Schiff base / methyl methacrylate composite material and preparation method and application thereof

By preparing a colorless and transparent Schiff base/methyl methacrylate composite material, the problem of the dark color of 3,5-di-tert-butyl salicylaldehyde aniline powder is solved, and rapid coloration and visible light stimulation are achieved The photochromic properties can be restored at low temperature and are suitable for a variety of applications.

CN116515020BActive Publication Date: 2024-10-11ANHUI EASPEED TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310484712.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-11
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

3,5-Di-tert-butylsalicylaldehyde aniline powder is dark and opaque, which hinders the widespread application of Schiff bases in photochromism.

Method used

By mixing Schiff base, methyl methacrylate and initiator, and heating and cooling, a colorless and transparent Schiff base/methyl methacrylate composite material is prepared, and the initiator is used to polymerize methyl methacrylate. , Schiff bases are dispersed randomly inside the polymer to achieve photochromism of the material.

Benefits of technology

The obtained composite material is quickly colored under ultraviolet light stimulation, quickly recovers under visible light stimulation, is colorless and transparent, has good photochromic properties, and is suitable for use in transparent displays, batteries, wearable devices and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116515020B_ABST
    Figure CN116515020B_ABST
Patent Text Reader

Abstract

The present invention provides a Schiff base / methyl methacrylate composite material and a preparation method and application thereof. The method for preparing the Schiff base / methyl methacrylate composite material comprises: mixing a Schiff base, methyl methacrylate and an initiator, and subjecting the mixture to heating and cooling treatment to obtain the Schiff base / methyl methacrylate composite material, wherein the Schiff base comprises 3,5-di-tert-butyl salicylaldehyde aniline. Thus, the preparation method is simple, and the obtained Schiff base / methyl methacrylate composite material is colorless and transparent, can be quickly colored under ultraviolet light stimulation, and quickly recovers under visible light stimulation, and has good photochromic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of organic photochromism and high molecular polymers, and in particular, to a Schiff base / methyl methacrylate composite material and a preparation method and application thereof. Background Art

[0002] Salicylaldehyde aniline is an aromatic Schiff base. This type of molecule exhibits excellent photochromic properties and has great application potential in the fields of optical information storage, anti-counterfeiting, textiles, wearable devices, etc., which has aroused great interest among scientific researchers. Salicylaldehyde aniline and its derivatives have good fatigue resistance, and the life of their photochromic forms in the crystalline state can reach hundreds of days. The simplest and most common photochromic cycle hypothesis of salicylaldehyde aniline and its derivatives is as follows. After the initial enol (trans-enol) tautomer is excited, ultrafast excited state intramolecular proton transfer (ESIPT) occurs to form an excited state ketone tautomer (cis-ketone or its zwitterionic form), which exhibits a strong Stokes shift fluorescence band. Having a sufficiently large reaction volume for photoinduced isomerization in a confined medium is a way to improve the photochromic ability of salicylaldehyde aniline derivatives. Therefore, 3,5-di-tert-butyl salicylaldehyde aniline with a di-tert-butyl group introduced into the structure has a more stable photochromic ability. In many application scenarios such as optical films, photochromic glasses, transparent displays, etc., the material is required to be colorless and transparent, but the 3,5-di-tert-butyl salicylaldehyde aniline powder is dark and opaque, which hinders the widespread application of Schiff base in photochromism. This application aims to propose a method for preparing a Schiff base / methyl methacrylate composite material to solve the above problem. Summary of the invention

[0003] The present invention aims to solve one of the technical problems in the related art at least to a certain extent.

[0004] In one aspect of the present invention, a method for preparing a Schiff base / methyl methacrylate composite material is proposed, the method comprising: mixing a Schiff base, methyl methacrylate, and an initiator, and subjecting the mixture to heating and cooling treatment to obtain a Schiff base / methyl methacrylate composite material, wherein the Schiff base comprises 3,5-di-tert-butyl salicylaldehyde aniline. Thus, the preparation method is simple, and the obtained Schiff base / methyl methacrylate composite material is colorless and transparent, can be quickly colored under ultraviolet light stimulation, and can be quickly restored under visible light stimulation, and has good photochromic properties.

[0005] According to some embodiments of the present invention, the method further includes uniformly mixing the Schiff base and the methyl methacrylate to obtain a first mixture; mixing the first mixture with the initiator to obtain a second mixture, and heating and cooling the second mixture to obtain the Schiff base / methyl methacrylate composite material.

[0006] According to some embodiments of the present invention, the mass ratio of the 3,5-di-tert-butyl salicylaldehyde aniline to the methyl methacrylate is 1:100000 to 1:1000.

[0007] According to some embodiments of the present invention, the mass ratio of the 3,5-di-tert-butyl salicylaldehyde aniline to the methyl methacrylate is 1:50000 to 1:1000.

[0008] According to some embodiments of the present invention, the mass ratio of the initiator to the methyl methacrylate is 1:1000 to 1:100.

[0009] According to some embodiments of the present invention, the method includes: subjecting the second mixture to a first heating treatment to obtain a first reactant; cooling the first reactant and placing it in a mold; subjecting the cooled first reactant to a second heating treatment and cooling to obtain a second reactant; subjecting the second reactant to a third heating treatment and cooling to obtain the Schiff base / methyl methacrylate composite material, wherein the temperature of the third heating treatment is greater than the temperature of the first heating treatment, and the temperature of the first heating treatment is greater than the temperature of the second heating treatment.

[0010] According to some embodiments of the present invention, the method satisfies at least one of the following conditions: the temperature of the first heating treatment is 80°C to 95°C; the temperature of the second heating treatment is 40°C to 60°C; the temperature of the third heating treatment is 90°C to 120°C.

[0011] According to some embodiments of the present invention, the initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile and benzoyl peroxide.

[0012] In another aspect of the present invention, a Schiff base / methyl methacrylate composite material is provided, which is prepared by the above method. Thus, the Schiff base / methyl methacrylate composite material is colorless and transparent, can be quickly colored under ultraviolet light stimulation, and can be quickly restored under visible light stimulation, and has good photochromic properties.

[0013] In another aspect of the present invention, an application of the aforementioned Schiff base / methyl methacrylate composite material is proposed, including at least one of the fields of transparent display, battery, wearable device, and three-dimensional data storage. Therefore, when the Schiff base / methyl methacrylate composite material is used in the relevant devices in the above fields, its good photochromic performance and anti-fatigue ability can be exerted. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0015] Figure 1 A schematic flow chart of a method for preparing a Schiff base / methyl methacrylate composite material according to an embodiment of the present invention is shown.

[0016] Figure 2 The absorption spectra and photos of the composite material prepared in Example 1 before and after photochromism are shown.

[0017] Figure 3 The absorption spectrum and photos of the composite material prepared in Example 2 before and after photochromism are shown.

[0018] Figure 4 The absorption spectra and photos of the composite material prepared in Example 3 before and after photochromism are shown.

[0019] Figure 5 The absorption spectra and photos of the composite material prepared in Example 4 before and after photochromism are shown.

[0020] Figure 6 The absorption spectra and photos of the composite material prepared in Example 5 before and after photochromism are shown.

[0021] Figure 7 The absorption spectra and photos of the composite material prepared in Example 6 before and after photochromism are shown.

[0022] Figure 8 The absorption spectrum and photos of the composite material prepared in Example 7 before and after photochromism are shown.

[0023] Fig. 9 The absorption spectra and photos of the composite material prepared in Example 8 before and after photochromism are shown.

[0024] Fig.10 The absorption spectra and photos of the composite material prepared in Example 9 before and after photochromism are shown.

[0025] Fig.11 The absorption spectrum and photographs of the composite material prepared in Example 10 before and after photochromism are shown.

[0026] Fig.12 The absorption spectra and photos of pure polymethyl methacrylate prepared in Comparative Example 1 before and after photochromism are shown.

[0027] Fig.13 The photographs of 3,5-di-tert-butyl salicylaldehyde aniline prepared in Comparative Example 2 before and after photochromism are shown. DETAILED DESCRIPTION

[0028] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.

[0029] In one aspect of the present invention, a method for preparing a Schiff base / methyl methacrylate composite material is proposed, comprising: mixing a Schiff base, methyl methacrylate, and an initiator, and subjecting the mixture to heating and cooling treatment to obtain a Schiff base / methyl methacrylate composite material, wherein the Schiff base comprises 3,5-di-tert-butyl salicylaldehyde aniline. Specifically, the initiator polymerizes the methyl methacrylate, and the Schiff base is randomly dispersed inside the polymerized methyl methacrylate. Thus, the preparation method is simple, and the obtained Schiff base / methyl methacrylate composite material is colorless and transparent, can be quickly colored under ultraviolet light stimulation, and can be quickly restored under visible light stimulation, and has good photochromic properties.

[0030] According to some embodiments of the present invention, the method further comprises: uniformly mixing the 3,5-di-tert-butyl salicylaldehyde aniline and the methyl methacrylate to obtain a first mixture; mixing the first mixture with the initiator to obtain a second mixture, and heating and cooling the second mixture to obtain the Schiff base / methyl methacrylate composite material. Thus, the 3,5-di-tert-butyl salicylaldehyde aniline and methacrylic acid are first mixed and then the initiator is added. During the polymerization of methyl methacrylate, the 3,5-di-tert-butyl salicylaldehyde aniline can be further wrapped inside the polymerized methyl methacrylate to improve the photochromic properties of the Schiff base / methyl methacrylate.

[0031] According to some embodiments of the present invention, the mass ratio of the 3,5-di-tert-butyl salicylaldehyde aniline to the methyl methacrylate is 1:100000 to 1:1000. Specifically, the mass ratio of the 3,5-di-tert-butyl salicylaldehyde aniline to the methyl methacrylate may be 1:90000 to 1:2000, 1:80000 to 1:3000, 1:70000 to 1:4000, 1:60000 to 1:5000, 1:50000 to 1:6000, 1:40000 to 1:7000, 1:30000 to 1:8000, or 1:20000 to 1:9000, etc. If the content of 3,5-di-tert-butyl salicylaldehyde aniline is too much, it will affect the color of the Schiff base / methyl methacrylate composite material to a certain extent, making the color of the Schiff base / methyl methacrylate composite material darker or even yellowish; if the content of 3,5-di-tert-butyl salicylaldehyde aniline is too little, it will affect the photochromic effect of the Schiff base / methyl methacrylate composite material to a certain extent.

[0032] According to some embodiments of the present invention, the mass ratio of the 3,5-di-tert-butyl salicylaldehyde aniline to the methyl methacrylate is 1:50000 to 1:1000. For example, the mass ratio of the 3,5-di-tert-butyl salicylaldehyde aniline to the methyl methacrylate may be 1:40000 to 1:2000, 1:30000 to 1:3000, 1:20000 to 1:4000, 1:10000 to 1:5000, 1:9000 to 1:6000, 1:8000 to 1:7000, etc.

[0033] According to some embodiments of the present invention, the mass ratio of the initiator to the methyl methacrylate is 1:1000 to 1:100. For example, the mass ratio of the initiator to the methyl methacrylate may be between 1:900 and 1:200, 1:800 to 1:300, 1:700 to 1:400, or 1:600 ​​to 1:500. If the content of the initiator is too little, the polymerization rate of the methyl methacrylate will be reduced to a certain extent; if the content of the initiator is too much, the intensity of the polymerization of the methyl methacrylate will be increased to a certain extent, causing implosion.

[0034] According to some embodiments of the present invention, the method for preparing a Schiff base / methyl methacrylate composite material may further include: subjecting the second mixture to a first heating treatment to obtain a first reactant; cooling the first reactant and placing it in a mold; subjecting the cooled first reactant to a second heating treatment and cooling to obtain a second reactant; subjecting the second reactant to a third heating treatment and cooling to obtain the Schiff base / methyl methacrylate composite material, wherein the temperature of the third heating treatment is greater than the temperature of the first heating treatment, and the temperature of the first heating treatment is greater than the temperature of the second heating treatment. Thus, by heating the second mixture in sections to control the speed of the polymerization reaction and prevent implosion during the polymerization process, the photochromic properties of the Schiff base / methyl methacrylate composite material are improved.

[0035] The various steps of the present invention are described in detail below. Figure 1 , the method for preparing the Schiff base / methyl methacrylate composite material may include:

[0036] S100: Mix 3,5-di-tert-butyl salicylaldehyde aniline, methyl methacrylate and initiator

[0037] Specifically, in this step, the 3,5-di-tert-butyl salicylaldehyde aniline and the methyl methacrylate are firstly mixed uniformly to obtain a first mixture, and then the first mixture is mixed with an initiator to obtain a second mixture.

[0038] S200: Performing a first heating treatment on the second mixture to obtain a first reactant

[0039] Specifically, in this step, the temperature of the first heat treatment can be 80°C to 95°C. For example, it can be 82°C, 84°C, 86°C, 88°C, 90°C, 92°C or 94°C, etc. According to some embodiments of the present invention, the heating method is not particularly limited, and the second mixture can be placed in a water bath for heating. During the heating process, methyl methacrylate polymerizes. Due to the low heating temperature, the polymerization reaction proceeds slowly. It should be noted that the time for the first heat treatment is not particularly limited, and those skilled in the art can control it according to actual needs. Specifically for the present application, the first heat treatment can be terminated when the polymerization reaction proceeds to about 15% to 25%.

[0040] S300: Cooling the first reactant

[0041] Specifically, in this step, the temperature of the cooled first reactant is not particularly limited. For example, the first reactant can be cooled to 30° C. to 40° C. and poured into a mold.

[0042] S400: performing a second heating treatment on the cooled first reactant to obtain a second reactant

[0043] Specifically, in this step, the temperature of the second heating treatment is 40°C to 60°C, for example, it can be 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C or 58°C, etc. According to some embodiments of the present invention, the method of the second heating treatment is not particularly limited, and the first reactant can be placed in a water bath for heating, and methyl methacrylate continues to undergo polymerization during the heating process. It should be noted that the time for the second heating treatment is not particularly limited, and those skilled in the art can control it according to actual needs. Specifically for the present application, the time for the second heating treatment can be 10h to 40h, for example, it can be 15h, 20h, 25h, 30h or 35h, etc.

[0044] S500: The second mixture is subjected to a third heating treatment and cooled to obtain a Schiff base / methyl methacrylate composite material

[0045] Specifically, in this step, the temperature of the third heating treatment can be 90° C. to 120° C., for example, 95° C., 100° C., 105° C., 110° C. or 115° C. Thus, methyl methacrylate is completely polymerized to obtain a solid Schiff base / methyl methacrylate composite material, which can be demolded after slowly cooling to room temperature.

[0046] In another aspect of the present invention, a Schiff base / methyl methacrylate composite material is provided, which is prepared by the above method. Thus, the Schiff base / methyl methacrylate composite material is colorless and transparent, can be quickly colored under ultraviolet light stimulation, and can be quickly restored under visible light stimulation, and has good photochromic properties.

[0047] In another aspect of the present invention, an application of the aforementioned Schiff base / methyl methacrylate composite material is proposed, including at least one of the fields of transparent display, battery, wearable device, and three-dimensional data storage. Therefore, when the Schiff base / methyl methacrylate composite material is used in the relevant devices in the above fields, its good photochromic performance and anti-fatigue ability can be exerted.

[0048] According to some embodiments of the present invention, the Schiff base / methyl methacrylate composite material can be used in transparent displays, solar cells, organic light emitting diodes, three-dimensional data storage, optical films, photochromic glasses, wearable devices, etc.

[0049] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.

[0050] Example 1

[0051] 3,5-di-tert-butyl salicylaldehyde aniline and methyl methacrylate are uniformly mixed in a mass ratio of 1:10000, 0.4% benzoyl peroxide is added based on the total mass of methyl methacrylate, and prepolymerized in a water bath at 85°C until the raw material liquid has a glycerol viscosity, the raw material liquid is cooled to 30°C and poured into a mold, placed in a 50°C water bath for insulation for 10 hours, and finally high-temperature polymerized at 100°C for 1 hour, slowly cooled to room temperature, and demolded to obtain a Schiff base / methyl methacrylate composite material.

[0052] After irradiation with 365nm ultraviolet light for 5s, the composite material absorbs visible light in the range of 400-550nm and changes from colorless to orange-yellow, and recovers after irradiation with visible light. Figure 2 .

[0053] Example 2

[0054] The specific preparation process is the same as that of Example 1, except that the mass ratio of 3,5-di-tert-butyl salicylaldehyde aniline to methyl methacrylate is 1:50000.

[0055] After irradiation with 365nm ultraviolet light for 5s, the composite material absorbs visible light in the range of 400-550nm and changes from colorless to orange-yellow, and recovers after irradiation with visible light. Figure 3 .

[0056] Example 3

[0057] The specific preparation process is the same as that of Example 1, except that the mass ratio of 3,5-di-tert-butyl salicylaldehyde aniline to methyl methacrylate is 1:90000.

[0058] After irradiation with 365nm ultraviolet light for 5s, the composite material absorbs visible light in the range of 400-550nm and changes from colorless to orange-yellow, and recovers after irradiation with visible light. Figure 4 .

[0059] Example 4

[0060] The specific preparation process is the same as that of Example 1, except that the mass ratio of 3,5-di-tert-butyl salicylaldehyde aniline to methyl methacrylate is 1:1100.

[0061] After irradiation with 365nm ultraviolet light for 5s, the composite material absorbs visible light in the range of 400-550nm and changes from colorless to orange-yellow, and recovers after irradiation with visible light. Figure 5 .

[0062] Example 5

[0063] The specific preparation process is the same as that in Example 1, except that the mass ratio of 3,5-di-tert-butyl salicylaldehyde aniline to methyl methacrylate is 1:200000.

[0064] After the composite material was irradiated with 365nm ultraviolet light for 5s, Figure 6 , weakly absorbing visible light in the range of 400-550nm, changing from colorless to light yellow. The photochromic phenomenon is not obvious, mainly due to the low doping amount of 3,5-di-tert-butyl salicylaldehyde aniline.

[0065] Example 6

[0066] The specific preparation process is the same as that of Example 1, except that the mass ratio of 3,5-di-tert-butyl salicylaldehyde aniline to methyl methacrylate is 1:500.

[0067] After the composite material was irradiated with 365nm ultraviolet light for 5s, Figure 7 The absorption peak at 400-550nm is not obvious and the color is too dark, which is mainly caused by excessive doping of 3,5-di-tert-butyl salicylaldehyde aniline, which prevents ultraviolet light from penetrating.

[0068] Example 7

[0069] The specific preparation process is the same as that of Example 1, except that 0.9% benzoyl peroxide is added based on the total mass of methyl methacrylate.

[0070] The composite material has a uniform and transparent appearance. After being irradiated with 365nm ultraviolet light for 5s, it absorbs visible light in the range of 400-550nm and changes from colorless to orange-yellow. It recovers after irradiation with visible light. Figure 8 .

[0071] Example 8

[0072] The specific preparation process is the same as that of Example 1, except that 0.12% of benzoyl peroxide is added based on the total mass of methyl methacrylate.

[0073] The composite material has a uniform and transparent appearance. After being irradiated with 365nm ultraviolet light for 5s, it absorbs visible light in the range of 400-550nm and changes from colorless to orange-yellow. It recovers after irradiation with visible light. Fig. 9 .

[0074] Example 9

[0075] The specific preparation process is the same as that of Example 1, except that, based on the total mass of methyl methacrylate, 0.08% benzoyl peroxide is added, and the insulation time in a 50° C. water bath is extended to 45 h.

[0076] like Fig.10 The composite material has a uniform, transparent appearance and can be photochromic, but the polymerization time is too long, which affects the production efficiency.

[0077] Example 10

[0078] The specific preparation process is the same as that of Example 1, except that 1.5% benzoyl peroxide is added based on the total mass of methyl methacrylate.

[0079] Due to the intense heat release during the polymerization process, the composite material is not uniformly transparent. However, the block can still photochromic after being irradiated with 365nm ultraviolet light for 5s, such as Fig.11 .

[0080] Comparative Example 1

[0081] Add 0.4% benzoyl peroxide to methyl methacrylate and prepolymerize it in a 85°C water bath until the raw material liquid has a glycerol viscosity. The raw material liquid is cooled to 30°C and poured into a mold. It is placed in a 50°C water bath and kept warm for 10 hours. Finally, it is high-temperature polymerized at 100°C for 1 hour, slowly cooled to room temperature, and demolded to obtain pure polymethyl methacrylate.

[0082] Polymethyl methacrylate showed no change after being irradiated with 365nm ultraviolet light for 5s. Fig.12 .

[0083] Comparative Example 2

[0084] 3,5-di-tert-butyl salicylaldehyde (0.47 g, 2 mmol) and aniline (0.28 g, 2 mmol) were mixed in 20 mL of anhydrous ethanol, heated to reflux at 78°C, and reacted for 4 hours under stirring; after the reaction, the solvent was removed by rotary evaporation to obtain a crude product, which was recrystallized from anhydrous ethanol to obtain 3,5-di-tert-butyl salicylaldehyde aniline.

[0085] After irradiation with 365nm ultraviolet light for 5s, the 3,5-di-tert-butyl salicylaldehyde aniline powder changes from yellow to orange, and recovers after irradiation with visible light. Fig.13 .

[0086] Test method:

[0087] UV-Vis absorption spectrum: A 1cm thick pure PMMA transparent block was used as the standard sample to scan the baseline in the range of 300-700nm. The samples to be tested were cut, ground and polished to a thickness of 1cm, and the UV-Vis absorption spectrum data were tested before and after irradiation with 365nm UV light for 5s, and the test temperature was 15℃.

[0088] In the present invention, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0089] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0090] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a Schiff base / methyl methacrylate composite material, characterized in that: include: The Schiff base, methyl methacrylate and an initiator are mixed, and the mixture is heated and cooled to obtain a Schiff base / methyl methacrylate composite material, wherein the Schiff base includes 3,5-di-tert-butyl salicylaldehyde aniline. The mass ratio of the 3,5-di-tert-butyl salicylaldehyde aniline to the methyl methacrylate is 1:100000 to 1:1000; The mass ratio of the initiator to the methyl methacrylate is 1:1000 to 1:

100. Mixing the 3,5-di-tert-butyl salicylaldehyde aniline and the methyl methacrylate evenly to obtain a first mixture; mixing the first mixture with the initiator to obtain a second mixture; subjecting the second mixture to a first heating treatment to obtain a first reactant; Cooling the first reactant and placing it in a mold; The cooled first reactant is subjected to a second heating treatment and then cooled to obtain a second reactant; The second reactant is subjected to a third heating treatment and then cooled to obtain the Schiff base / methyl methacrylate composite material. The temperature of the third heating treatment is higher than the temperature of the first heating treatment, and the temperature of the first heating treatment is higher than the temperature of the second heating treatment.

2. The method according to claim 1, characterized in that The mass ratio of the 3,5-di-tert-butyl salicylaldehyde aniline to the methyl methacrylate is 1:50000 to 1:1000.

3. The method according to claim 1, characterized in that: Satisfy at least one of the following conditions: The temperature of the first heating treatment is 80°C to 95°C; The temperature of the second heating treatment is 40°C to 60°C; The temperature of the third heating treatment is 90°C to 120°C.

4. The method according to claim 1, characterized in that: The initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile and benzoyl peroxide.

5. A Schiff base / methyl methacrylate composite material, characterized in that: The invention is prepared by the method according to any one of claims 1 to 4.

6. An application of the Schiff base / methyl methacrylate composite material according to claim 5, characterized in that: It includes at least one of the fields of transparent display, battery, wearable device and three-dimensional data storage.