallite size of 5 μm to 50 μm, heating the USY zeolite in an oven at a temperature of 500° C. to 700° C., forming a suspension of the thus calcined USY zeolite at a pH of less than 2, mixing a zirconium compound and / or a titanium compound and / or a hafnium compound with the USY zeolite, and neutralizing the resulting suspension to produce a FS-USY zeolite. The resulting catalyst composition is as described above.

[0051] Y-type zeolite can be formed by any method. The following is an exemplary, non-limiting method. An alumina solution is prepared by combining sodium hydroxide and aluminum powder in water. Similarly, a silica solution is prepared by combining sodium hydroxide with colloidal silica. The alumina solution is added to the silica solution while mixing in an ice bath and then kept at room temperature for at least 24 hours.

[0052] In conventional synthesis methods, Y-type zeolite is recrystallized under conditions that provide a zeolite having an average crystallite size of about 2 μm. For example, conventional recrystallization is performed at 60°C for more than one day. However, according to the embodiments described herein, Y-type zeolite is recrystallized under conditions that provide a zeolite having an average crystallite size of 5 μm to 50 μm, 6 μm to 50 μm, 7 μm to 50 μm, 8 μm to 50 μm, 9 μm to 50 μm, 10 μm to 50 μm, 11 μm to 50 μm, 12 μm to 50 μm, 13 μm to 50 μm, 14 μm to 50 μm, 15 μm to 50 μm, 16 μm to 50 μm, 17 μm to 50 μm, 18 μm to 50 μm, 19 μm to 50 μm, 20 μm to 50 μm, 21 μm to 50 μm, 22 μm to 50 μm, 23 μm to 50 μm, 24 μm to 50 μm, 25 μm to 50 μm, 26 μm to 50 μm, 27 μm to 50 μm, 28 μm to 50 μm, 29 μm to 50 μm, 30 μm to 50 μm, 31 μm to 50 μm, 32 μm to 50 μm, 33 μm to 50 μm, 34 μm to 50 μm, 35 μm to 50 μm, 36 μm to 50 μm, 37 μm to 50 μm, 38 μm to 50 μm, 39 μm 0μm, 17μm to 50μm, 18μm to 50μm, 19μm to 50μm, 20μm to 50μm, 21μm to 50μm, 22μm to 50μm, 23μm to 50μm, 24μm to 50μm, 25μm to 50μm, 26μm to 50μm, 27μm to 50μm, 28μm to 50μm, 29μm to 50μm, 30μm to 50 μm, 5μm to 49μm, 5μm to 48μm, 5μm to 47μm, 5μm to 46μm, 5μm to 45μm, 5μm to 44μm, 5μm to 43μm, 5μm to 42μm, 5μm to 41μm, 5μm to 40μm, 5μm to 39μm, 5μm to 38μm, 5μm to 37μm, 5μm to 36μm, 5μm to 35μm, 5μm The crystallite may be recrystallized under conditions of 5 to 34 μm, 5 to 33 μm, 5 to 32 μm, 5 to 30 μm, 5 to 29 μm, 5 to 28 μm, 5 to 27 μm, 5 to 26 μm, 5 to 25 μm, 10 to 20 μm, 11 to 19 μm, 12 to 18 μm, 13 to 17 μm, or even 14 to 16 μm. For example, Table 1 provides the time and temperature conditions for obtaining an average crystallite size of 5 μm and 25 μm.

[0053]

[0054] A detailed method for preparing FS-USY zeolite from Y-type zeolite is provided in US Pat. No. 10,293,332, the entire contents of which are incorporated herein by reference.

[0055] The Y-type zeolite synthesized by the ordinary method is subjected to the exchange of sodium ions with ammonium ions by the conventional method to provide USY zeolite. For example, the Y-type zeolite is dispersed in water to prepare a suspension, and ammonium sulfate is added thereto. The solid material is washed with water and then washed with an aqueous ammonium sulfate solution at a temperature of 40°C to 80°C. Then, the product is washed with water again at a temperature of 40°C to 95°C and dried at a temperature of 100°C to 180°C for 30 minutes to obtain an ammonium-exchanged Y-type zeolite. Subsequently, a hydrogen-type Y-type zeolite is prepared by calcining the above-mentioned ammonium-exchanged Y-type zeolite at 500°C to 800°C in a saturated steam atmosphere for 10 minutes to 10 hours. The repetition of this process increases the amount of ammonium contained on the Y-type zeolite. In this regard, the final ammonium ion exchange rate can be 90% or more.

[0056] In order to provide FS-USY zeolite, the USY zeolite prepared as described above is first calcined at 500°C to 700°C, for example, at 550°C to 650°C, for 30 minutes to 10 hours. If the calcination temperature of the USY zeolite is lower than 500°C, a lower amount of zirconium atoms and / or titanium atoms and / or hafnium atoms tends to be introduced when a framework substitution treatment is performed in a subsequent step relative to a method of calcining at 500°C to 700°C. However, if the calcination temperature exceeds 700°C, the specific surface area of ​​the USY zeolite may be reduced, and a lower amount of zirconium atoms and / or titanium atoms and / or hafnium atoms tends to be introduced when a framework substitution treatment is performed in a subsequent step relative to a method of calcining at 500°C to 700°C. Calcination can be performed in various atmospheres, including but not limited to air.

[0057] The calcined USY zeolite may then be suspended in water at a temperature of about 20° C. to about 30° C. to form a USY zeolite suspension. The liquid / solid mass ratio of the suspension may be in the range of 5 to 15. For example, the liquid / solid mass ratio may be 8 to 12.

[0058] Next, an inorganic acid or an organic acid may be added to the suspension to obtain an acidified USY zeolite suspension. Exemplary acids include, but are not limited to, sulfuric acid, nitric acid, hydrochloric acid, carboxylic acids, and mixtures of two or more thereof. Advantageously, the acid may be used to adjust the pH of the suspension to less than 2, such as 1 to 2. It has been observed that when an aqueous solution of a zirconium compound and / or an aqueous solution of a titanium compound and / or an aqueous solution of a hafnium compound is mixed with a suspension for a framework substitution treatment discussed further below, a pH within the above range may prevent precipitation.

[0059] A solution containing a zirconium compound and / or a titanium compound and / or a hafnium compound can be added to the acidified suspension and mixed. The addition of the zirconium compound and / or the titanium compound and / or the hafnium compound can be carried out gradually, for example by dropwise addition. The mixing can be carried out for 3 to 5 hours at room temperature, i.e., from about 25°C to about 35°C. Then, the mixed solution can be neutralized to a pH of 7 to 7.5 by adding a base and dried at 80°C to 180°C to obtain a FS-USY zeolite, wherein the zirconium atom and / or the titanium atom and / or the hafnium atom form a part of the zeolite framework by replacing the aluminum atom that was previously part of the zeolite framework. Exemplary bases include, but are not limited to, aqueous ammonia.

[0060] In embodiments, exemplary zirconium compounds include but are not limited to zirconium sulfate, zirconium nitrate, zirconium chloride and a combination of two or more thereof. In embodiments, relative to the mass of the USY zeolite used, the amount of the zirconium compound added can be 0.1% to 5% by mass in terms of zirconium oxide. For example, 0.2% to 4% by mass of zirconium compound can be added. Adding zirconium compound in an amount less than 0.1% by mass cannot obtain the desired USY zeolite properties. Adding zirconium compound in an amount exceeding 5% by mass may cause pore blockage of zeolite. In embodiments, an aqueous solution of a zirconium compound prepared by dissolving the zirconium compound in water can be used as the zirconium compound.

[0061] In an embodiment, exemplary titanium compounds include, but are not limited to, titanium sulfate, titanium acetate, titanium chloride, titanium nitrate, titanium lactate, and a combination of two or more thereof. In an embodiment, relative to the mass of the USY zeolite used, the amount of the titanium compound added can be 0.1% to 5% by mass in terms of titanium oxide. For example, 0.2% to 4% by mass of titanium compound can be added. Adding a titanium compound in an amount less than 0.1% by mass cannot obtain the desired USY zeolite properties. Adding a titanium compound in an amount exceeding 5% by mass may cause pore blockage of the zeolite. In an embodiment, an aqueous solution of a titanium compound prepared by dissolving the titanium compound in water can be used as the titanium compound.

[0062] In an embodiment, exemplary hafnium compounds include, but are not limited to, hafnium chloride, hafnium nitrate, hafnium fluoride, hafnium bromide, hafnium oxalate, and the like. In an embodiment, the amount of the hafnium compound added may be 0.1% to 5% by mass in terms of hafnium oxide relative to the mass of the USY zeolite used. For example, 0.2% to 4% by mass of the hafnium compound may be added. Adding a hafnium compound in an amount less than 0.1% by mass does not obtain the desired USY zeolite properties. Adding a hafnium compound in an amount exceeding 5% by mass may result in the clogging of the zeolite pores and may also significantly increase the cost of the catalyst. In an embodiment, an aqueous solution of a hafnium compound prepared by dissolving the hafnium compound in water is suitable for use as the hafnium compound.

[0063] The FS-USY zeolite prepared as described above can then be impregnated with a hydrogenation metal component by conventional methods. For example, the hydrogenation metal component can include iron, cobalt, nickel, rhodium, palladium, silver, iridium, platinum, gold, chromium, molybdenum, tungsten, or a combination of two or more thereof.

[0064] On the other hand, a method for hydrocracking a hydrocarbon oil comprises contacting at least one hydrocarbon oil stream with at least one hydrocracking catalyst composition and hydrogen in a reactor to hydrocrack the hydrocarbon oil stream. The hydrocracking catalyst may be as described above. That is, the hydrocracking catalyst may include a catalyst support and at least one hydrogenation metal component disposed on the catalyst support. The catalyst support may include at least one average crystallite size of 5 μm to 50 μm, 6 μm to 50 μm, 7 μm to 50 μm, 8 μm to 50 μm, 9 μm to 50 μm, 10 μm to 50 μm, 11 μm to 50 μm, 12 μm to 50 μm, 13 μm to 50 μm, 14 μm to 50 μm, 15 μm to 50 μm, 16 μm to 50 μm, 17 μm to 50 μm, 18 μm to 50 μm, 19 μm to 50 μm, 20 μm to 50 μm, 21 μm to 50 μm, 22 μm to 50 μm, 23 μm to 50 μm, 24 μm to 50 μm, 25 μm to 50 μm, 26 μm to 50 μm, 27 μm to 50 μm, 28 μm to 50 μm, 29 μm to 50 μm, 30 μm to 50 μm, 31 μm to 50 μm, 32 μm to 50 μm, 33 μm to 50 μm, 34 μm to 50 μm, 36 μm to 50 μm, 37 μm to 50 μm, 38 μm to 50 μm, 39 μm to 50 μm, 40 μm to 50 μ to 50μm, 18μm to 50μm, 19μm to 50μm, 20μm to 50μm, 21μm to 50μm, 22μm to 50μm, 23μm to 50μm, 24μm to 50μm, 25μm to 50μm, 26μm to 50μm, 27μm to 50μm, 28μm to 50μm, 29μm to 50μm, 30μm to 50μm, 5μ m to 49μm, 5μm to 48μm, 5μm to 47μm, 5μm to 46μm, 5μm to 45μm, 5μm to 44μm, 5μm to 43μm, 5μm to 42μm , 5μm to 41μm, 5μm to 40μm, 5μm to 39μm, 5μm to 38μm, 5μm to 37μm, 5μm to 36μm, 5μm to 35μm, 5μm to 3 11 μm to 19 μm, 12 μm to 18 μm, 13 μm to 17 μm, or even 14 μm to 16 μm FS-USY zeolite.

[0065] The reactor may be operated in a temperature range of 300° C. to 500° C. For example, the reactor may be operated in a temperature range of 310° C. to 490° C., 320° C. to 480° C., 330° C. to 470° C., 340° C. to 460° C., 350° C. to 450° C., 360° C. to 440° C., 370° C. to 430° C., 380° C. to 420° C., 390° C. to 410° C., or even 395° C. to 405° C. It should be understood that the reactor may be operated in a temperature range formed by any lower limit of such temperature described herein and any upper limit of such temperature described herein.

[0066] The boiling point of the hydrocarbon oil may be from 375° C. to 833° C. For example, the boiling point of the hydrocarbon oil may be from 400° C. to 800° C., 450° C. to 750° C., 500° C. to 700° C., 550° C. to 650° C., or even 575° C. to 625° C. It should be understood that the boiling point of the hydrocarbon oil may be within a temperature range formed by any lower limit of such temperature described herein and any upper limit of such temperature described herein.

[0067] Hydrogen can be used to produce saturated hydrocarbons in the hydrocracking process. Hydrogen can be added to the reactor at a pressure of 3.5 MPa to 25 MPa. For example, hydrogen can be added to the reactor at a pressure of 4 MPa to 24.5 MPa, 4.5 MPa to 24 MPa, 5 MPa to 23.5 MPa, 5.5 MPa to 23 MPa, 6 MPa to 22.5 MPa, 6.5 MPa to 22 MPa, 7 MPa to 21.5 MPa, 7.5 MPa to 21 MPa, 8 MPa to 20.5 MPa, 8.5 MPa to 20 MPa, 9 MPa to 19.5 MPa, The reactor is added to the pressure of 9.5MPa to 19MPa, 10MPa to 18.5MPa, 10.5MPa to 18MPa, 11MPa to 17.5MPa, 11.5MPa to 17MPa, 12MPa to 16.5MPa, 12.5MPa to 16MPa, 13MPa to 15.5MPa, 13.5MPa to 15MPa or even 14MPa to 14.5MPa. It should be understood that hydrogen can be added to the reactor in a pressure range from any lower limit of this pressure as described herein to any upper limit of this pressure as described herein. It is not intended to be bound by any particular theory, and it is believed that process performance will be significantly reduced under lower hydrogen pressure. On the contrary, it is believed that the process using high hydrogen pressure requires special equipment, which may significantly increase the cost of the process.

[0068] The hydrogen feed and hydrocarbon oil feed can be adjusted so that the hydrogen / oil ratio in the reactor can be 500 standard cubic meters per cubic meter (hereinafter referred to as "Nm 3 / m 3 ”) to 2500Nm 3 / m3 , the standard cubic meter is defined as the volume in cubic meters at standard temperature and pressure (15°C and 0.1 MPa). For example, the hydrogen / oil ratio may be 550 Nm 3 / m 3 Up to 2450Nm 3 / m 3 、600Nm 3 / m 3 Up to 2400Nm 3 / m 3 、650Nm 3 / m 3 Up to 2350Nm 3 / m 3 、700Nm 3 / m 3 Up to 2300Nm 3 / m 3 、750Nm 3 / m 3 Up to 2250Nm 3 / m 3 、800Nm 3 / m 3 Up to 2200Nm 3 / m 3 、850Nm 3 / m 3 Up to 2150Nm 3 / m 3 、900Nm 3 / m 3 Up to 2100Nm 3 / m 3 、950Nm 3 / m 3 Up to 2050Nm 3 / m 3 、1000Nm 3 / m 3 Up to 2000Nm 3 / m 3 、1050Nm 3 / m 3 Up to 1950Nm 3 / m 3 、1100Nm 3 / m 3 Up to 1900Nm 3 / m 3 、1150Nm 3 / m 3 Up to 1850Nm 3 / m 3 、1200Nm 3 / m 3Up to 1800Nm 3 / m 3 、1250Nm 3 / m 3 Up to 1750Nm 3 / m 3 、1300Nm 3 / m 3 Up to 1700Nm 3 / m 3 、1250Nm 3 / m 3 Up to 1650Nm 3 / m 3 、1300Nm 3 / m 3 Up to 1500Nm 3 / m 3 , or even 1350Nm 3 / m 3 Up to 1450Nm 3 / m 3 It should be understood that the hydrogen / oil ratio can be within a range of ratios from any lower limit of such ratios described herein to any upper limit of such ratios described herein. Without intending to be bound by any particular theory, it is believed that process performance will be significantly reduced at lower hydrogen / oil ratios. Conversely, it is believed that processes using high hydrogen / oil ratios require specialized equipment, which may significantly increase the cost of the process, and may increase the gas holdup in the system, thereby reducing process performance.

[0069] The liquid space velocity (hereinafter "LHSV") of the hydrocarbon feed in the reactor can be from 0.1 to 10 per hour. For example, the liquid space velocity can be from 0.5 to 9.5 per hour, from 1 to 9 per hour, from 1.5 to 8.5 per hour, from 2 to 8 per hour, from 2.5 to 7.5 per hour, from 3 to 7 per hour, from 3.5 to 6.5 per hour, from 4 to 6 per hour, or even from 4.5 to 5.5 per hour. It should be understood that the LHSV can be within a range formed from any lower limit of the LHSV described herein to any upper limit of the LHSV described herein.

[0070] As described above, the hydrocracking process can be carried out in one or more reactors. Continuous flow reactors are well suited for this process, although the subject matter described herein is not limited thereto. Exemplary continuous flow reactors include, but are not limited to, stirred tank reactors, ebullating bed reactors, baffled slurry tanks, fixed bed reactors, rotary tubular reactors, slurry bed reactors, moving bed reactors, and combinations of two or more thereof.

[0071] According to one aspect, whether alone or in combination with any other aspect, the catalyst composition includes at least one hydrogenation metal component and a support. The support comprises a framework-substituted ultrastable Y-type (USY) zeolite substituted with zirconium atoms, titanium ions, or both zirconium atoms and titanium atoms. The average crystallite size of the framework-substituted USY zeolite is 5 μm to 50 μm.

[0072] According to the second aspect, either alone or in combination with any other aspect, the framework-substituted ultrastable Y-type zeolite is substituted with 0.1 to 5 mass % of zirconium atoms calculated as oxide.

[0073] According to the third aspect, either alone or in combination with any other aspect, the framework-substituted ultrastable Y-type zeolite is substituted with 0.1 to 5 mass % of titanium calculated as oxide.

[0074] According to a fourth aspect, alone or in combination with the third aspect, the framework-substituted ultrastable Y-type zeolite is substituted with 0.1 to 5 mass % of zirconium atoms in terms of oxide.

[0075] According to a fifth aspect, either alone or in combination with any other aspect, the framework-substituted ultrastable Y-type zeolite comprises hafnium atoms.

[0076] According to a sixth aspect, alone or in combination with the fifth aspect, the framework-substituted ultrastable Y-type zeolite is further substituted with hafnium atoms.

[0077] According to a seventh aspect, whether alone or in combination with any other aspect, the catalyst composition further comprises an inorganic oxide compound.

[0078] According to the eighth aspect, alone or in combination with the seventh aspect, the inorganic oxide compound comprises alumina, silica, titania, silica-alumina, alumina-titania, alumina-zirconia, alumina-boria, phosphorus-alumina, silica-alumina-boria, phosphorus-alumina-boria, phosphorus-alumina-silica, silica-alumina-titania, silica-alumina-zirconia and combinations of two or more thereof.

[0079] According to a ninth aspect, whether alone or in combination with any other aspect, the at least one hydrogenation metal component comprises 0.01 mass % to 40 mass % of the catalyst composition.

[0080] According to the tenth aspect, whether alone or in combination with any other aspect, the framework-substituted ultrastable Y-type zeolite has a lattice constant of 2.42 nm to 2.45 nm, a lattice constant of 600 nm 2 / g to 900m 2 / g specific surface area and 5 to 100 SiO 2 With Al 2O 3 molar ratio.

[0081] According to the eleventh aspect, whether alone or in combination with any other aspect, the catalyst composition has 200 m 2 / g to 450m 2 The specific surface area and multiple diameters of or smaller pores having a pore volume of 0.4 ml / g to 0.75 ml / g, wherein the at least one hydrogenation metal component accounts for 0.01 mass % to 40 mass % of the catalyst composition.

[0082] According to the twelfth aspect, whether alone or in combination with any other aspect, the at least one hydrogenation metal component is selected from the group consisting of iron, cobalt, nickel, rhodium, palladium, silver, iridium, platinum, gold, chromium, molybdenum, tungsten and combinations of two or more thereof.

[0083] According to a thirteenth aspect, either alone or in combination with any other aspect, the framework-substituted USY zeolite has an average crystallite size of 10 μm to 20 μm.

[0084] According to the fourteenth aspect, whether alone or in combination with any other aspect, the catalyst composition also includes an inorganic oxide compound, which is selected from the group consisting of alumina, silica and a mixture of alumina and silica; wherein the at least one hydrogenation metal component is selected from the group consisting of iron, cobalt, nickel, rhodium, palladium, silver, iridium, platinum, gold, chromium, molybdenum, tungsten and a combination of two or more thereof.

[0085] According to the fifteenth aspect, whether alone or in combination with any other aspect, the method for preparing a catalyst composition includes forming an ultrastable Y-type (USY) zeolite having an average crystallite size of 5 μm to 50 μm; heating the USY zeolite at a temperature of 500°C to 700°C; forming a suspension comprising the USY zeolite, the liquid / solid ratio of the suspension being 5 to 15; adding at least one inorganic acid, at least one organic acid, or a mixture of at least one inorganic acid and at least one organic acid to the suspension so that the pH of the suspension is less than or equal to 2; mixing a zirconium compound, a titanium compound, a hafnium compound, or a mixture of two or more thereof with the suspension having a pH less than or equal to 2; and adding a base so that the pH of the suspension is 6 to 8 to obtain a framework-substituted USY zeolite.

[0086] According to a sixteenth aspect, whether alone or in combination with any other aspect, in the method, the ultrastable Y-type zeolite has a lattice constant of 2.42 nm to 2.45 nm, a lattice constant of 600 nm to 1.5 nm, a 2 / g to 900m 2 / g specific surface area and 5 to 100 SiO 2 With Al 2 O 3 molar ratio.

[0087] According to a seventeenth aspect, whether alone or in combination with any other aspect, the method further comprises adding at least one hydrogenation metal to the catalyst composition.

[0088] According to the eighteenth aspect, whether alone or in combination with any other aspect, in the method, the at least one hydrogenation metal component is selected from the group consisting of iron, cobalt, nickel, rhodium, palladium, silver, iridium, platinum, gold, chromium, molybdenum, tungsten and a combination of two or more thereof.

[0089] According to a nineteenth aspect, whether alone or in combination with any other aspect, in the method, the at least one hydrogenation metal is added such that the at least one hydrogenation metal accounts for 0.01 mass % to 40 mass % of the catalyst composition.

[0090] According to the twentieth aspect, whether alone or in combination with any other aspect, in the method, the average crystallite size of the framework-substituted USY zeolite is from 10 μm to 20 μm.

[0091] According to the twenty-first aspect, whether alone or in combination with any other aspect, the method also includes adding an inorganic oxide compound, wherein the inorganic oxide compound is selected from the group consisting of aluminum oxide, silicon dioxide, and a mixture of aluminum oxide and silicon dioxide; and adding at least one hydrogenation metal component, wherein the hydrogenation metal component is selected from the group consisting of iron, cobalt, nickel, rhodium, palladium, silver, iridium, platinum, gold, chromium, molybdenum, tungsten, and a combination of two or more thereof.

[0092] According to the twenty-second aspect, whether alone or in combination with any other aspect, a method for hydrocracking a hydrocarbon oil comprises contacting the hydrocarbon oil with at least one catalyst composition and hydrogen in a reactor to hydrocrack the hydrocarbon oil. The catalyst composition comprises at least one hydrogenation metal component and a carrier. The carrier comprises a framework-substituted ultrastable Y-type (USY) zeolite substituted with zirconium atoms, titanium ions, or both zirconium atoms and titanium atoms. The average crystallite size of the framework-substituted USY zeolite is 5 μm to 50 μm.

[0093] According to a twenty-third aspect, whether alone or in combination with any other aspect, the hydrocracking is carried out at a temperature of 300°C to 500°C.

[0094] According to the twenty-fourth aspect, whether alone or in combination with any other aspect, the reactor is a continuous flow reactor, the boiling point of the hydrocarbon stream is 375°C to 833°C; hydrogen is added to the reactor at a pressure of 3.5 MPa to 25 MPa; the liquid space velocity of the reactor is 0.1 to 10 per hour; and the hydrogen / oil ratio of the reactor is 500 Nm 3 / m 3 Up to 2500Nm 3 / m 3 .

[0095] In accordance with a twenty-fifth aspect, whether alone or in combination with any other aspect, the method further comprises collecting a distillate from the reactor.

[0096] According to the twenty-sixth aspect, whether alone or in combination with any other aspect, the reactor includes a continuous flow reactor, which is selected from the group consisting of a stirred tank reactor, a boiling bed reactor, a baffled slurry tank, a fixed bed reactor, a moving bed reactor, a rotating tubular reactor, a slurry bed reactor and a combination of two or more thereof.

[0097] According to a twenty-seventh aspect, whether alone or in combination with any other aspect, the hydrocarbon oil comprises a refined oil obtained from crude oil, synthetic crude oil, asphalt, oil sands, shale oil, kerosene, or a combination of two or more thereof.

[0098] According to the twenty-eighth aspect, whether alone or in combination with any other aspect, the refined oil comprises vacuum gas oil, deasphalted oil, demetallized oil, light coker gas oil, heavy coker gas oil, cycle oil obtained from a fluid catalytic cracking process, gas oil obtained from a visbreaking process, or a combination of two or more thereof.

[0099] According to the twenty-ninth aspect, whether alone or in combination with any other aspect, the framework-substituted USY zeolite has an average crystallite size of 10 μm to 20 μm.

[0100] Example

[0101] Using the above-described embodiments, exemplary catalyst compositions were prepared and characterized as follows.

[0102] Synthesis of Y-type zeolite

[0103] Conventional size Y zeolite (NaY):

[0104] Alumina solution was prepared by dissolving 10 g of NaOH in 20 g of double distilled water and then slowly adding 0.945 g of aluminum powder with a purity of 99.5%.2 , pH = 9.8) with 8.6g NaOH and 17g double distilled water to prepare a silica solution. The container was placed in an oven at 100°C for 6 minutes. The alumina solution was added to the silica solution while mixing in an ice bath. The resulting mixture was stirred at room temperature for 24 hours for aging. Crystallization was carried out at 60°C for 1500 minutes to provide a conventional size NaY zeolite, which is used in the following comparative examples.

[0105] Large crystal Y-type zeolite:

[0106] Alumina solution was prepared by dissolving 10 g of NaOH in 20 g of double distilled water and then slowly adding 0.945 g of aluminum powder with a purity of 99.5%. 2 , pH = 9.8) with 8.6 g NaOH and 17 g double distilled water to prepare a silica solution. The container was placed in an oven at 100° C. for 6 minutes. The alumina solution was added to the silica solution while mixing in an ice bath. The resulting mixture was stirred at room temperature for 24 hours for aging. Crystallization was carried out at 100° C. for 330 minutes to provide large crystal NaY zeolite.

[0107] Measurement of crystallite size

[0108] Scanning electron microscope (SEM) images were taken of regular sized NaY zeolite and large crystal NaY zeolite. Figure 1 Shown is a SEM image of a conventionally sized NaY zeolite at 10,000 times magnification. Figure 2 Shown is a SEM image of large crystal NaY zeolite at 10,000 times magnification. Figure 3 Shown is a SEM image of a conventionally sized NaY zeolite at 30,000 times magnification. Figure 4 SEM images of large crystal NaY zeolite at 30,000 times magnification are shown. Qualitatively, all figures show a significant difference in zeolite crystallite size between conventional sized NaY zeolite and large crystal NaY zeolite. Quantitatively, Figure 5 The crystallite size distribution curves of conventional sized NaY zeolite (a) and large crystal NaY zeolite (b) are shown. The peak 1a of the distribution curve (a) is at about 2 μm, while the peak 1b of the distribution curve (b) is at about 15 μm.

[0109] Post-modification of NaY zeolite

[0110] The conventional sized NaY zeolite and the large crystal NaY zeolite are then post-modified by dealumination and then insertion of titanium and zirconium into the framework of the zeolite as described in U.S. Pat. No. 10,293,332 (the entire contents of which are incorporated herein by reference) to provide conventional sized titanium-zirconium framework substituted ultrastable Y-type ("TiZr-USY") zeolite and large crystal TiZr-USY zeolite, respectively.

[0111] NaY zeolite is first subjected to sodium ion exchange with ammonium ion by conventional methods. In an exemplary method, Y-type zeolite is dispersed in water to prepare a suspension, to which ammonium sulfate is added. The solid material is then washed with water, followed by an aqueous ammonium sulfate solution at a temperature of 40°C to 80°C. The solid is then further washed with water at 40°C to 95°C and dried at 100°C to 180°C for 30 minutes, thereby producing an ammonium-exchanged Y-type zeolite, wherein 50% to 70% of the sodium contained in the Y-type zeolite is replaced by NH4.

[0112] Subsequently, hydrogen-type Y-type zeolite (HY) is prepared by calcining the above-mentioned ammonium-exchanged Y-type zeolite at 500° C. to 800° C. in a saturated steam atmosphere for 10 minutes to 10 hours. Then, by dispersing the above-obtained HY zeolite in water at 40° C. to 95° C. to prepare a suspension, and adding ammonium sulfate thereto, an ammonium-exchanged Y-type zeolite can be obtained, wherein 80% to 97% of the sodium contained in the initial NaY zeolite is ion-exchanged with NH4. The suspension is stirred at 40° C. to 95° C. for 10 minutes to 3 hours. The solid matter is then washed with water at 40° C. to 95° C., followed by washing with an aqueous ammonium sulfate solution at 40° C. to 95° C. Then, the solid is further washed with water at 40° C. to 80° C., and dried at 100° C. to 180° C. for 30 minutes to 30 hours. In this regard, the final ammonium ion exchange rate is at least 90%.

[0113] The ammonium-exchanged Y zeolite thus obtained is calcined at 500 to 700° C. for 10 minutes to 10 hours in, for example, a saturated steam atmosphere to provide USY zeolite.

[0114] The USY zeolite is then treated to remove extra-framework aluminum (aluminum atoms that do not form a zeolite framework). Extra-framework aluminum can be removed by, for example, dispersing the above-mentioned USY zeolite in warm water at 40°C to 95°C to prepare a suspension, adding sulfuric acid to the above-mentioned suspension, and stirring the suspension for 10 minutes to 3 hours while maintaining a temperature of 40°C to 95°C to dissolve the extra-framework aluminum. After dissolving the extra-framework aluminum, the suspension is filtered, the filter residue is washed with pure water at 40°C to 95°C, and dried at 100°C to 180°C for 3 to 30 hours. USY zeolite with extra-framework aluminum removed is thus obtained.

[0115] The USY zeolite with the aluminum outside the framework removed is calcined at 500°C to 700°C for 30 minutes to 10 hours. The calcined ultrastable Y-type zeolite is suspended in water at a temperature of about 20°C to about 30°C to form a suspension having a liquid / solid mass ratio in the range of 5 to 15. Next, an inorganic acid or an organic acid is added so that the pH of the suspension is less than 2, followed by gradual addition of a solution containing a zirconium compound and a titanium compound and mixing. The mixed solution is then neutralized (pH 7.0 to 7.5) and dried at 80°C to 180°C to provide a TiZr-USY zeolite.

[0116] Preparation of catalyst composition

[0117] Catalyst composition 1 (comparative) was formulated using 30 wt% of conventional size TiZr-USY zeolite and 70 wt% of pure alumina binder. Catalyst composition 2 (inventive) was formulated using 30 wt% of large crystallite size TiZr-USY zeolite and 70 wt% of pure alumina binder. The combined TiZr-USY zeolite and binder are referred to as the "support". Both Catalyst composition 1 and Catalyst composition 2 had 16 wt% molybdenum trioxide and 4 wt% nickel oxide, calculated as the components of the support.

[0118] Pilot Plant Hydrocracking Process

[0119] Both catalyst composition 1 and catalyst composition 2 were used in a hydrocracking process with a vacuum gas oil (VGO) feed. The density of VGO at 15°C is 0.9203 g / cm 3 , sulfur content was 2.231 wt. %, nitrogen content was 815 ppm (wt.). The initial boiling point of the feed was 190° C., 10 wt. % VGO was fed to boil at 366° C., 30 wt. % VGO was fed to boil at 424° C., 50 wt. % VGO was fed to boil at 462° C., 70 wt. % VGO was fed to boil at 500° C., and 90 wt. % VGO was fed to boil at 480° C. The final boiling point was 580° C.

[0120] For the hydrocracking process, a pilot plant with two reactors in series was used. Two sets of experiments were conducted: (1) using a zeolite catalyst with large crystallite size (catalyst composition 2); (2) using a conventional size catalyst (catalyst composition 1). The first reactor was loaded with 112.5 ml of a commercial pre-treated catalyst, which was an amorphous silica-alumina catalyst with Ni and W as active phase metals, followed by 112.5 ml of catalyst composition 1. The second reactor was loaded with a commercial hydrocracking catalyst, 15 wt% zeolite and 85 wt% silica-alumina catalyst with Ni and W as active phase metals. At a partial pressure of 11.5 MPa (115 bar), the reaction mixture was heated to 1263 Nm 3 / m 3 Hydrogen was added to the pilot plant at a hydrogen / oil ratio of (1263 StLt / Lt) and a total LHSV of 0.326 per hour. The reactions were carried out sequentially in the first reactor at 360.8°C, 371.1°C and 381.3°C using catalyst composition 1 and in the second reactor at 350.6°C, 359.7°C and 370.1°C using a commercial hydrocracking catalyst, 15 wt% zeolite and 85 wt% silica-alumina containing catalyst with Ni and W as active phase metals without cooling between additions. In experiment 2, the first reactor was loaded with 112.5 ml of a commercial pre-treatment catalyst, which was an amorphous silica-alumina catalyst with Ni and W as active phase metals, followed by 112.5 ml of catalyst composition 2. The second reactor was loaded with a commercial hydrocracking catalyst, 15 wt% zeolite and 85 wt% silica-alumina containing catalyst with Ni and W as active phase metals. At a partial pressure of 11.5 MPa (115 bar), the 3 / m 3 Hydrogen was added to the pilot plant at a hydrogen / oil ratio of (1263 NLt / Lt) and a total LHSV of 0.326 per hour. Reactions were carried out sequentially at 361.6°C and 370.9°C in the first reactor using Catalyst Composition 2 and at 351.5°C and 359.0°C in the second reactor using a commercial hydrocracking catalyst without cooling between increases.

[0121] Figure 6 A plot of VGO feed conversion versus reactor temperature is provided, and Table 2 summarizes the data. Figure 6 As shown, Catalyst Composition 2 including large crystal USY ("15 μm") zeolite provides greater conversion at the same temperature than Catalyst Composition 1 including conventional sized USY ("2 μm") zeolite. Therefore, Catalyst Composition 2 is more active than Catalyst Composition 1.

[0122]

[0123]

[0124] Figure 7 A plot of middle distillate (MD) and naphtha selectivity versus VGO feed conversion is provided and Table 3 summarizes the data. Figure 7 As shown, Catalyst Composition 2, which includes large crystal USY ("15 μm") zeolite, provides greater selectivity for naphtha in the conversion studied than Catalyst Composition 1, which includes conventional sized USY ("2 μm") zeolite. In contrast, Catalyst Composition 2 provides less selectivity for middle distillates than Catalyst Composition 1.

[0125]

[0126] Note that, in contrast to statements of intended use, statements in this disclosure about components of the disclosure being "operable" or "sufficient" to embody a particular property or function in a particular manner are structural statements. More specifically, references in this disclosure to the manner in which a component is "operable" or "sufficient" denote an existing physical condition of the component and, therefore, should be considered as explicit statements of a structural feature of the component.

[0127] The subject matter of the present disclosure has been described in detail with reference to specific embodiments, and it is noted that the various details disclosed in the present disclosure should not be considered as implying that these details relate to elements that are essential components of the various embodiments described in the present disclosure. In addition, it is apparent that modifications and variations are possible without departing from the scope of the present disclosure, including but not limited to the embodiments defined in the appended claims.

[0128] The singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0129] Throughout this disclosure, ranges are provided. It is contemplated that each discrete value contained within the range is also included. Additionally, ranges formed from each discrete value contained within the explicitly disclosed range are also contemplated.

[0130] As used in this disclosure and the appended claims, the words "comprising," "having," and "including" and all grammatical variations thereof are intended to have an open, non-limiting meaning that does not exclude additional elements or steps.

[0131] As used in the present disclosure, terms such as "first" and "second" are arbitrarily assigned and are intended only to distinguish between two or more instances or components. It should be understood that the words "first" and "second" have no other purpose and are not part of the name or description of the component, nor do they necessarily define the relative positioning, position, or order of the components. In addition, it should be understood that the mere use of the terms "first" and "second" does not require the existence of any "third" component, although such a possibility is contemplated within the scope of the present disclosure.

Claims

1. A catalyst composition comprising: at least one hydrogenation metal component; and Carrier; in The support comprises a framework-substituted ultrastable Y (USY) zeolite substituted with zirconium atoms, titanium atoms, or both zirconium atoms and titanium atoms; and The average crystallite size of the framework-substituted USY zeolite is 11 μm to 50 μm.

2. The catalyst composition according to claim 1, wherein The framework-substituted ultrastable Y-type zeolite is substituted with 0.1-5 mass % of zirconium atoms calculated as oxide, or 0.1-5 mass % of titanium calculated as oxide, or 0.1-5 mass % of zirconium atoms calculated as oxide and 0.1-5 mass % of titanium calculated as oxide.

3. The catalyst composition according to claim 1 or 2, wherein The framework-substituted ultrastable Y-type zeolite includes hafnium atoms.

4. The catalyst composition according to claim 1 or 2, further comprising an inorganic oxide compound, wherein the inorganic oxide compound comprises alumina, silica, titania, silica-alumina, alumina-titania, alumina-zirconia, alumina-boria, phosphorus-alumina, silica-alumina-boria, phosphorus-alumina-boria, phosphorus-alumina-silica, silica-alumina-titania, silica-alumina-zirconia and a combination of two or more thereof.

5. The catalyst composition according to claim 1 or 2, wherein The at least one hydrogenation metal component comprises 0.01 mass % to 40 mass % of the catalyst composition.

6. The catalyst composition according to claim 1 or 2, wherein The framework-substituted ultrastable Y-type zeolite has a lattice constant of 2.42 nm to 2.45 nm, a 2 / g to 900m 2 / g specific surface area and a molar ratio of SiO2 to Al2O3 of 5 to 100.

7. The catalyst composition according to claim 1 or 2, wherein The catalyst composition has 200m 2 / g to 450m 2 The specific surface area and multiple diameters of Or smaller pores, the pore volume is 0.4ml / g to 0.75ml / g.

8. The catalyst composition according to claim 1 or 2, wherein The at least one hydrogenation metal component is selected from the group consisting of iron, cobalt, nickel, rhodium, palladium, silver, iridium, platinum, gold, chromium, molybdenum, tungsten, and combinations of two or more thereof.

9. The catalyst composition according to claim 1 or 2, further comprising an inorganic oxide compound, the inorganic oxide compound being selected from the group consisting of alumina, silica and a mixture of alumina and silica; wherein the at least one hydrogenation metal component is selected from the group consisting of iron, cobalt, nickel, rhodium, palladium, silver, iridium, platinum, gold, chromium, molybdenum, tungsten and a combination of two or more thereof.

10. A method for making a catalyst composition, the method comprising: forming an ultrastable Y-type (USY) zeolite having an average crystallite size of 11 μm to 50 μm; heating the USY zeolite at a temperature of 500° C. to 700° C.; forming a suspension comprising the USY zeolite, wherein the liquid / solid ratio of the suspension is 5 to 15; adding at least one inorganic acid, at least one organic acid, or a mixture of at least one inorganic acid and at least one organic acid to the suspension so that the pH value of the suspension is less than or equal to 2; mixing a zirconium compound, a titanium compound, a hafnium compound, or a mixture of two or more thereof with the suspension having a pH value of less than or equal to 2; as well as A base is added to adjust the pH value of the suspension to 6 to 8 to obtain framework-substituted USY zeolite.

11. The method according to claim 10, wherein: The ultrastable Y-type zeolite has a lattice constant of 2.42 nm to 2.45 nm, a 2 / g to 900m 2 / g specific surface area and a molar ratio of SiO2 to Al2O3 of 5 to 100.

12. The method according to claim 10 or 11, further comprising adding at least one hydrogenation metal to the catalyst composition, wherein: The at least one hydrogenation metal component is selected from the group consisting of iron, cobalt, nickel, rhodium, palladium, silver, iridium, platinum, gold, chromium, molybdenum, tungsten, and combinations of two or more thereof.

13. A method for hydrocracking a hydrocarbon oil comprising: contacting the hydrocarbon oil with at least one catalyst composition and hydrogen in a reactor to hydrocracking the hydrocarbon oil, the catalyst composition comprising: at least one hydrogenation metal component; and carrier; wherein The support comprises a framework-substituted ultrastable Y (USY) zeolite substituted with zirconium atoms, titanium ions, or both zirconium atoms and titanium atoms; and The average crystallite size of the framework-substituted USY zeolite is 11 μm to 50 μm.

14. The method according to claim 13, wherein: The hydrocracking is carried out at a temperature of 300°C to 500°C.

15. The method according to claim 13 or 14, wherein: The reactor is a continuous flow reactor, the boiling point of the hydrocarbon oil is 375°C to 833°C; the hydrogen is added to the reactor at a pressure of 3.5MPa to 25MPa; the liquid space velocity of the reactor is 0.1 to 10 per hour; and the hydrogen / oil ratio of the reactor is 500Nm 3 / m 3 Up to 2500Nm 3 / m 3 .

16. The method of claim 13, further comprising collecting a distillate from the reactor.