Preparation method and application of I-TFBPT-COF@MXene composite material
By preparing I-TFBPT-COF@MXene composite material as SPME coating, the insufficient application of MXene composite material in PAEs detection is solved, and efficient and accurate detection of multiple PAEs is achieved, which improves detection efficiency and accuracy.
Patent Information
- Application Number
- CN202310606504.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-26
AI Technical Summary
The existing PAEs detection technology has problems of low efficiency and poor accuracy, especially the application of MXene composites in sample pretreatment has not yet been fully developed, making it difficult to effectively detect PAEs in water bodies.
I-TFBPT-COF@MXene composite material was prepared by one pot method, by 1,3,5-tris(4-aminophenyl)benzene and 2,4,6-tris(4-formyl-biphenyl-4 -base)-1,3,5-triazine is mixed with MXene to form a composite material with high specific surface area and hydrophobicity, as a SPME coating for the detection of PAEs.
Simultaneous detection of up to 13 PAEs is achieved, with high sensitivity, low detection limit and good stability and repeatability, improving detection accuracy and efficiency.
Smart Images

Figure CN116550301B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new materials, and in particular to a method for preparing an I-TFBPT-COF@MXene composite material, and also to applications of the I-TFBPT-COF@MXene composite material. Background Art
[0002] Phthalates (PAEs) are commonly used in a large number of plastic consumer products, including medical devices, building materials, food packaging, and personal care products. Among them, the most common plasticizers are 2-ethylhexyl phthalate (DEHP), diethyl phthalate (DEP), dibutyl phthalate (DBP), benzyl butyl phthalate (BBP), dioctyl phthalate (DNOP), and nonyl phthalate (DNP). At present, due to the large amount of plastics produced and consumed worldwide and the lack of chemical bonds between PAEs and plastics, a large amount of PAEs are released from plastics into the environment (such as water, air, and sediments), causing environmental pollution. Studies have shown that PAEs pollution is a serious environmental problem that endangers human health. Therefore, it is necessary to provide cheap, sensitive, and accurate methods to measure PAEs in real samples, such as environmental samples, food, and organisms, which is of great significance for studying and controlling the effects of PAEs on human health.
[0003] Traditional detection and analysis techniques for PAEs mainly include liquid-liquid extraction (LLE) and solid phase extraction (SPE). In recent years, several microextraction techniques for detecting PAEs have also been developed: solid phase microextraction (SPME), dispersed liquid-liquid microextraction (DLLME) and hollow fiber liquid phase microextraction (HF-LPME). Compared with traditional methods, microextraction has many advantages: they are faster, simpler, cheaper and environmentally friendly. Among them, SPME is the most popular, which achieves the purpose of extracting and concentrating the analyte through the adsorption equilibrium between the sample matrix and the fiber coating. Therefore, the development of new fiber coating materials is a key factor affecting the extraction efficiency of SPME.
[0004] In recent years, many new adsorption materials, such as conjugated microporous polymers (CMPs), metal organic frameworks (MOFs) and covalent organic frameworks (COFs), have been developed and applied in the field of chemistry. COFs are a kind of crystalline porous functional materials with the characteristics of periodic and stable framework, unique porosity, large specific surface area, monomer diversity and easy modification at the molecular level. Due to its special structural characteristics and excellent physical and chemical properties, it is used to adsorb trace pollutants and drugs in various matrices. However, the high density of COFs leads to a large mass transfer resistance, which is not conducive to the full exposure of active sites, thereby reducing its affinity with the target substance, which limits the application of COFs to a certain extent.
[0005] MXene is a two-dimensional material obtained by exfoliation of transition metal carbides or nitrides. It has a multilayer structure, abundant recognition sites and good surface hydrophilicity. At the same time, the surface of MXene contains abundant -F, -O or -OH functional groups, which makes it show excellent performance in adsorbing dyes, nuclear radioactive ions, heavy metal ions and organic pollutants. However, MXene has a low specific surface area and few active sites, which limits its wide application as an extraction adsorbent in sample pretreatment. To this end, many researchers have synthesized MXene composites to improve the degree of surface functionalization. At present, MXene composites have been widely studied and applied in the fields of catalysis, electrochemical sensors, removal of pollutants in water environments, batteries and electrode materials. However, the surface modification and adsorption properties of MXene-based composites still need further study, and there are no reports on the detection of PAEs in water using MXene-based composites. Summary of the invention
[0006] In view of this, the present invention provides a method for preparing an I-TFBPT-COF@MXene composite material, and also provides an application of the I-TFBPT-COF@MXene composite material prepared by the present invention as an SPME coating for sensitive analysis of PAEs in complex matrices.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] The preparation method of the I-TFBPT-COF@MXene composite material of the present invention comprises: using 1,3,5-tris(4-aminophenyl)benzene (TPB) and 2,4,6-tris(4-formyl-biphenyl-4-yl)-1,3,5-triazine (TFBPT) as monomers, and preparing the monomers and MXene by a one-pot method, which specifically comprises:
[0009] Step 1, adding 1,3,5-tris(4-aminophenyl)benzene, 2,4,6-tris(4-formyl-biphenyl-4-yl)-1,3,5-triazine and MXene into a reaction vessel, then adding an organic solvent and a catalyst, degassing by freeze-pump-thaw cycle, and reacting at 120-150° C. under vacuum conditions for 2-6 days;
[0010] Step 2: After the reaction is completed, centrifuge to obtain a precipitate, wash the precipitate with the first solvent and the second solvent in turn, and dry to obtain an I-TFBPT-COF@MXene composite material.
[0011] Preferably, the amount of TPB, TFBPT and MXene in step 1 is 0.03mmol: 0.028mmol: (2mg~10mg). For the I-TFBPT-COF@MXene composite material, when the amount of TPB and TFBPT monomers remains unchanged, the amount of MXene directly affects the crystal structure, hydrophobicity and adsorption of the I-TFBPT-COF@MXene composite material. When the molar ratio of TPB to TFBPT is 0.03: 0.028, the amount of MXene is 2mg~10mg, preferably controlled at 2mg~4mg, and optimally 2mg.
[0012] In the present invention, the organic solvent in step 1 includes 1,3,5-trimethylbenzene and n-butanol; the catalyst is glacial acetic acid (preferably at a concentration of 9 M). More preferably, the organic solvent in step 1 is prepared from 1,3,5-trimethylbenzene and n-butanol in a volume ratio of 425 / 75.
[0013] In the present invention, in step 2, washing the precipitate with the first solvent and the second solvent successively specifically comprises: first performing Soxhlet extraction on the precipitate with the first solvent, and then performing Soxhlet extraction with the second solvent to remove monomers and solvents that do not participate in the reaction. The Soxhlet extraction time for each time is preferably 12 hours. The first solvent is preferably methanol, and the second solvent is preferably acetone.
[0014] The present invention also provides an application of the I-TFBPT-COF@MXene composite material. Specifically, the I-TFBPT-COF@MXene composite material is used as a solid phase microextraction coating material in the detection of PAEs. Among them, PAEs include DMP, DEP, DIBP, DBP, DEEP, DNPP, DHXP, BBP, DBEP, DCHP, DEHP, DNOP and DNP, and can achieve simultaneous detection of up to 13 PAEs.
[0015] The present invention detects PAEs based on SPME-GC-MS / MS technology, and specifically includes the following steps:
[0016] Step S1, using a direct coating method to coat the I-TFBPT-COF@MXene composite material on a solid phase microextraction probe to obtain an SPME probe coated with the I-TFBPT-COF@MXene composite material coating;
[0017] Step S2, filtering the collected sample with a filter membrane to remove insoluble particles in the sample, and then storing it in a clean brown bottle and refrigerating it at low temperature for future use;
[0018] The mixed standard mother solution of phthalates is diluted according to a concentration gradient to obtain mixed standard working solutions of different concentrations, and the solutions are refrigerated at low temperature for later use;
[0019] Insert the SPME probe prepared in step S1 into the sample or mixed standard solution, and perform solid phase microextraction by direct immersion method, wherein the extraction temperature is 20°C to 60°C; the extraction time is 10 min to 50 min, and the stirring speed during the extraction process is 100 rpm to 900 rpm;
[0020] Step S4, desorbing and quantitatively analyzing the SPME probe enriched with PAEs by GC-MS / MS.
[0021] In the present invention, in step S4, the desorption temperature of the SPME probe enriched with phthalates is 250°C to 300°C, and the desorption time is 1 to 6 minutes. More preferably, the desorption temperature is 270°C, and the desorption time is 5 minutes, so that the PAEs on the probe are completely desorbed, ensuring the reliability and accuracy of the detection results.
[0022] In the present invention, in step S4, the mass spectrometry conditions for detecting the probe enriched with PAEs by GC-MS / MS are: using MRM scanning mode, the electron impact ionization is set at 70 eV; the solvent delay time is 3 min; the transmission line temperature and the ion source temperature are 250° C. and 230° C. respectively;
[0023] The gas chromatography conditions included: helium (99.999%) as the carrier gas, a flow rate of 1.0 mL / min in splitless mode, a purge flow of 3.0 mL / min, an inlet temperature of 250°C to 300°C, and a specific heating program as follows: the initial temperature was 100°C, maintained for 1 min; first increased to 200°C at a rate of 30°C / min; then increased to 261°C at a rate of 2°C / min; finally increased to 300°C at a rate of 30°C / min and maintained for 1 min.
[0024] In the present invention, the injection port temperature of the gas chromatograph is the desorption temperature of the analyte on the SPME probe. In order to completely desorb the analyte, the injection port temperature of the gas chromatograph is controlled at 250° C. to 300° C., preferably at 270° C. In addition, the mass spectrometry and chromatographic conditions of the present invention can achieve the separation of 13 PAEs with good separation, thereby achieving the simultaneous detection of 13 PAEs, and having a wide range of applications.
[0025] The present invention adopts a one-pot method to directly mix two monomers, TPB and TFBPT, with MXene to prepare an I-TFBPT-COF@MXene composite material. A variety of functional groups are evenly distributed in the composite material, which is conducive to the formation of electron-donor-acceptor interactions, thereby accelerating the effective capture of PAEs by the I-TFBPT-COF@MXene composite material without post-modification; in addition, the I-TFBPT-COF@MXene of the present invention has a large number of benzene rings, which can form π-π interactions with the benzene rings in PAEs, further accelerating the effective capture of PAEs. Furthermore, the I-TFBPT-COF@MXene composite material of the present invention has good hydrophobicity (contact angle of 119.5°) and a large specific surface area (up to 599.85 m2 / g), further promoting the effective capture of PAEs by the I-TFBPT-COF@MXene composite material, thereby improving the accuracy of the PAEs detection results in actual samples.
[0026] Based on the prepared I-TFBPT-COF@MXene composite material, the present invention proposes a method for detecting PAEs using SPME-GC-MS / MS. This method not only has a wide linear range, but also has a low detection limit and high sensitivity, and also has good stability, repeatability and reproducibility. It can achieve simultaneous detection of up to 13 PAEs, opening up a new path for the qualitative and quantitative analysis of PAEs, and has important research significance and promotion value. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a flow chart of preparing COF using TPB and TFBPT as monomers in the present invention.
[0028] Figure 2 FT-IR graphs of I-TFBPT-COF@MXene and I-TFBPT-COF of the present invention.
[0029] Figure 3 It is the SEM image of I-TFBPT-COF@MXene and I-TFBPT-COF of the present invention.
[0030] exist Figure 3 In the figure, (a) is the SEM image of I-TFBPT-COF, (b) is the SEM image of MXene; (c) is the SEM image of I-TFBPT-COF@MXene composite material; (d) is the SEM image of I-TFBPT-COF@MXene composite material as SPME coating.
[0031] Figure 4 TEM images of I-TFBPT-COF@MXene and I-TFBPT-COF prepared by the present invention.
[0032] Figure 4 In the figure, (a) is the TEM image of COF; (b) is the high-footed annular dark field image of COF; (c) is the C element mapping image of COF; (d) is the N element mapping image of COF; (e) is the transmission electron microscope image of I-TFBPT-COF@MXene composite material; (f) is the C element mapping image of I-TFBPT-COF@MXene composite material; (g) is the N element mapping image of I-TFBPT-COF@MXene composite material; (h) is the Ti element mapping image of I-TFBPT-COF@MXene composite material.
[0033] Figure 5 It is the XRD diagram of the I-TFBPT-COF@MXene composite material and I-TFBPT-COF of the present invention.
[0034] Figure 6 The XPS graphs of the I-TFBPT-COF@MXene composite material and I-TFBPT-COF of the present invention are shown in Figure 1. (a) is the full XPS spectrum of COF and I-TFBPT-COF@MXene; (b) is the high-resolution spectrum of COF (C 1s), (c) is the high-resolution spectrum of COF (N 1s); (d) is the high-resolution spectrum of I-TFBPT-COF@MXene composite material (C 1s), (e) is the high-resolution spectrum of I-TFBPT-COF@MXene composite material (N 1s), and (f) is the high-resolution spectrum of I-TFBPT-COF@MXene composite material (Ti 2p).
[0035] Figure 7 It is a nitrogen adsorption-desorption isotherm diagram and pore size distribution diagram of the I-TFBPT-COF@MXene composite material and I-TFBPT-COF in the present invention.
[0036] Figure 8 is the contact angle of the I-TFBPT-COF@MXene composite material, I-TFBPT-COF and MXene in the present invention. Wherein, (a)-(c) correspond to I-TFBPT-COF, MXene and I-TFBPT-COF@MXene composite material, respectively.
[0037] Fig. 9 It is the TGA graph of the I-TFBPT-COF@MXene composite material and I-TFBPT-COF in the present invention.
[0038] Fig.10 It is a scatter plot of different spiked concentrations and relative standard deviations in Example 3 of the present invention.
[0039] Fig.11 This is the chromatogram of PAEs in the actual sample of Example 3.
[0040] Fig.12 This is the chromatogram of the spiked sample (spiking concentration is 200 ng / L) in Example 3.
[0041] Fig.13 This is a comparison chart of the extraction effects of the I-TFBPT-COF@MXene composite material prepared by the present invention and existing commercially available fibers on PAEs in mixed standard samples.
[0042] exist Fig.13 In the figure, the ordinate is the peak area of PAEs; the bar graphs corresponding to each PAEs correspond from left to right to I-TFBPT-COF@MXene composite coating, COF coating, commercial 100 μm PDMS fiber, commercial 65 μm PDMS / DVB fiber and commercial 50 / 30 μm DVB / CAR / PDMS fiber. DETAILED DESCRIPTION
[0043] The following is a detailed description of an embodiment of the present invention in conjunction with the accompanying drawings. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.
[0044] Example 1 Preparation and characterization of I-TFBPT-COF@MXene and COF according to the present invention
[0045] 1. Preparation of I-TFBPT-COF@MXene composites by one-pot method
[0046] The present invention uses 1,3,5-tris(4-aminophenyl)benzene and 2,4,6-tris(4-formyl-biphenyl-4-yl)-1,3,5-triazine as monomers and adopts a one-pot method to prepare an I-TFBPT-COF@MXene composite material, which specifically includes the following steps:
[0047] Step 1, add 1,3,5-tris(4-aminophenyl)benzene (10.54 mg, 0.03 mmol), 2,4,6-tris(4-formyl-biphenyl-4-yl)-1,3,5-triazine (12.4 mg, 0.028 mmol) and 2 mg MXene (the amount of MXene can also be other values within 2 mg to 10 mg) to a reaction container (preferably a Pyrex reaction tube), then add 1.0 mL of organic solvent and 0.05 mL of catalyst, degas through three freeze-pump-thaw cycles, and react at 140° C. for 4 days under vacuum conditions (in actual operation, the reaction tube can be sealed with a flame);
[0048] The organic solvent is a mixture of 1,3,5-trimethylbenzene and n-butanol in a volume ratio of 425:75; the catalyst is preferably glacial acetic acid at a concentration of 9M;
[0049] Step 2, after the reaction is completed, centrifuge to obtain a precipitate, wash the precipitate with the first solvent and the second solvent respectively (preferably the precipitate washing method is Soxhlet extraction method, preferably extraction for 12 hours); dry (preferably vacuum drying, drying at 80°C for 12 hours) to obtain a powdered I-TFBPT-COF@MXene composite material;
[0050] Among them, the first solvent is preferably methanol, and the second solvent is acetone.
[0051] 2. Preparation of I-TFBPT-COF by Solvothermal Method
[0052] In order to better verify whether the I-TFBPT-COF@MXene composite material has been successfully prepared, the present invention uses 1,3,5-tris(4-aminophenyl)benzene and 2,4,6-tris(4-formyl-biphenyl-4-yl)-1,3,5-triazine as monomers and adopts a solvothermal method to prepare I-TFBPT-COF. Figure 1 ), specifically including the following steps:
[0053] Step 1, TPB (21.08 mg, 0.06 mmol), TFBPT (24.8 mg, 0.056 mmol) were added to a Pyrex reaction tube, and then 1.0 mL of an organic solvent (mixed from 1,3,5-trimethylbenzene and n-butanol at a ratio of 425:75) and 0.05 mL of glacial acetic acid (9 M) were added, and after degassing by three freeze-pump-thaw cycles, the reaction was carried out at 140 ° C for 4 days under vacuum conditions (the reaction tube can be sealed with a flame in actual operation);
[0054] Step 2 is the same as step 2 of the preparation method of I-TFBPT-COF@MXene composite material, and finally I-TFBPT-COF is obtained, and its structural formula is as follows:
[0055]
[0056] 3. Characterization of I-TFBPT-COF and I-TFBPT-COF@MXene Composites Synthesized in the Present Invention
[0057] 1. FT-IR was used to characterize the prepared I-TFBPT-COF and I-TFBPT-COF@MXene composites. The characterization results are shown in Figure 2 . Combined Figure 2It can be seen that in the FT-IR images of I-TFBPT-COF and I-TFBPT-COF@MXene composites, the stretching vibrations of -CHO of TFBPT monomer and NH of TPB monomer disappeared, indicating that the condensation reaction between the aldehyde group of TFBPT and the amino group of TPB was successful; in addition, I-TFBPT-COF and I-TFBPT-COF@MXene composites have characteristic bands of phenyl framework at 1615 cm-1, 1589 cm-1 and 1444 cm-1, and both have -C=N stretching vibration at 1620 cm-1, indicating the successful preparation of I-TFBPT-COF and I-TFBPT-COF@MXene composites.
[0058] 2. I-TFBPT-COF, MXene and I-TFBPT-COF@MXene composites were characterized by SEM. The characterization results are shown in Figure 3 .Depend on Figure 3 (a) It can be seen that I-TFBPT-COF has a rod-like structure with a rough surface and uniformity; Figure 3 (b) It can be seen that commercial MXene is a typical single-layer structure with a smooth surface; Figure 3 (c) The rod-like structure of the I-TFBPT-COF@MXene composite material becomes short and thick, but its surface morphology is also combined with the MXene layer structure to form a multi-layer wrinkled rod-like structure, indicating the successful preparation of the I-TFBPT-COF@MXene composite material.
[0059] The I-TFBPT-COF@MXene composite material was coated on a stainless steel wire by direct coating to obtain a probe with an I-TFBPT-COF@MXene composite coating, which was characterized by SEM. Figure 3 (d) It can be seen that the surface of the I-TFBPT-COF@MXene coating prepared by the direct coating method is uniform, the diameter of the coating and the stainless steel wire is 341.5 μm, and the coating thickness is about 105 μm.
[0060] 3. TEM was used to further investigate the surface morphology of I-TFBPT-COF and I-TFBPT-COF@MXene. Figure 4 .Depend on Figure 4 (a) and (b) show that the I-TFBPT-COF synthesized in the present invention is a rod-shaped hollow structure, which is consistent with the SEM characterization results; Figure 4 (c) and (d) show that the elemental mapping of I-TFBPT-COF shows that the C and N elements are evenly distributed in the material. Figure 4(e) It can be seen that the I-TFBPT-COF@MXene composite material presents a multi-layer rod-like structure, which is consistent with the SEM characterization results; Figure 4 From (e)-(g), it can be seen intuitively that C, N and Ti elements are uniformly distributed in I-TFBPT-COF@MXene, which further illustrates the successful preparation of I-TFBPT-COF@MXene composite materials.
[0061] 4. PXRD was used to characterize I-TFBPT-COF, MXene and I-TFBPT-COF@MXene composites. The results are shown in Figure 5 .Depend on Figure 5 (a) It can be seen that I-TFBPT-COF has high crystallinity, and its main diffraction peaks are 3.2° and 5.6° respectively; Figure 5 (b) It can be seen that the main diffraction peaks of MXene are 9.2°, 21.6° and 33.7°.
[0062] Depend on Figure 5 (a) It can also be seen that in the XRD spectrum of the I-TFBPT-COF@MXene composite material, the main diffraction peaks of MXene and I-TFBPT-COF materials can be observed, indicating that the composite material has a good crystalline morphology and the crystallinity of MXene and I-TFBPT-COF materials still exists during the modification process.
[0063] XPS was used to analyze I-TFBPT-COF and I-TFBPT-COF@MXene composites. The results are shown in Figure 6 .Depend on Figure 6 (a) It can be seen that the structure of I-TFBPT-COF is mainly composed of two elements, C and N. The heterogeneous structure of I-TFBPT-COF@MXene is mainly composed of C, N and Ti. Due to the introduction of MXene, its C 1s and N 1s signals are stronger than those of pure I-TFBPT-COF. Figure 6 (b) It can be seen that the high-resolution C 1s of I-TFBPT-COF contains three components at 284.8, 285.6 and 289.7 eV, which are CC / C=C, C=N and triazinic C respectively; Figure 3 (c) It can be seen that the high-resolution N 1s of COF is divided into two peaks at 398.8 and 400.1 eV, which are attributed to C=N and triazinic N, respectively.
[0064] Depend on Figure 6 (d) It can be seen that the high-resolution C 1s of I-TFBPT-COF@MXene has a C-Ti bond at 287.3 eV; Figure 6(f) It can be seen that using three double states (Ti 2p3 / 2-Ti 2p1 / 2) fitting, it can be seen that the Ti2p3 / 2 binding energies of 458.9 eV, 458.1 eV and 463.9 eV correspond to Ti-C, Ti (II) and Ti-O bonds, respectively.
[0065] It can be seen from the above that the I-TFBPT-COF@MXene composite material of the present invention is composed of MXene and I-TFBPT-COF, and the various functional groups on the surface of MXene make the I-TFBPT-COF@MXene heterogeneous structure have good adsorption.
[0066] 5. N2 adsorption isotherms of I-TFBPT-COF and I-TFBPT-COF@MXene are shown in Figure 7 .Depend on Figure 7 It can be seen that the isothermal adsorption lines of I-TFBPT-COF and I-TFBPT-COF@MXene are typical type IV isotherms, indicating that both I-TFBPT-COF and I-TFBPT-COF@MXene composite materials are mesoporous materials. Among them, the specific surface area and pore size of I-TFBPT-COF are 470.49 m2 / g and 1.16 nm respectively; the specific surface area of I-TFBPT-COF@MXene composite material is 599.85 m2 / g, and the pore size is 1.48nm. The results show that the I-TFBPT-COF@MXene composite material prepared by the present invention has a large specific surface area, which is conducive to adsorption.
[0067] 6. The contact angle meter was used to characterize I-TFBPT-COF, MXene and I-TFBPT-COF@MXene. The results are shown in Figure 8 .Depend on Figure 8 It can be seen that the contact angles of I-TFBPT-COF and MXene are 123.2° and 84.2°, respectively, while the contact angle of the I-TFBPT-COF@MXene composite material can reach 119.5°, indicating that the I-TFBPT-COF@MXene composite material prepared by the invention has good hydrophobicity and is an ideal adsorbent for adsorbing hydrophobic analytes.
[0068] 7. Thermogravimetric analysis of I-TFBPT-COF and I-TFBPT-COF@MXene prepared by the present invention (under argon atmosphere, the temperature was increased from 30°C to 800°C at a rate of 10°C / min). Fig. 9It can be seen that before 500°C, the weight loss rate of I-TFBPT-COF and I-TFBPT-COF@MXene composites is only about 5%, which is mainly attributed to the evaporation of water and organic solvents. The results show that the I-TFBPT-COF@MXene composite material of the present invention has good thermal stability.
[0069] In summary, the present invention successfully prepared a highly hydrophobic I-TFBPT-COF@MXene composite material, which not only ensures a good crystallinity, but also has strong hydrophobicity and a large specific surface area. In addition, the I-TFBPT-COF@MXene composite material has a large number of functional groups (such as a large number of benzene rings, oxygen-containing functional groups, etc.) evenly distributed on it, which lays the foundation for the quantitative detection of PAEs and is of great significance.
[0070] Example 2 Based on the I-TFBPT-COF@MXene composite material prepared in Example 1, the present invention proposes a SPME-GC-MS / MS detection method for PAEs
[0071] It should be noted that since PAEs exist not only in plastic materials but also in solvents, chemicals, water and air, the risk of sample contamination is very high. To avoid sample contamination, the containers used in the detection method of the present invention (including volumetric flasks, pipettes, etc. used in the mixed standard preparation process and extraction containers used in extraction) are all clean glass containers or glass bottles.
[0072] In addition, it should be pointed out that the PAEs standard of the present invention is a mixed standard of DMP, DEP, DIBP, DBP, DEEP, DNPP, DHXP, BBP, DBEP, DCHP, DEHP, DNOP and DNP. The structural formula of PAEs is shown in Table 1.
[0073] Table 1 Chemical abbreviations and structural formulas of phthalates of the present invention
[0074]
[0075] The GC-MS / MS detection method of PAEs of the present invention is described in more detail below based on the I-TFBPT-COF@MXene composite material prepared in Example 1 of the present invention, including the following steps:
[0076] In the first step, the I-TFBPT-COF@MXene composite material prepared in Example 1 is coated on a stainless steel wire (with a diameter of about 127 μm) by a direct coating method to obtain an SPME probe with an I-TFBPT-COF@MXene composite material coating;
[0077] Step 2: 1000 mg / L mixed standard stock solution (commercially available) was stored at -20°C (or a lower freezing temperature to prevent the volatilization of n-hexane); the mixed standard stock solution was diluted, 10.0 mL of the diluted mixed standard working solution was added to a 20 mL glass headspace bottle, the prepared SPME probe was directly inserted into the glass bottle, and the direct immersion solid phase microextraction (DI-SPME) mode was used for extraction; the extraction time was controlled at 40 min, the extraction temperature was controlled at 30°C, and the stirring speed was controlled at 500 rpm;
[0078] In the third step, after the extraction, the SPME probe enriched with PAEs was desorbed and detected by gas chromatography-tandem mass spectrometry (GC-MS / MS, Shimadzu QP-8050 NX, Japan);
[0079] In order to maximize the peak area of each PAEs, the optimal desorption temperature of the SPME probe enriched with PAEs is controlled at 270°C; the desorption time is controlled at 3 to 7 minutes, preferably at 5 minutes.
[0080] The mass spectrometry detection conditions of GC-MS / MS included the following: MRM scanning mode was selected; electron impact ionization was set at 70 eV; solvent delay time was 3 min; transfer line temperature and ion source temperature were 250°C and 230°C, respectively;
[0081] The GC conditions included: Rtx-5MS capillary column (30 m×0.25 mm id×0.25 μm, Shimadzu, Japan); helium (99.999%) as carrier gas, flow rate of 1.0 mL / min in splitless mode, purge flow of 3.0 mL / min, injection port temperature set to 270°C (i.e., the desorption temperature of PAEs on the probe was 270°C), and the specific heating program was as follows: initial temperature was 100°C, maintained for 1 min; first increased to 200°C at a rate of 30°C / min; then increased to 261°C at a rate of 2°C / min; finally increased to 300°C at a rate of 30°C / min and maintained for 1 min.
[0082] Example 3 Reliability of the method established in Example 2 of the present invention
[0083] 1. Retention time, quantitative ions and optimal collision voltage of PAEs
[0084] The present invention determines the retention time, quantitative ion and optimal collision voltage of each PAEs based on the above detection method. Specifically, a mixed standard with a concentration of 1000 mg / L is diluted to 2 mg / L with acetone, and extraction, desorption and quantitative detection and analysis are performed in sequence according to the detection method in Example 2. The results are shown in Table 2.
[0085] Table 2 Retention time, quantitative ions and optimal collision voltage of PAEs
[0086]
[0087] Note: R is the retention time; Q1 is the quantitative ion, Q2 and Q3 are the reference ions; CE1 is the optimal collision voltage of Q1, CE2 is the optimal collision voltage of Q2, and CE3 is the optimal collision voltage of Q3.
[0088] 2. Standard curve, detection limit and quantification limit of PAEs
[0089] The present invention dilutes the mixed standard mother solution with a concentration of 1000 mg / L according to a certain concentration gradient to obtain a mixed standard solution, and the concentrations are 500 ng / L, 400 ng / L, 200 ng / L, 100 ng / L, 50 ng / L, 10 ng / L, 5ng / L and 1 ng / L. The PAEs in the mixed standard solution are quantitatively analyzed using the detection method in Example 2, and the results are shown in Table 3.
[0090] Table 3 Standard curve, detection limit and quantification limit of PAEs
[0091]
[0092] Note: EFs (i.e., enrichment factor) = the ratio of the peak area after enrichment of the target analyte to the peak area before enrichment.
[0093] As shown in Table 3, the R values of PAEs in the range of 1-500 ng / L are all greater than 0.99, indicating that the detection method of the present invention shows a good linear relationship for each PAEs; the detection limit (LODs, S / N=3) of PAEs is in the range of 0.005-11.72 ng / L, and the quantitative limit is 0.016-39.06 ng / L. The results show that the detection method established by the present invention not only shows a good linear relationship, but also has a lower detection limit and higher sensitivity, indicating that the GC-MS / MS detection method of PAEs based on the I-TFBPT-COF@MXene composite material of the present invention is suitable for the quantitative analysis of trace or ultra-trace PAEs in samples.
[0094] 3. Repeatability and reproducibility analysis
[0095] The mixed standard solution was extracted with the same SPME probe (with the same extraction conditions) and quantitatively detected using the detection method of the present invention. The extraction-desorption was repeated for multiple times. The repeatability of the SPME probe of the present invention was calculated based on the quantitative detection results of each time. The results are shown in Table 4.
[0096] Two SPME probes (each SPME probe is coated with I-TFBPT-COF@MXene composite material) were used to extract the mixed standard solution (with the same extraction conditions), and the detection method of the present invention was used for quantitative detection. The reproducibility of the SPME probe of the present invention was calculated based on the detection results. The results are shown in Table 4.
[0097] Table 4 Repeatability and reproducibility of the present invention
[0098]
[0099] It can be seen from Table 4 that the repeatability RSD of PAEs is <7.0%, and the reproducibility RSD is <8.5%. The results show that the SPME-GC-MS / MS detection method of PAEs based on I-TFBPT-COF@MXene composite material has good repeatability and reproducibility.
[0100] In summary, the SPME-GC-MS / MS detection method for PAEs established in the present invention can not only detect more types of PAEs (at least 13 types of PAEs can be detected simultaneously), but also has a wide linear range, lower detection limit and quantification limit, good stability and reproducibility, as well as high sensitivity and relatively short extraction time, which provides a new detection idea for the high-precision detection of PAEs and has a good application prospect.
[0101] Example 3 Application of the SPME probe with I-TFBPT-COF@MXene composite material coating prepared by the present invention in detecting phthalates in actual water
[0102] This example uses the SPME-GC-MS / MS method for detecting PAEs established in Example 2 to perform quantitative detection and analysis of PAEs in actual water samples, specifically including the following contents:
[0103] In the first step, the I-TFBPT-COF@MXene composite material was coated on the stainless steel wire by direct coating method to obtain an SPME probe coated with the I-TFBPT-COF@MXene composite material coating;
[0104] In the second step, the environmental surface water samples (from 18 cities in Henan Province) were filtered with a 0.22 µm filter membrane to remove insoluble particles in the water, and stored in clean brown bottles and refrigerated at 4 °C for future use;
[0105] In the third step, 10.0 mL of the sample was added to a 20 mL glass headspace bottle, and the SPME probe was directly inserted into the glass bottle. The direct immersion solid phase microextraction (DI-SPME) mode was used for extraction. The extraction time was controlled at 40 min, the extraction temperature was controlled at 30 °C, and the stirring speed was controlled at 500 rpm.
[0106] In the fourth step, after the extraction is completed, the SPME probe after extraction is inserted into the vaporization chamber of the gas chromatograph of GC-MS / MS, so that the PAEs on the SPME probe are continuously desorbed, and then the desorbed extract is quantitatively analyzed by GC-MS / MS. The results are shown in Tables 5 and 6.
[0107] Table 5
[0108]
[0109] Table 6
[0110]
[0111] In order to verify the accuracy of this embodiment, the present invention conducted a spike test on the actual samples of a river in Zhengzhou in Table 6 (i.e., a mixed standard solution with known concentrations was added to the actual sample, and the concentrations of the mixed standard solution were 10 ng / L, 50 ng / L and 200 ng / L, respectively). The spike recovery rate and RSD are shown in Table 7, and the deviation of the spike recovery rate from the relative standard is shown in Fig.10 The separation results of the actual sample and the spiked sample are shown in Fig.11 , where the GC-MS / MS chromatogram of the spiked sample with a spike concentration of 200 ng / L is shown in Fig.12 .
[0112] Table 7 Spiked recoveries of phthalates in actual samples
[0113]
[0114] As shown in Table 6, the spiked recoveries of 13 PAEs are in the range of 83.49-112.40%, and the RSDs of the spiked recoveries are in the range of 1.06-7.03%, indicating that the detection of PAEs is not affected by the complex matrix. This indicates that the detection method of the present invention has certain reliability and applicability for the enrichment and analysis of target substances in environmental systems, and can be used for the enrichment and detection of trace and ultra-trace PAEs in complex samples.
[0115] Example 4 Comparison of the I-TFBPT-COF@MXene composite material of the present invention with commercial fibers
[0116] In this example, I-TFBPT-COF@MXene composite material, I-TFBPT-COF synthesized in Example 1, commercial 100 μm PDMS fiber, commercial 65 μm PDMS / DVB fiber and commercial 50 / 30 μm DVB / CAR / PDMS fiber were used to extract PAEs in the mixed standard working solution and quantitatively detect them. The extraction, desorption and GC-MS / MS conditions were the same as those in Example 2. The specific analysis results are shown in Fig.13 .
[0117] Depend on Fig.13 It can be seen that the extraction efficiency of PAEs by the I-TFBPT-COF@MXene composite prepared by the present invention is significantly better than that of the existing commercial fibers on the market. This is because the I-TFBPT-COF@MXene composite material not only has a large comparative area, but also has a large number of benzene rings and high hydrophobic properties. The benzene rings in the material can form π-π interactions with the benzene rings in PAEs. The hydrophobic interaction and π-π interaction further promote the enrichment of the target analyte, providing a new material for the detection of PAEs, which has important promotion significance.
Claims
1. A method for preparing an I-TFBPT-COF@MXene composite material, characterized in that: The preparation method is to use 1,3,5-tris(4-aminophenyl)benzene and 2,4,6-tris(4-formyl-biphenyl-4-yl)-1,3,5-triazine as monomers, and directly mix the monomers with MXene to prepare the product, and specifically comprises the following steps: Step 1, adding 1,3,5-tris(4-aminophenyl)benzene, 2,4,6-tris(4-formyl-biphenyl-4-yl)-1,3,5-triazine and MXene into a reaction vessel, then adding an organic solvent and a catalyst, degassing by freeze-pump-thaw cycle, and reacting at 120-150° C. under vacuum conditions for 2-6 days; Among them, the amount of 1,3,5-tris(4-aminophenyl)benzene, 2,4,6-tris(4-formyl-biphenyl-4-yl)-1,3,5-triazine and MXene is 0.03mmol: 0.028mmol: (2mg~10mg); Step 2: After the reaction is completed, centrifuge to obtain a precipitate, wash the precipitate with the first solvent and the second solvent respectively, and dry to obtain an I-TFBPT-COF@MXene composite material.
2. The method for preparing the I-TFBPT-COF@MXene composite material according to claim 1, characterized in that: The organic solvent in step 1 includes 1,3,5-trimethylbenzene and n-butanol; and the catalyst is glacial acetic acid.
3. The method for preparing the I-TFBPT-COF@MXene composite material according to claim 2, characterized in that: The organic solvent in step 1 is prepared from 1,3,5-trimethylbenzene and n-butanol in a volume ratio of 425 / 75.
4. The method for preparing the I-TFBPT-COF@MXene composite material according to claim 1, characterized in that: In step 2, washing the precipitate with the first solvent and the second solvent successively specifically includes: first performing Soxhlet extraction on the precipitate with the first solvent, and then performing Soxhlet extraction on the precipitate with the second solvent; wherein the first solvent is methanol and the second solvent is acetone.
5. Use of the I-TFBPT-COF@MXene composite material prepared according to any one of claims 1 to 4 as a solid phase microextraction coating material in the extraction and detection of phthalates.
6. The use according to claim 5, characterized in that: The phthalates include DMP, DEP, DIBP, DBP, DEEP, DNPP, DHXP, BBP, DBEP, DCHP, DEHP, DNOP and DNP.
7. The use according to claim 6, characterized in that: The SPME-GC-MS / MS method is used to detect phthalates, which specifically includes the following steps: Step S1, using a direct coating method to coat the I-TFBPT-COF@MXene composite material on a stainless steel wire to obtain an SPME probe coated with the I-TFBPT-COF@MXene composite material coating; Step S2, filtering the collected sample with a filter membrane to remove insoluble particles in the sample, and then storing it in a clean brown bottle and refrigerating it at low temperature for future use; The mixed standard mother solution of phthalates is diluted according to a concentration gradient to obtain mixed standard working solutions of different concentrations, and the solutions are refrigerated at low temperature for later use; Step S3, inserting the SPME probe prepared in step S1 into the sample or mixed standard solution, and performing solid phase microextraction by direct immersion method, wherein the extraction temperature is 20° C. to 60° C.; the extraction time is 10 min to 50 min, and the stirring speed during the extraction process is 100 rpm to 900 rpm; Step S4: after the extraction is completed, the SPME probe enriched with phthalates is desorbed and quantitatively analyzed by GC-MS / MS.
8. The use according to claim 7, characterized in that: In the step S4, the desorption temperature of the SPME probe enriched with phthalates is 250° C. to 300° C., and the desorption time is 1 to 6 minutes.
9. The use according to claim 7, characterized in that: In step S4, the mass spectrometry conditions of GC-MS / MS include: using MRM scanning mode, the electron impact ionization is set at 70 eV; the solvent delay time is 3 min; the transfer line temperature and the ion source temperature are 250° C. and 230° C. respectively; The gas chromatography conditions included: helium with a purity of 99.999% as the carrier gas, a flow rate of 1.0 mL / min in the splitless mode, a purge flow of 3.0 mL / min, an inlet temperature of 250°C to 300°C, and a specific heating program as follows: the initial temperature was 100°C, maintained for 1 min; first increased to 200°C at a rate of 30°C / min; then increased to 261°C at a rate of 2°C / min; finally increased to 300°C at a rate of 30°C / min and maintained for 1 min.
Citation Information
Patent Citations
Reticular covalent organic framework material as well as preparation method and application thereof
CN111777730A
Preparation and application of MXene@COF composite membrane
CN113019137A
Preparation method of MXene-COF composite catalyst and application of MXene-COF composite catalyst in photocatalytic hydrogen production
CN115382575A
Method for simultaneously detecting phthalate acid ester compound and metabolite thereof, and application thereof
WO2021098662A1