Phosphor powder, light-emitting device, image display device, and lighting device
By optimizing the chemical composition and manufacturing process of the phosphor powder, the internal quantum efficiency and blue light conversion efficiency of the phosphor are improved, solving the deficiencies in the blue light conversion efficiency and internal quantum efficiency of the phosphor in the existing technology, and achieving high efficiency. light absorption and luminescence properties.
Patent Information
- Application Number
- CN202180076620.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-11-04
AI Technical Summary
There is room for improvement in the blue light conversion efficiency and internal quantum efficiency of existing phosphors, especially in improving the efficiency of converting blue light into longer wavelength light, which has not yet achieved optimal results.
Use phosphor powder represented by the general formula Mx(Si,Al)2(N,O)3±y, where M is Li and more than one alkaline earth metal element, 0.52≤x≤0.9, 0.06≤y≤0.36, Si/Al atomic ratio is 1.5~6, O/N The atomic ratio is 0 to 0.1, 5 to 50 mol% of M is Li, and 0.5 to 10 mol% of M is Ce phosphor powder, and its light absorption rate and particle size distribution are optimized through acid treatment, classification treatment and crushing methods to Improve the light absorption rate and luminous efficiency of phosphors.
It achieves high internal quantum efficiency and good blue light conversion efficiency, and the light absorption rate at the wavelength of 700nm is reduced, which improves the overall luminous performance and durability of the phosphor and is suitable for use in various light-emitting devices.
Smart Images

Figure CN116507693B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to phosphor powder, a light-emitting device, an image display device and a lighting device. Background Art
[0002] In order to manufacture a white LED (Light Emitting Diode), a phosphor is generally used. That is, a phosphor can be used as a wavelength conversion material for obtaining white light from blue light emitted from a blue LED.
[0003] With the popularization of white LEDs for lighting applications and research on the application of white LEDs to image display devices, the development of phosphors capable of converting blue light into light with a longer wavelength has continued.
[0004] One approach to improving phosphors is to change the chemical composition of the phosphors.
[0005] For example, Patent Document 1 describes a phosphor having a general formula M x (Si,Al)2(N,O) 3±y (wherein M is Li and one or more alkaline earth metal elements, 0.52≤x≤0.9, 0.06≤y≤0.23) and a part of M is substituted by Ce element, the Si / Al atomic ratio is 1.5~6, and the O / N atomic ratio is 0~0.1, 5~50mol% of M is Li, and 0.5~10mol% of M is Ce.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 5969391 Summary of the invention
[0009] The present inventors have found that the phosphor described in Patent Document 1 has room for improvement in terms of blue light conversion efficiency, specifically, in terms of improving internal quantum efficiency.
[0010] One of the objectives of the present inventors is to provide a phosphor powder having high internal quantum efficiency and improved blue light conversion efficiency, and the present inventors conducted this study.
[0011] The present inventors have conducted research and have completed the invention provided below.
[0012] According to the present invention, there is provided a phosphor powder, comprising phosphor particles,
[0013] The above-mentioned phosphor particles are of the general formula M x (Si,Al)2(N,O) 3±y(wherein M is Li and one or more alkaline earth metal elements, 0.52≤x≤0.9, 0.06≤y≤0.36) and a part of M is substituted by Ce element, Si / Al atomic ratio is 1.5 to 6, and O / N atomic ratio is 0 to 0.1, 5 to 50 mol% of M is Li, 0.5 to 10 mol% of M is Ce,
[0014] The light absorption rate of the above fluorescent powder at a wavelength of 700nm is A 700 Less than 10%.
[0015] Furthermore, according to the present invention, there is provided a light-emitting device comprising the above-mentioned phosphor powder and a light source.
[0016] Furthermore, according to the present invention, there is provided an image display device including the above-mentioned light emitting device.
[0017] Furthermore, according to the present invention, there is provided a lighting device including the above-mentioned light emitting device.
[0018] The phosphor powder of the present invention has high internal quantum efficiency and good blue light conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is a schematic cross-sectional view showing an example of the structure of a light emitting device.
[0020] Figure 2 This is an XRD pattern obtained by measuring the phosphor of Example 1 by X-ray powder diffraction (XRD). DETAILED DESCRIPTION
[0021] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0022] In the drawings, the same components are denoted by the same reference numerals, and the description thereof will be appropriately omitted.
[0023] The drawings are for illustration purposes only, and the shapes, dimensional ratios, etc. of the components in the drawings do not necessarily correspond to actual products.
[0024] In the present specification, "X to Y" in the description of a numerical range means greater than or equal to X and less than or equal to Y unless otherwise specified. For example, "1 to 5 mass %" means "greater than or equal to 1 mass % and less than or equal to 5 mass %".
[0025] <Phosphor powder>
[0026] The phosphor powder of this embodiment comprises a phosphor having a general formula M x (Si,Al)2(N,O) 3±yPhosphor particles represented by. In the general formula, M is Li and one or more alkaline earth metal elements, 0.52≤x≤0.9, 0.06≤y≤0.36. In addition, a part of M is replaced by Ce element, Si / Al atomic ratio is 1.5-6, O / N atomic ratio is 0-0.1, 5-50 mol% of M is Li, and 0.5-10 mol% of M is Ce.
[0027] In addition, the light absorption rate A of the phosphor powder of this embodiment at a wavelength of 700 nm is 700 Less than 10%.
[0028] The phosphor powder of this embodiment has at least A 700 This point of being 10% or less is different from the phosphor described in Patent Document 1. Compared with the phosphor described in Patent Document 1, the phosphor powder of this embodiment can efficiently convert blue light into light of a longer wavelength, for example, in terms of internal quantum efficiency.
[0029] The absorption of phosphors includes light absorption accompanying the electron transition of the luminescent center ion and light absorption unrelated to fluorescence due to impurities or crystal defects of the parent material. When a phosphor emitting visible light is irradiated with light in the near-infrared region, such as light with a wavelength of 700nm, the light absorption has nothing to do with fluorescence. Therefore, it is believed that the absorption rate of light with a wavelength of 700nm is related to the fluorescence characteristics.
[0030] In order to quantitatively evaluate the relationship between the above-mentioned light absorption rate and fluorescence characteristics, the inventors of the present invention have newly made a method based on the general formula M x (Si,Al)2(N,O) 3±y The absorbance of various phosphors shown in Figure 1 was measured for light with a wavelength of 700 nm. The results showed that when the light absorbance A at a wavelength of 700 nm is 700 Based on this discovery, the inventors of the present invention re-made a system comprising the general formula M x (Si,Al)2(N,O) 3±y The phosphor represented by A 700 The phosphor powder has a concentration of less than 10%. Furthermore, the internal quantum efficiency has been successfully improved.
[0031] The phosphor powder of this embodiment can be produced by using appropriate materials and selecting appropriate production methods and production conditions. Examples of "appropriate production methods and production conditions" include (i) subjecting the phosphor powder to an acid treatment under specific conditions, (ii) subjecting the phosphor powder to an appropriate classification treatment (preferably sedimentation classification), and (iii) designing a method for pulverizing the phosphor powder. The details of the production methods and production conditions will be described in detail later.
[0032] The description of the phosphor powder of this embodiment will be continued.
[0033] (Crystal structure, chemical composition, etc.)
[0034] The skeleton structure of the phosphor crystal is composed of (Si, Al)-(N, O)4 regular tetrahedral bonds, and the M element is located in the gaps. The composition of the above general formula is established in a wide range in which electrical neutrality is maintained as a whole by the parameters of the valence and amount of the M element, the Si / Al ratio, and the N / O ratio. As a representative phosphor represented by the above general formula, there is CaAlSiN3, in which the M element is Ca, x=1, Si / Al=1, and O / N=0. When a part of Ca in CaAlSiN3 is replaced by Eu, it becomes a red phosphor, and when it is replaced by Ce, it becomes a yellow to orange phosphor.
[0035] The crystal structure of the phosphor particles contained in the phosphor powder of this embodiment is generally based on CaAlSiN3 crystals. One of the characteristics of the phosphor particles is that the constituent elements and composition are greatly changed so that very high luminous efficiency can be obtained even when Ce is activated.
[0036] In the above general formula, the M element is a combination of the Li element and an alkaline earth metal element, a part of which is replaced by the Ce element that becomes the luminescence center. By using the Li element and utilizing its combination with a divalent alkaline earth element and a trivalent Ce element, the average valence of the M element can be widely controlled. + The ionic radius of ions is very small, and the crystal size can be greatly changed according to its amount to obtain a variety of fluorescent luminescence.
[0037] The coefficient x of the M element in the above general formula is 0.52 to 0.9, preferably 0.6 to 0.9, and more preferably 0.7 to 0.9. If the coefficient x exceeds 0.9, that is, close to the CaAlSiN3 crystal, there is a tendency for the fluorescence intensity to decrease. If the coefficient x is less than 0.52, a large amount of heterophases other than the target crystal phase are generated, so there is a tendency for the fluorescence intensity to decrease significantly.
[0038] In the present embodiment, electrical neutrality is maintained by the average valence or amount of the M element, the Si / Al ratio, and the O / N ratio, and when there are no defects in a single crystal, y=0. However, when the overall composition of the phosphor is considered, there is a second crystalline phase or an amorphous phase, or when the crystal itself is considered, charge imbalance may also occur due to crystal defects. In the present embodiment, from the viewpoint of improving the fluorescence intensity, y is preferably 0.06 to 0.36, more preferably 0.1 to 0.35, and further preferably 0.06 to 0.23.
[0039] In this embodiment, the O / N atomic ratio (molar ratio) is 0 to 0.1, preferably 0.01 to 0.08, and more preferably 0.02 to 0.07. If the O / N atomic ratio is too large, the amount of heterogeneous phase generation increases, the luminous efficiency decreases, and the covalency of the crystal decreases, resulting in a tendency for the temperature characteristics to deteriorate (brightness decreases at high temperatures).
[0040] The Si / Al atomic ratio (molar ratio) is usually determined when the average valence or amount of the M element and the O / N atomic ratio are within a predetermined range. The Si / Al atomic ratio is 1.5 to 6, preferably 2 to 4, and more preferably 2.5 to 4.
[0041] The content of Li in the phosphor particles is 5 to 50 mol%, preferably 15 to 45 mol%, and more preferably 25 to 45 mol% of the element M. The effect of Li is easily exerted when it is 5 mol% or more, but if it exceeds 50 mol%, the crystal structure of the target phosphor cannot be maintained and a heterogeneous phase is generated, and the luminous efficiency is easily reduced.
[0042] For the sake of caution, "Li content" refers to the Li content in the final phosphor powder, not the amount of raw material blending base. The Li compound used in the raw material has a high vapor pressure and is easily volatilized. When synthesizing nitrides and nitrogen oxides at high temperatures, a large amount of volatilization occurs. In other words, the amount of Li in the raw material blending base is very different from the content in the final product, and does not mean the Li content in the phosphor.
[0043] If the Ce content, which is the luminescence center of the phosphor particles, is too low, the contribution to luminescence tends to decrease. If the Ce content is too high, the Ce 3+ Therefore, the Ce content is 0.5 to 10 mol %, preferably 0.5 to 5 mol %, of the M element.
[0044] The alkaline earth metal element used as the M element in the above general formula can be any element, but when Ca is used, a high fluorescence intensity can be obtained, and the crystal structure can be stabilized in a wide composition range. Therefore, the M element preferably contains Ca. The M element can be a combination of multiple alkaline earth metal elements, for example, a part of the Ca element can be replaced by the Sr element.
[0045] The crystal structure of the phosphor particles is an orthorhombic system, and can be the same structure as the above-mentioned CaAlSiN3 crystal. As an example of the lattice constant of the CaAlSiN3 crystal, a=0.98007nm, b=0.56497nm, c=0.50627nm. In the present embodiment, the lattice constant is usually a=0.935~0.965nm, b=0.550~0.570nm, c=0.480~0.500nm, which are all smaller values compared with the CaAlSiN3 crystal. The range of the lattice constant reflects the above-mentioned constituent elements and composition.
[0046] The crystalline phase present in the phosphor particles is preferably the above-mentioned single crystalline phase. However, the phosphor particles may contain heterophases as long as they do not have a significant effect on the fluorescence characteristics. Examples of heterophases that have a low effect on the fluorescence characteristics under blue light excitation include α-sialon, AlN, LiSi2N3, LiAlSi2N4, etc. The amount of the heterophase is preferably an amount in which the intensity of the diffraction line of the other crystalline phases when evaluated by X-ray powder diffraction is 40% or less relative to the intensity of the strongest diffraction line of the above-mentioned crystalline phase.
[0047] The phosphor powder of this embodiment is excited by light in a wide wavelength range from ultraviolet light to visible light. For example, when irradiated with blue light of a wavelength of 455nm, it sometimes exhibits a broad fluorescence emission with an orange peak wavelength of 570 to 610nm and a half-peak width of the fluorescence spectrum of more than 125nm. Such phosphor powder is suitable as a phosphor for various light-emitting devices. In addition, the phosphor powder of this embodiment is similar to the existing nitride and oxynitride phosphors represented by CaAlSiN3, and has excellent heat resistance and chemical stability, and also has the characteristic of small brightness reduction due to temperature rise. Such characteristics are particularly suitable for applications requiring durability.
[0048] (Light Absorption)
[0049] As described above, the light absorption rate A of the phosphor powder of this embodiment at a wavelength of 700 nm is 700 Less than 10%. 700 It is preferably 1% to 10%, more preferably 2% to 10%, and particularly preferably 3% to 10%.
[0050] As another viewpoint, the light absorptivity of the phosphor powder of this embodiment at a wavelength of 600 nm is denoted by A. 600 (%), A 600 -A 700 It is preferably 6% to 10%, more preferably 7% to 10%, and even more preferably 7% to 9%. 600 -A 700 There is a tendency for phosphor powder having an appropriate numerical value to have better blue light conversion efficiency.
[0051] Although the detailed reason is unknown, due to the general formula M x (Si,Al)2(N,O) 3±y The peak wavelength of the light emission (fluorescence) of the phosphor shown is about 600nm when irradiated with blue light, so the light absorption rate A at a wavelength of 600nm is included. 600 The above indicators (A 600 -A 700 ) may be related to the conversion efficiency of blue light. For example, A 600 -A 700 The fact that the ratio is 6% to 10% may mean that the balance between the improvement of the fluorescence characteristics due to the increase in the absorption rate when excited with blue light and the decrease in the fluorescence characteristics due to the re-excited emission is good.
[0052] In addition, as another viewpoint, the light absorption rate A of the phosphor powder of this embodiment at a wavelength of 600 nm is 600 The value itself is preferably 8% to 20%, more preferably 10% to 20%, and even more preferably 11% to 17%.
[0053] When a phosphor is irradiated with light of wavelength 600nm, which is roughly the fluorescence peak wavelength, not only non-luminescent absorption due to impurities, crystal defects, etc., but also absorption caused by the electron transition of the luminescent center ion occurs. 600 Greater than A 700 However, light absorption near the peak wavelength can be used as an indicator of re-excited luminescence, which is a factor that reduces efficiency. 600 However, the larger the value, the smaller the contribution to the luminescence excitation. 600 Not too large, the fluorescence characteristics are further improved.
[0054] (Particle size distribution)
[0055] By appropriately designing the particle size distribution of the phosphor powder of this embodiment, it is sometimes possible to further improve the quantum efficiency or improve the balance of various performances.
[0056] Specifically, the volume-based cumulative 50% diameter D of the phosphor powder of this embodiment measured by the laser diffraction scattering method is 50 The (so-called median diameter) is preferably 8 μm to 25 μm, more preferably 10 μm to 20 μm, and further preferably 12 μm to 20 μm.
[0057] As another viewpoint, the volume-based cumulative 10% diameter D of the phosphor powder of the present embodiment measured by the laser diffraction scattering method is 10 It is preferably 2 μm to 15 μm, and more preferably 5 μm to 12 μm. 10The larger the value, the smaller the amount of fine powder (excessively fine phosphor particles that tend to reduce the conversion efficiency of blue light) in the phosphor powder. 10 As the value becomes larger to a certain extent, there is a tendency that the conversion efficiency of blue light is further improved.
[0058] As another viewpoint, the volume-based cumulative 90% diameter D of the phosphor powder of the present embodiment measured by the laser diffraction scattering method is 90 It is preferably 15 μm to 50 μm, and more preferably 18 μm to 40 μm. 90 However, the larger the number, the smaller the amount of coarse particles in the phosphor powder. 90 However, larger phosphor powder is effective in reducing the chromaticity deviation of the light-emitting device.
[0059] By the way, generally speaking, as the particle size of the particles contained in the powder increases, the influence of light scattering decreases and the light absorption rate increases. In other words, there is a trade-off relationship between the particle size and the light absorption rate. However, although the preferred particle size (D 50 etc.) are larger, there is still a tendency that the light absorptivity of the phosphor powder of this embodiment is smaller.
[0060] (Manufacturing method)
[0061] The phosphor powder of this embodiment can be produced, for example, by a series of steps including the following (1) to (4), a series of steps including (1) to (3) and (5), or a series of steps including (1) to (5). From the viewpoint of appropriately adjusting the non-luminescent absorption of the phosphor powder, the production process of the phosphor powder preferably includes (4) an acid treatment step and / or (5) a classification step (preferably sedimentation classification).
[0062] (1) Preparation process of raw material mixed powder
[0063] (2) Calcination process
[0064] (3) Pulverization step of calcined product
[0065] (4) Acid treatment process
[0066] (5) Classification step (preferably sedimentation classification)
[0067] Hereinafter, (1) to (5) will be described in detail.
[0068] (1) Preparation process of raw material mixed powder
[0069] In the step of preparing the raw material mixed powder, appropriate raw material powders are usually mixed to obtain the raw material mixed powder.
[0070] As raw material powder, it is preferred to use nitrides of constituent elements, i.e. silicon nitride, aluminum nitride, lithium nitride, cerium nitride, nitrides of alkaline earth elements (e.g. calcium nitride), etc. In general, nitride powders are unstable in the air, and the surface of the particles will be covered with an oxide layer. Even when nitride raw materials are used, the raw materials will contain a certain degree of oxides. When controlling the O / N ratio of the phosphor, while considering these, when oxygen is insufficient, a part of the nitride can be made into an oxide (containing a compound that becomes an oxide by heat treatment). As examples of oxides, cerium oxide, etc. can be cited.
[0071] In the raw material powder, the lithium compound volatilizes significantly when heated, and sometimes most of it volatilizes depending on the calcination conditions. Therefore, the amount of the lithium compound to be added is preferably determined according to the calcination conditions in consideration of the amount of volatilization during the calcination process.
[0072] Among the nitride raw material powders, lithium nitride, cerium nitride, and nitrides of alkaline earth elements react vigorously with moisture in the air. Therefore, these operations are preferably performed in a glove box replaced with an inert atmosphere.
[0073] From the perspective of operational efficiency, it is preferred that (i) first, silicon nitride, aluminum nitride and various oxide raw material powders that can be handled in air are weighed in predetermined amounts and mixed thoroughly in air to prepare a premixed powder, and (ii) thereafter, in a glove box, the premixed powder is mixed with a substance that easily reacts with water, such as lithium nitride, to prepare a raw material mixed powder.
[0074] (2) Calcination process
[0075] In the calcining step, the raw material mixed powder prepared in the raw material mixed powder preparation step (1) is filled into an appropriate container and heated using a calcining furnace or the like.
[0076] From the viewpoint of allowing the reaction to proceed sufficiently and from the viewpoint of suppressing lithium volatilization, the calcination temperature is preferably 1600 to 2000°C, more preferably 1700 to 1900°C.
[0077] From the viewpoint of allowing the reaction to proceed sufficiently and from the viewpoint of suppressing lithium volatilization, the calcination time is preferably 2 to 24 hours, more preferably 4 to 16 hours.
[0078] The calcination process is preferably carried out under a nitrogen atmosphere. In addition, it is preferred to appropriately adjust the pressure of the calcination atmosphere. Specifically, the pressure of the calcination atmosphere is preferably 0.5 MPa·G or more. When the calcination temperature is particularly above 1800°C, there is a tendency for the phosphor to decompose easily, but by increasing the pressure of the calcination atmosphere, the decomposition of the phosphor can be suppressed.
[0079] Incidentally, from the viewpoint of industrial productivity, the pressure of the calcining atmosphere is preferably less than 1 MPa·G.
[0080] The container filled with the raw material mixed powder is preferably made of a material that is stable in a high-temperature nitrogen atmosphere and does not react with the raw material mixed powder or its reaction product. The material of the container is preferably boron nitride.
[0081] (3) Pulverization step of calcined product
[0082] The calcined product obtained in (2) is usually in a bulk form, and therefore it is preferably pulverized into a small size to a certain extent by applying a mechanical force.
[0083] The pulverization can be performed using various devices such as a pulverizer, a mortar, a ball mill, a vibration mill, a jet mill, and a stamping machine. Two or more of these devices can be combined for pulverization. In the examples described below, a stamping machine is first used to obtain a coarse pulverization of the calcined product, and then the coarse pulverization is further pulverized using a jet mill. Although the detailed reason is unknown, by performing such pulverization, A is easily obtained. 700 The phosphor powder is less than 10%.
[0084] (4) Acid treatment process
[0085] In the acid treatment step, for example, the pulverized product obtained in the above (3) is immersed in an acidic aqueous solution. Although the detailed reason is unknown, it is believed that the "heterogeneous phase" in the phosphor that does not contribute to luminescence or reduces luminescence efficiency can be removed or reduced by acid treatment. 700 The fact that the amount is 10% or less may correspond to the removal or reduction of the heterogeneous phase.
[0086] The acidic aqueous solution may include an acidic aqueous solution containing one acid selected from acids such as hydrofluoric acid, nitric acid, and hydrochloric acid, or a mixed acid aqueous solution obtained by mixing two or more of the above acids. As the acid, nitric acid or hydrochloric acid is preferred, and hydrochloric acid is more preferred.
[0087] The concentration of the acidic aqueous solution can be appropriately set depending on the strength of the acid used, and is, for example, 0.5 to 50% by mass, preferably 1 to 30% by mass, and more preferably 1 to 10% by mass.
[0088] The temperature for acid treatment is preferably 25°C to 90°C, more preferably 60°C to 90°C. By treating at a relatively high temperature, A is easily obtained. 700 The phosphor powder is less than 10%.
[0089] The acid treatment time (immersion time) is preferably 15 to 80 minutes, more preferably 15 to 60 minutes.
[0090] After the acid treatment, the phosphor powder is preferably thoroughly washed with water and then dried.
[0091] (5) Grading process
[0092] In order to reduce the amount of fine powder (excessively fine phosphor particles that tend to reduce the conversion efficiency of blue light) in the powder, it is preferable to perform appropriate classification. In order to effectively remove the fine powder, the classification method is preferably sedimentation classification as described below.
[0093] First, the powder obtained in the (3) calcined product pulverization step or the powder subjected to the (4) acid treatment step is dispersed in an appropriate liquid, for example, an aqueous sodium hexametaphosphate solution, to prepare a dispersion.
[0094] Next, the dispersion is allowed to stand for a certain period of time to allow the particles with larger particle sizes to precipitate among the powders in the dispersion.
[0095] Thereafter, the supernatant was discharged.
[0096] Thereafter, the sodium hexametaphosphate aqueous solution is further added to the container where the precipitate remains, the powder is dispersed, the mixture is allowed to stand, and the supernatant is discharged, and these operations are repeated multiple times. "Multiple times" is preferably 5 times or more. The upper limit of the number of times is not particularly limited, and from the perspective of cost, for example, it is 15 times or less, specifically 10 times or less.
[0097] The amount of fine powder (excessively fine phosphor particles that tend to reduce the conversion efficiency of blue light) in the powder can be reduced by classification. 700 The fact that the content is less than 10% may be related to the small amount of fine powder in the phosphor powder.
[0098] The specific conditions for grading are as long as you can get an A in the end. 700 The phosphor powder with a particle size of less than 10% is not particularly limited. It is preferred to set the classification conditions in a manner to remove fine powder with a particle size of less than 10 μm, and more preferably to set the classification conditions in a manner to remove fine powder with a particle size of less than 7.5 μm, but this is for reference only. In the case of sedimentation classification, when setting the conditions, Stoke's law related to the sedimentation velocity of particles can be referred to.
[0099] <Light-emitting device, image display device, and lighting device>
[0100] By combining the phosphor powder of this embodiment with a light source, a light-emitting device can be obtained.
[0101] The light source typically emits ultraviolet light or visible light. For example, when the light source is a blue LED, the blue light emitted from the light source is irradiated on the phosphor powder, and then the blue light is converted into light with a longer wavelength. That is, the phosphor powder of this embodiment can be used as a wavelength conversion material that converts blue light into light with a longer wavelength.
[0102] Reference Figure 1An example of a specific configuration of the light emitting device will be described.
[0103] Figure 1 FIG. 1 is a cross-sectional schematic diagram showing an example of the structure of a light emitting device. Figure 1 As shown, the light emitting device 100 includes a light emitting element 120 , a heat sink 130 , a housing 140 , a first lead frame 150 , a second lead frame 160 , bonding wires 170 , 172 , and a composite body 40 .
[0104] The light emitting element 120 is mounted on a predetermined area of the upper surface of the heat sink 130. By mounting the light emitting element 120 on the heat sink 130, the heat dissipation of the light emitting element 120 can be improved. In addition, a package substrate may be used instead of the heat sink 130.
[0105] The light emitting element 120 is a semiconductor element that emits excitation light. As the light emitting element 120, for example, an LED chip that emits light with a wavelength of 300 nm to 500 nm, which is equivalent to near ultraviolet light to blue light, can be used. An electrode (not shown) disposed on the upper surface side of the light emitting element 120 is connected to the surface of the first lead frame 150 via a bonding wire 170 such as a metal wire. In addition, another electrode (not shown) formed on the upper surface of the light emitting element 120 is connected to the surface of the second lead frame 160 via a bonding wire 172 such as a metal wire.
[0106] A substantially funnel-shaped recessed portion whose aperture gradually increases from the bottom surface to the top is formed in the housing 140. The light emitting element 120 is disposed on the bottom surface of the recessed portion. The wall surface of the recessed portion surrounding the light emitting element 120 functions as a reflector.
[0107] The composite body 40 is filled into the above-mentioned recessed portion whose wall surface is formed by the housing 140. The composite body 40 is a wavelength conversion member that converts the excitation light emitted from the light emitting element 120 into light with a longer wavelength.
[0108] The composite 40 is obtained by dispersing at least the phosphor powder of the present embodiment in a sealing material 30 such as a resin. In order to obtain higher quality white light, the sealing material 30 may contain not only the phosphor powder of the present embodiment but also other phosphor powders.
[0109] Light emitting device 100 emits a mixed color of light from light emitting element 120 and light from phosphor particles 1 that absorb and are excited by light from light emitting element 120. Light emitting device 100 preferably emits white light by mixing the light from light emitting element 120 and light from phosphor particles 1.
[0110] By the way, Figure 1Although a surface-mounted light-emitting device is illustrated in the figure, the light-emitting device is not limited to the surface-mounted type, and may be a bullet type, COB (chip on board) type, CSP (chip scale package) type, or the like.
[0111] Examples of the use of the light emitting device include image display devices such as displays and lighting devices. For example, a liquid crystal display can be manufactured using the light emitting device 100 as a backlight. Alternatively, a lighting device can be manufactured using one or more light emitting devices 100 and implementing appropriate wiring, etc.
[0112] The embodiments of the present invention are described above, but these are examples of the present invention, and various configurations other than the above can be adopted. In addition, the present invention is not limited to the above-mentioned embodiments, and modifications and improvements within the scope of achieving the purpose of the present invention are included in the present invention.
[0113] Example
[0114] The embodiments of the present invention will be described in detail based on examples and comparative examples. However, for the sake of caution, it should be noted that the present invention is not limited to the examples.
[0115] <Manufacturing of phosphor powder>
[0116] (Example 1)
[0117] (1) Preparation of raw material mixed powder
[0118] First, premixing was performed. Specifically, Si3N4, AlN and CeO2 in the raw materials listed in Table 1 were mixed for 30 minutes (dry mixing) using a small V-type mixer, and then sieved using a nylon sieve with a mesh size of 150 μm. Thus, a premixed powder was obtained.
[0119] Next, in a glove box with a nitrogen atmosphere, the remaining raw materials (Ca3N2 and Li3N) listed in Table 1 were added to the premixed powder, and the mixture was thoroughly dry-mixed and then sieved with a sieve having a mesh size of 500 μm. Thus, a raw material mixed powder was obtained.
[0120] (2) Calcination
[0121] The raw material mixed powder was filled into a container made of boron nitride, and the container was placed in a furnace, and the raw material mixed powder was calcined at 1800° C. for 8 hours in a 0.72 MPa·G N 2 atmosphere.
[0122] (3) Crushing of calcined material
[0123] The calcined product obtained in (2) was pulverized using a stamp mill. The pulverization using the stamp mill was repeated until the passing rate of a vibration sieve with a mesh size of 250 μm exceeded 90%.
[0124] The calcined product obtained by the pulverization by the stamp mill was further pulverized using a jet mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd., PJM-80SP) under the conditions of sample supply rate: 50 g / min, pulverization gas pressure: 0.3 MPa.
[0125] (4) Acid treatment
[0126] The pulverized calcined product is put into hydrochloric acid for acid treatment.
[0127] Specifically, first, a hydrochloric acid aqueous solution was prepared by mixing 35-37 mass % hydrochloric acid and distilled water at a volume ratio of 50 mL:300 mL and heating to 80° C. The calcined product crushed in (3) was added to the hydrochloric acid aqueous solution and stirred for 0.5 hours for acid treatment.
[0128] The acid-treated calcined product was thoroughly washed with distilled water and then dried at 110° C. for 3 hours. Thereafter, the calcined product was passed through a sieve with an opening of 45 μm to remove coarse and aggregated particles.
[0129] (5) Removal of fine powder by sedimentation classification
[0130] First, a 0.05 mass % sodium hexametaphosphate aqueous solution was prepared, and then the aqueous solution was added to a container having an inner diameter of 70 mm and a height of 120 mm until the height reached 110 mm.
[0131] Next, the acid-treated calcined product was added to the above-mentioned container with the aqueous solution, stirred thoroughly to disperse it, and then allowed to stand for 22 minutes. After standing, the supernatant of 90 mm from the top was discharged. Thereafter, sodium hexametaphosphate aqueous solution was added until the height reached 110 mm, and the powder was dispersed by stirring again and the same treatment was performed. This operation was repeated 7 times to remove the fine powder contained in the acid-treated powder. (By the way, based on Stokes' law, the classification point is 7.5 μm.)
[0132] Thereafter, the slurry at the bottom of the container was filtered while being washed with water to recover the solid content, which was then dried at 110° C. for 3 hours and passed through a sieve with an opening of 45 μm to break up the aggregated particles.
[0133] Through the above operation, phosphor powder is obtained.
[0134] (Example 2)
[0135] A phosphor powder was obtained in the same manner as in Example 1 except that sedimentation classification was not performed.
[0136] (Example 3)
[0137] (a) using the materials listed in Table 1 as raw materials; (b) not performing acid treatment (the calcined product crushed by the jet mill is subjected to sedimentation classification without acid treatment); and (c) setting the pulverizing gas pressure in the jet mill to 0.6 MPa, the phosphor powder is obtained in the same manner as in Example 1.
[0138] (Example 4)
[0139] A phosphor powder was obtained in the same manner as in Example 1 except that (a) the materials listed in Table 1 were used as raw materials; and (b) sedimentation classification was not performed.
[0140] (Example 5)
[0141] The phosphor powder was obtained in the same manner as in Example 4 except that nitric acid having a concentration of 60% by mass was used instead of hydrochloric acid for the acid treatment.
[0142] (Example 6)
[0143] A phosphor powder was obtained in the same manner as in Example 1 except that (a) the materials listed in Table 1 were used as raw materials; and (b) no acid treatment was performed (the calcined product pulverized by the jet mill was subjected to sedimentation classification without acid treatment).
[0144] (Comparative Example 1)
[0145] A phosphor powder was obtained in the same manner as in Example 4 except that the acid treatment was not performed.
[0146] (Example 7)
[0147] The phosphor powder was obtained in the same manner as in Example 1 except that (a) the materials listed in Table 1 were used as raw materials; (b) no acid treatment was performed (the calcined product crushed by a jet mill was subjected to sedimentation classification without acid treatment); and (c) the calcined product crushed by a jet mill was passed through a sieve with a mesh size of 45 μm to remove coarse / agglomerated particles and then subjected to sedimentation classification.
[0148] <Confirmation of chemical composition / crystal structure>
[0149] The composition of a part of the phosphor powder was analyzed as follows.
[0150] Amounts of Ca, Li, Ce, Si, and Al: The phosphor powder was melted by an alkali fusion method, and then measured using an ICP emission spectrometer (CIROS-120 manufactured by Rigaku Corporation).
[0151] Amounts of O and N: Measured using an oxygen and nitrogen analyzer (EMGA-920, manufactured by HORIBA Corporation).
[0152] Based on the measurement results, the general formula M is obtained. x (Si,Al)2(N,O) 3±y x, y, Si / Al atomic ratio, O / N atomic ratio, Li ratio of M and Ce ratio of M.
[0153] In addition, regarding the Cr element and the Fe element as impurities, the phosphor powder was dissolved by a pressurized acid decomposition method using a mixed acid of hydrofluoric acid and nitric acid, and then measured using an ICP emission spectrometer.
[0154] The phosphor of Example 1 was also subjected to X-ray powder diffraction (XRD) using Cu-Kα rays using an X-ray diffractometer (Ultima IV-N manufactured by Rigaku Corporation). The obtained XRD pattern is shown in FIG. Figure 2 According to the analysis of the obtained XRD pattern, it was confirmed that the main phase was an orthorhombic crystal with lattice constants of a=0.9486nm, b=0.5586nm, and c=0.4933nm, and a small amount of LiAlSi2N4 existed as a heterophase.
[0155] Incidentally, the mixing ratio of the raw materials was the same in all Examples 3, 4, and 5, and the manufacturing process until the pulverization of the calcined product was the same in all these Examples. Therefore, the chemical composition of the phosphor powders of Examples 4 and 5 was considered to be almost the same as that of the phosphor powder of Example 3, and therefore the chemical composition of the phosphor powders of Examples 4 and 5 was not measured.
[0156] <Measurement of light absorbance at a wavelength of 700 nm>
[0157] The light absorption rate of each phosphor powder at a wavelength of 700 nm was determined according to the following procedure using a spectrophotometer equipped with an integrating sphere (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.).
[0158] (1) A standard reflector plate (Spectralon manufactured by Labsphere) with a reflectivity of 99% was installed at a predetermined position (sample portion) in the integrating sphere, and monochromatic light with a wavelength of 700 nm from a light source (Xe lamp) was irradiated onto the standard reflector plate. Then, the number of photons (Qex) of the excitation light was calculated in the wavelength range of 695 to 710 nm.
[0159] (2) The same procedure as (1) is performed except that the standard reflector is replaced by the measurement sample to calculate the number of excitation reflected photons (Qref) of the sample. As the measurement sample, a sample in which the concave portion of a concave groove is filled with phosphor powder so that the surface is smooth is used.
[0160] (3) According to the formula (Qex-Qref) / Qex, calculate the light absorption rate A at a wavelength of 700nm 700 .
[0161] <Measurement of light absorbance at a wavelength of 600 nm>
[0162] The light absorption rate of each phosphor powder at a wavelength of 600 nm was determined according to the following procedure using a spectrophotometer equipped with an integrating sphere (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.).
[0163] (1) A standard reflector plate (Spectralon manufactured by Labsphere) with a reflectivity of 99% is installed at a predetermined position (sample portion) in the integrating sphere, and monochromatic light with a wavelength of 600 nm from a light source (Xe lamp) is irradiated onto the standard reflector plate. Then, the number of photons (Qex) of the excitation light is calculated in the wavelength range of 595 to 610 nm.
[0164] (2) The same procedure as (1) is performed except that the standard reflector is replaced by the measurement sample to calculate the number of excitation reflected photons (Qref) of the sample. As the measurement sample, a sample in which the concave portion of a concave groove is filled with phosphor powder so that the surface is smooth is used.
[0165] (3) According to the formula (Qex-Qref) / Qex, calculate the light absorption rate A at a wavelength of 600nm 600 .
[0166] <Measurement of particle size distribution>
[0167] The particle size distribution was measured using LS13 320 (manufactured by Beckman Coulter, Inc.) by a laser diffraction scattering method in accordance with JIS R1629: 1997. Water was used as a measurement solvent.
[0168] As a specific procedure, first, a small amount of phosphor powder is added to an aqueous solution of sodium hexametaphosphate as a dispersant at 0.05 mass%. Next, a horn-type ultrasonic homogenizer (output 300W, horn diameter 26mm) is used to perform a dispersion treatment to prepare a dispersion liquid. The particle size distribution is measured using the dispersion liquid. The 10% volume diameter (D 10 ), 50% volume diameter (D 50 ) and 90% volume diameter (D 90 ).
[0169] <Evaluation>
[0170] (Fluorescence peak intensity)
[0171] The fluorescence spectrum of the phosphor powder was measured using a fluorescence spectrophotometer (F-7000 manufactured by Hitachi High-Tech Corporation) calibrated with rhodamine B and a sub-standard light source. Specifically, the spectrum of fluorescence emitted by the phosphor powder when excited with monochromatic light of a wavelength of 455 nm was measured to determine the fluorescence peak intensity and fluorescence peak wavelength.
[0172] The fluorescence peak intensity varies depending on the measuring device and conditions. The fluorescence peak intensity described in the table below is a value when the fluorescence peak intensity of the standard sample (YAG, more specifically, P46Y3 manufactured by Mitsubishi Chemical Corporation) is set to 100.
[0173] (Internal quantum efficiency and external quantum efficiency)
[0174] The internal quantum efficiency and external quantum efficiency of each phosphor powder were determined by the following procedure using a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.).
[0175] (1) Fill the concave part of the concave groove with phosphor powder in a smooth surface. Install the concave groove in a specified position (sample part) in the integrating sphere. Use optical fiber to introduce monochromatic light from a light source (Xe lamp) with a wavelength of 455nm into the integrating sphere. Irradiate the monochromatic light (excitation light) to the phosphor powder filled in the concave part of the concave groove, and measure the fluorescence spectrum. Calculate the peak wavelength from the obtained spectral data, and calculate the number of excitation reflected light photons (Qref) and the number of fluorescence photons (Qem). Calculate the number of excitation reflected light photons in the wavelength range of 450nm to 465nm, and calculate the number of fluorescence photons in the range of 465nm to 800nm.
[0176] (2) In addition, a standard reflector plate (Spectralon manufactured by Labsphere) with a reflectivity of 99% was installed on the sample portion instead of the concave groove, and the spectrum of the excitation light with a wavelength of 455 nm was measured. Then, the number of excitation light photons (Qex) was calculated from the spectrum in the wavelength range of 450 nm to 465 nm.
[0177] (3) The internal quantum efficiency and the external quantum efficiency are calculated from Qref, Qem and Qex obtained in (1) and (2) above according to the following formula.
[0178] Internal quantum efficiency = (Qem / (Qex-Qref)) × 100
[0179] External quantum efficiency = (Qem / Qex) × 100
[0180] Various information is shown in Table 1.
[0181] In Table 1, "ND" is the abbreviation for Not Detected.
[0182] In addition, in Table 1, each raw material described in the column of "Raw materials used" is as follows.
[0183] Ca3N2-1: Ca3N2 made by TAIHEIYO CEMENT CORPORATION
[0184] Ca3N2-2: Ca3N2 made by CERAC (now Materion)
[0185] Li3N-1: Li3N made by Materion
[0186] Li3N-2: Li3N made by CERAC (now Materion)
[0187] Li3N-3: Li3N produced by a high-purity chemical research institute
[0188] CeO2-1: CeO2 manufactured by Shin-Etsu Chemical Co., Ltd., C grade
[0189] Si3N4-1: Si3N4 manufactured by Ube Industries, E10 grade
[0190] AlN-1: AlN manufactured by Tokuyama Corporation, E grade [Table 1]
[0191]
[0192] As shown in Table 1, it comprises the general formula M x (Si,Al)2(N,O) 3±y The light absorption rate of the phosphor particles at a wavelength of 700nm is A 700 The phosphor powders with a concentration of 10% or less (Examples 1 to 7) showed good fluorescence peak intensity, internal quantum efficiency, and external quantum efficiency.
[0193] On the other hand, A 700 The phosphor powder with a content of more than 10% (Comparative Example 1) is inferior to Examples 1 to 7 at least in terms of internal quantum efficiency.
[0194] If we look at Table 1 more carefully, we can see from the comparison between Examples 1 to 6 and Example 7 that by making A 600 -A 700 The relative fluorescence peak intensity, internal quantum efficiency and external quantum efficiency are further improved.
[0195] This application claims priority based on Japanese patent application No. 2020-189210 filed on November 13, 2020, and all the disclosed contents are cited herein.
[0196] Explanation of symbols
[0197] 1 Phosphor particles
[0198] 30 Sealing material
[0199] 40 Complex
[0200] 100 Lighting Device
[0201] 120 Light emitting element
[0202] 130 Heat sink
[0203] 140 Housing
[0204] 150 1st lead frame
[0205] 160 2nd lead frame
[0206] 170 welding wire
[0207] 172 welding wire
Claims
1. A phosphor powder comprising phosphor particles, wherein the phosphor particles are of the general formula M x (Si,Al)2(N,O) 3±y A phosphor wherein M is Li and one or more alkaline earth metal elements, 0.52≤x≤0.9, 0.06≤y≤0.36, a portion of M is substituted by a Ce element, the Si / Al atomic ratio is 1.5 to 6, and the O / N atomic ratio is 0 to 0.1, 5 to 50 mol% of M is Li, and 0.5 to 10 mol% of M is Ce, The light absorption rate A of the phosphor powder at a wavelength of 700 nm is measured according to the following measurement of the light absorption rate at a wavelength of 700 nm: 700 Less than 10%, Determination of light absorbance at a wavelength of 700nm: Use a spectrophotometer equipped with an integrating sphere to determine the light absorption rate of the phosphor powder at a wavelength of 700 nm according to the following steps: (1) A standard reflector is installed at a predetermined position in the integrating sphere, and monochromatic light with a wavelength of 700 nm from a light source is irradiated onto the standard reflector. Then, the number of photons of the excitation light, i.e., Qex, is calculated in the wavelength range of 695 to 710 nm. (2) The same procedure as (1) is performed except that the standard reflector is replaced by the measurement sample, and the number of excited reflected photons of the sample, i.e., Qref, is calculated. (3) According to the formula (Qex-Qref) / Qex, calculate the light absorption rate A at a wavelength of 700nm 700 .
2. The phosphor powder according to claim 1, wherein The light absorbance at a wavelength of 600 nm measured by the following measurement of the light absorbance at a wavelength of 600 nm is defined as A. 600 When A 600 The value of A minus 700 The value obtained is 6% to 10%, Determination of light absorbance at a wavelength of 600nm: Use a spectrophotometer equipped with an integrating sphere to determine the light absorption rate of the phosphor powder at a wavelength of 600 nm according to the following steps: (1) A standard reflector is installed at a predetermined position in the integrating sphere, and monochromatic light with a wavelength of 600 nm from a light source is irradiated onto the standard reflector. Then, the number of photons of the excitation light, i.e., Qex, is calculated in the wavelength range of 595 to 610 nm. (2) The same procedure as (1) is performed except that the standard reflector is replaced by the measurement sample, and the number of excited reflected photons of the sample, i.e., Qref, is calculated. (3) According to the formula (Qex-Qref) / Qex, calculate the light absorption rate A at a wavelength of 600nm 600 .
3. The phosphor powder according to claim 1 or 2, wherein Volume-based cumulative 50% diameter D measured by laser diffraction scattering method 50 8μm~25μm.
4. The phosphor powder according to claim 1 or 2, wherein Volume-based cumulative 10% diameter D measured by laser diffraction scattering method 10 5μm~12μm. 5 . A light-emitting device comprising the phosphor powder according to claim 1 and a light source.
6. The light emitting device according to claim 5, wherein: Luminescent light sources emit ultraviolet or visible light.
7. An image display device comprising the light emitting device according to claim 5 or 6.
8. A lighting device comprising the light emitting device according to claim 5 or 6.
Citation Information
Patent Citations
Rocking device for cable crane
JP1984069391A