Water-soluble heat-crosslinked multi-polymer, negative-working lithographic plate precursor and preparation method

By using water-soluble thermal crosslinked multivariate copolymer in the precursor of the negative plate, the problems of poor solvent resistance and low printing resistance are solved, and better on-machine development tolerance and UV ink printing adaptability are achieved. , improves the environmental protection and efficiency of the printing process.

CN116554392BActive Publication Date: 2024-11-26LUCKY HUAGUANG GRAPHICS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210111181.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-29
Publication Date
2024-11-26
Estimated Expiration
2042-01-29

AI Technical Summary

Technical Problem

In the machine development technology, the existing negative flat printing plate precursors have problems such as poor solvent resistance, low starting tolerance and low printing resistance under UV ink.

Method used

A water-soluble heat crosslinked multi-composite copolymer, including styrene, ethyl (meth)acrylate, copolymerization units with urethane-unsaturated double bond branching, and acrylamide copolymerization units containing sulfonic acid alkyl groups are formed. Water-soluble heat crosslinked multivariate copolymer, used to prepare negative plate precursors, improve their anti-solvent properties and on-machine development tolerance, and adapt to UV ink printing.

Benefits of technology

It has achieved the improvement of anti-solvent performance of the precursor of the negative flat printing plate, enhanced printing resistance, and supported direct-on-machine development without pre-development heating. It is suitable for UV ink printing, and improved the environmental protection and efficiency of the printing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure DEST_PATH_IMAGE001
    Figure DEST_PATH_IMAGE001
Patent Text Reader

Abstract

The present invention provides a water-soluble heat-crosslinked multi-polymer, a negative planographic plate precursor and a preparation method. The water-soluble heat-crosslinked copolymer provided in the present application is applied to a negative planographic plate precursor, has better solvent resistance, excellent printing resistance, good opening latitude, and is also suitable for UV ink printing. The negative planographic plate is a processing-free planographic plate. After being exposed by infrared laser scanning, it can be directly installed on a printing press for printing without any washing and processing steps, that is, the planographic plate is a negative on-press developing type processing-free plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative lithographic plate, and in particular to a water-soluble heat-crosslinked multi-polymer, a negative lithographic plate precursor and a preparation method. This application belongs to the green printing material of the 3.19 ecological environment material sub-direction under the 3.1 new functional material industry key direction of the 3 new material industry in the catalog of strategic emerging industries. Background Art

[0002] The present invention relates to on-press developable negative working printing plate precursors which are exposed to light radiation. In particular, the present invention relates to on-press developable printing plate precursors having a radiation-sensitive layer.

[0003] Lithographic printing plate precursors generally comprise a radiation-sensitive coating applied to a hydrophilic surface of a substrate. The radiation-sensitive coating generally comprises one or more radiation-sensitive components dispersed in an organic polymer binder. After exposing a portion of the coating to radiation (commonly referred to as exposure imaging), the exposed portion of the coating becomes easier or more difficult to develop in a particular liquid (developer) than the unexposed portion. When the exposed portion or area becomes difficult to develop in the developer, and the unexposed portion is removed during the development process, the plate precursor is generally considered to be a negative precursor (or negative printing plate, negative printing plate). After development in a suitable liquid, the imaged area (image portion) accepts ink when printed, while the exposed surface of the hydrophilic surface of the substrate repels ink.

[0004] Radiation-sensitive photopolymerizable compositions used in negative-working offset printing plate precursors generally comprise a polymerizable component, a radiation absorber, an initiator composition and optionally one or more polymeric binders.

[0005] In recent years, from the perspectives of global environmental protection and adaptation to digitalization, the industry has emphasized simplifying the lithographic plate manufacturing process, including omitting the pre-development heating step (preheating) and using lithographic ink, fountain solution or both for on-press development (develop on press, abbreviated as DOP) to remove unnecessary coating materials on the lithographic plate precursor. It is a method of using an image recording layer that can remove the non-image part of the lithographic printing plate precursor during ordinary printing, and removing the non-image part after exposure on the printing press to obtain a lithographic printing plate. As specific examples of on-press development, for example, a method of removing a soluble image recording layer of a lithographic printing plate precursor using a dampening solution, ink, or a dampening solution and ink; a method of mechanically removing an image recording layer by contacting with a roller and a rubber blanket of a printing press; and a method of mechanically removing an image recording layer by contacting with a roller and a rubber blanket after reducing the cohesive strength of the image recording layer or the adhesion strength of the image recording layer to the carrier by penetration of the dampening solution and ink.

[0006] Because this on-press developed lithographic plate technology is that the pre-coated lithographic plate material is scanned and plated by the CTP plate-making machine, and the coating of the non-image area is removed on the printing press by the action of dampening water and ink. Most of the peeled coating is taken away by the plate paper, and a small part may be dissolved in the dampening water, exposing the hydrophilic aluminum base. This method achieves the environmental protection goal of no pollution discharge in the pre-press process, but there is a potential risk of printing press pollution. The lithographic printing plate precursor designed for DOP applications usually does not have an oxygen barrier (protective) layer (which is common in other precursors) or if such an oxygen barrier layer exists, the layer is at a low coverage rate.

[0007] One of the key technologies for developing on-press development-free plates is the development of plate precursors, i.e., functional organic compounds. EP0980754 introduces the technology of carboxyl decarboxylation to achieve hydrophilic-hydrophobic transition, but the molecular weight of the phase transition compound is too large, the energy threshold becomes large, and decarboxylation is difficult, so the plate with this technology has poor printing resistance. W094 / 23954 introduces a microcapsule hot-melt technology. Laser hot-melt destroys the microcapsules, and the hydrophilic material is destroyed and converted to hydrophobic. However, the damaged material easily causes pollution to the blank space of the printing. US4004924 introduces a mixture of thermoplastic hydrophobic particles and hydrophilic binder, but it is not print-resistant. Agfa EP 2006-5-2406114475.4 and CN200780018820 introduce a semi-continuous emulsion method for manufacturing styrene and acrylonitrile emulsion thermoplastic particles, which can achieve hot melting, but do not contain self-emulsifying hydrophilic groups, require high particle control technology, and have poor emulsion stability, requiring the addition of antimicrobial agents. Kodak US 2006-7-27 11 / 494,235, CN200780028508 introduce a solvent-resistant polymer containing a hydrophilic group and a cyano side group, containing an allyl ester side chain, which is formed by a condensation reaction of a carboxyl side group and an allyl halide under the action of an alkali, but the side reaction byproducts are relatively large, the post-processing is troublesome, and the ester group is still not print-resistant; Fujifilm JP 2000-7-132000-213142, CN01120259 introduce a lithographic printing plate precursor, containing a polymer with a three-dimensional polyisocyanate pre-crosslinked structure and a hydrophilic grafted chain, and the three-dimensional pre-crosslinked structure improves the plate's printability, but reduces the plate's on-press developability. In recent years, the technology of processing-free plates that can be developed on the press has made great progress and has been commercialized, but there are still problems such as low plate opening tolerance, poor solvent resistance, and low printability under UV ink. Summary of the invention

[0008] In order to solve the above problems, the present invention provides a water-soluble thermally cross-linked multipolymer, a negative-working lithographic plate precursor and a preparation method. The water-soluble thermally cross-linked multipolymer provided in the present application is applied to the negative-working lithographic plate precursor, which improves the solvent resistance of the plate, has good on-machine development tolerance, and is suitable for UV ink printing.

[0009] The object of the present invention is achieved in the following manner: a water-soluble heat-crosslinked multi-polymer, the copolymer containing the following structure:

[0010] -ABCD-

[0011] A represents a styrene copolymer unit;

[0012] B represents ethyl (meth)acrylate copolymer units;

[0013] C represents a copolymer unit having an urethanized unsaturated double bond branch:

[0014]

[0015] R1 is a H atom or a methyl group, and R2 is a CH2=C(CH3)COOCH2CH2NCO- group;

[0016] D represents an acrylamide copolymer unit containing a sulfonic acid alkyl group:

[0017]

[0018] Wherein, n is an integer of 0-8, R is an alkyl or aryl group having 3-18 carbon atoms, and M is an alkali metal element.

[0019] For the acrylamide copolymer unit D containing sulfonic acid alkyl, wherein n is an integer of 1-4, R is any one selected from n-hexyl, n-octyl, n-nonyl, n-decyl, n-dodecyl, n-tetradecyl, p-octylphenyl and p-dodecylphenyl, and M is sodium or potassium.

[0020] For the acrylamide copolymer unit D containing a sulfonic acid alkyl group, n is 1 or 2, R is any one selected from n-octyl, n-dodecyl, n-tetradecyl, p-dodecylphenyl and n-hexadecyl, and M is sodium.

[0021] The water-soluble heat-crosslinked multipolymer of the present invention has a weight average molecular weight of 2000-300000; a glass transition temperature of 30-400°C; a weight percentage content of styrene copolymer units A in the water-soluble heat-crosslinked multipolymer of 20%-70%; a weight percentage content of ethyl (meth)acrylate copolymer units B in the water-soluble heat-crosslinked multipolymer of 1%-40%; a weight percentage content of copolymer units C having amined unsaturated double bond branches in the water-soluble heat-crosslinked multipolymer of 1%-40%; a weight percentage content of acrylamide copolymer units D containing sulfonic acid alkyl groups in the water-soluble heat-crosslinked multipolymer of 1%-40%.

[0022] The water-soluble heat-crosslinked multipolymer of the present invention has a weight average molecular weight of 10,000-200,000; a glass transition temperature of 40-300° C.; a weight percentage content of styrene copolymer units A in the water-soluble heat-crosslinked multipolymer of 30%-60%; a weight percentage content of ethyl (meth)acrylate copolymer units B in the water-soluble heat-crosslinked multipolymer of 1%-30%; a weight percentage content of copolymer units C having amined unsaturated double bond branches in the water-soluble heat-crosslinked multipolymer of 1%-30%; and a weight percentage content of acrylamide copolymer units D containing sulfonic acid alkyl groups in the water-soluble heat-crosslinked multipolymer of 1%-30%.

[0023] The water-soluble heat-crosslinked multipolymer of the present invention has a weight average molecular weight of 30,000-150,000; a glass transition temperature of 60-150° C.; a weight percentage content of styrene copolymer units A in the water-soluble heat-crosslinked multipolymer of 40%-60%; a weight percentage content of ethyl (meth)acrylate copolymer units B in the water-soluble heat-crosslinked multipolymer of 1%-25%; a weight percentage content of copolymer units C having amined unsaturated double bond side chains in the water-soluble heat-crosslinked multipolymer of 5%-20%; and a weight percentage content of acrylamide copolymer units D containing sulfonic acid alkyl groups in the water-soluble heat-crosslinked multipolymer of 5%-25%.

[0024] A negative planographic plate precursor of the present invention comprises an imageable layer, which comprises a water-soluble heat-crosslinked copolymer, a polymerizable / crosslinked component, an infrared radiation absorber and an initiator. The water-soluble heat-crosslinked copolymer comprises the water-soluble heat-crosslinked multipolymer described above.

[0025] The water-soluble thermally cross-linked copolymer accounts for 10%-60% of the weight of the imageable layer (the weight of the imageable layer refers to the dry weight of the imageable layer), the polymerizable / cross-linked component accounts for 10%-70% of the weight of the imageable layer, the infrared radiation absorber accounts for 1%-30% of the weight of the imageable layer, and the initiator accounts for 1%-30% of the weight of the imageable layer.

[0026] The water-soluble heat-crosslinked copolymer accounts for 20%-40% by weight of the imageable layer, the polymerizable / crosslinked component accounts for 20%-50% by weight of the imageable layer, the infrared radiation absorber accounts for 1%-15% by weight of the imageable layer, and the initiator accounts for 3%-20% by weight of the imageable layer.

[0027] The polymerizable / cross-linkable component is composed of at least one of an ethylenically unsaturated free radical polymerizable monomer or oligomer or a free radical cross-linkable polymer.

[0028] The infrared radiation absorbing dye is a cyanine dye that absorbs at 750~850nm.

[0029] The initiator is selected from one or more of iodonium salts, sulfonium salts, phosphonium salts and selenium salts.

[0030] The imageable layer further comprises at least one of a pigment, an organic or inorganic particle, a sensitized dye, a wetting agent, a plasticizer, a binder, a surfactant, an antioxidant, a coating aid, an anti-stabilizer and a brightener.

[0031] The method for preparing the negative lithographic plate precursor comprises mixing the raw materials of the imageable layer to obtain a photosensitive liquid preparation, then coating the photosensitive liquid preparation on a hydrophilic treated plate substrate using a rod coater or other equipment or method, and then drying in a suitable manner to obtain a negative lithographic plate precursor.

[0032] Compared with the prior art, the present invention provides a water-soluble heat-crosslinked copolymer, a negative lithographic plate precursor and a method for preparing a negative lithographic plate. The water-soluble heat-crosslinked copolymer provided in the present application is applied to the negative lithographic plate precursor, has better solvent resistance, excellent printing resistance, and good opening tolerance, and is also suitable for UV ink printing. The negative lithographic plate is a processing-free lithographic plate. After being exposed by infrared laser scanning, it can be directly installed on a printing press for printing without any washing and processing steps, that is, the lithographic plate is a negative on-press developing type processing-free plate. DETAILED DESCRIPTION

[0033] A water-soluble heat-crosslinked multi-polymer, the copolymer having the following structure:

[0034] -ABCD-

[0035] A represents a styrene copolymer unit;

[0036] B represents ethyl (meth)acrylate copolymer units;

[0037] C represents a copolymer unit having an urethanized unsaturated double bond branch:

[0038]

[0039] R1 is a H atom or a methyl group, and R2 is a CH2=C(CH3)COOCH2CH2NCO- group;

[0040] D represents an acrylamide copolymer unit containing a sulfonic acid alkyl group:

[0041]

[0042] Wherein, n is an integer of 0-8, R is an alkyl or aryl group having 3-18 carbon atoms, and M is an alkali metal element.

[0043] In the water-soluble heat-crosslinked multipolymer, the styrene structural unit A has good thermoplasticity and a moderate glass transition temperature. As an adhesive, it has the property of melting when heated, and can firmly combine the image and text of the hot part with the base, thereby enhancing the ink-receptive performance of the image and text part. The content of styrene in the water-soluble heat-crosslinked multipolymer directly affects the glass transition temperature and thermoplasticity of the polymer. In the present invention, the weight percentage content of the styrene copolymer unit A in the water-soluble heat-crosslinked multipolymer is 20-70%, and is further preferably 30%-70%, 30%-60%, 40%-60%, and 50%-60%.

[0044] In the water-soluble heat-crosslinked multi-polymer of the present invention, the (meth) acrylate copolymer unit B is a commonly used polymerization and copolymerization monomer, which can be used to manufacture polymers and copolymers, synthetic resins, adhesives, coatings, fiber treatment agents, and intermediates of molding materials, and can effectively enhance and improve the flexibility and toughness of the copolymer. The weight percentage content of the (meth) acrylate copolymer unit B in the water-soluble heat-crosslinked multi-polymer is 1%-40%, preferably 1%-30%, and more preferably 1-25%.

[0045] In the water-soluble heat-crosslinked multi-polymer of the present invention, the copolymerization unit C having a side chain of amined unsaturated double bonds, the unsaturated group ester of which crosslinks with the multifunctional prepolymer under the action of light or heat to form a three-dimensional crosslinked structure, can realize the coating from hydrophilic to hydrophobic, and realize the printing of plate imaging. In addition, polyurethane elastomer has high wear resistance due to the strong polar amine ester bond, and is called the "wear-resistant king" resin, so we introduce the strong polar amine ester bond into the water-soluble heat-crosslinked multi-polymer. After the introduction of the strong polar amine ester bond, the emulsion particles have better elasticity and wear resistance. At the same time, the adhesive containing the strong polar amine ester bond has a strong adsorption effect on the aluminum plate base, which can improve the printing resistance of the plate. In addition, the adhesive containing the polyurethane structure has better compatibility with the polyurethane prepolymer, and the plate is not prone to the appearance of pepper spots caused by the difference in solubility of the film-forming components.

[0046] The water-soluble heat-crosslinked multi-polymer of the present invention is designed with an amined unsaturated double-bond branched copolymer unit C, and its structure is as follows:

[0047]

[0048] R1 is a H atom or a methyl group, and R2 is a CH2=C(CH3)COOCH2CH2NHCO- group. The monomer used to copolymerize to form the copolymer unit C can be seen in the following structural formula:

[0049] Cl:

[0050]

[0051] C2:

[0052]

[0053] In the water-soluble heat-crosslinked multipolymer of the present invention, the weight percentage content of the copolymer unit C having a side chain of amined unsaturated double bonds is 1%-40%, preferably 1%-30%, more preferably 5%-25%, and even more preferably 5%-20%.

[0054] The copolymer units C1 and C2 of the urethanized unsaturated double-bond branches in the water-soluble heat-crosslinked multi-polymer of the present invention are already available as industrial products for sale and can be purchased conveniently or synthesized in batches in a laboratory.

[0055] The acrylamide copolymerization unit D containing sulfonic acid alkyl in the water-soluble heat-crosslinked multi-polymer of the present invention is generated in the water-soluble heat-crosslinked multi-polymer by using an amphiphilic polymerizable monomer when preparing the water-soluble heat-crosslinked multi-polymer. Wherein, n is an integer of 0-8, R is an alkyl or aryl group having 3-18 carbon atoms, and M is an alkali metal element.

[0056] The amphiphilic polymerizable monomer has both a hydrophilic group and a hydrophobic group in its molecular structure, and thus has good amphiphilicity. The amphiphilic polymerizable monomer has a self-solubilizing effect when used to prepare a polymer, and a copolymer having an amphiphilic microblock structure and good solubility can be obtained. The amphiphilic polymerizable monomer is a derivative of acrylamide, and is easily copolymerized with acrylamide monomers. The two hydrogen atoms on the amide N are replaced, thereby enhancing the stability of the amphiphilic monomer and the copolymer, and improving the solvent resistance of the copolymer.

[0057] Preferably, n is an integer of 1-4, R is any one selected from n-hexyl, n-octyl, n-nonyl, n-decyl, n-dodecyl, n-tetradecyl, p-octylphenyl and p-dodecylphenyl, and M is sodium or potassium.

[0058] More preferably, n is 1 or 2, R is any one selected from n-octyl, n-dodecyl, n-tetradecyl, p-dodecylphenyl and n-hexadecyl, and M is sodium. In this case, the obtained monomer has better solubility and higher surface activity.

[0059] The acrylamide copolymer unit D containing sulfonic acid alkyl in the water-soluble heat-crosslinked multipolymer of the present invention includes the following structure but is not limited thereto: 2-octyl acrylamide ethanesulfonate sodium D1, 2-dodecyl acrylamide ethanesulfonate sodium D2, 2-tetradecyl acrylamide ethanesulfonate sodium D3, 2-tetradecyl acrylamide propanesulfonate potassium D4, and 2-hexadecyl acrylamide ethanesulfonate sodium D5.

[0060] In the water-soluble heat-crosslinked multipolymer of the present invention, the weight percentage content of the acrylamide copolymer unit D containing sulfonic acid alkyl is 1%-40%, preferably 1%-30%, more preferably 5%-25%, and further preferably 10-25%.

[0061] The method for preparing the amphiphilic polymerizable monomer comprises contacting an aliphatic amine having 3 to 18 carbon atoms or an aromatic amine having 3 to 18 carbon atoms with an alkali metal salt of a halogenated alkylsulfonic acid represented by the following formula (1) in a mixture of an organic solvent and water under alkylation conditions to obtain an intermediate represented by the following formula (2); contacting the intermediate with acryloyl chloride in an alkaline solution;

[0062] X-CH2- (CH2) n- SO3M Formula (1)

[0063] R-NH- (CH2)n+1-SO3M Formula (2)

[0064] In formula (1) and formula (2): X represents a halogen, n is an integer of 0-8, M is an alkali metal element, and R is an alkyl group having 3-18 carbon atoms or an aryl group having 3-18 carbon atoms.

[0065] In a preferred case, the molar ratio of the aliphatic amine or aromatic amine to the alkali metal salt of halogenated alkyl sulfonate is generally 0.8-3:1, preferably 0.8-1.5:1; the molar ratio of the intermediate to acrylphthalein chloride is generally 0.3-1.2:1, preferably 0.5-1.2:1. When the amount of the aliphatic amine or aromatic amine to the alkali metal salt of halogenated alkyl sulfonate is within the above range, the obtained amphiphilic polymerizable monomer has better solubility and higher surface activity.

[0066] In the method for preparing the amphiphilic polymerizable monomer, the types of the aliphatic amine and aromatic amine having 3 to 18 carbon atoms and the alkali metal salt of the halogenated alkyl sulfonic acid have been described in detail above and will not be repeated here.

[0067] The amphiphilic polymerizable monomer is available in industrialized form for sale and can also be synthesized in batches in the laboratory.

[0068] According to the preparation method of the amphiphilic polymerizable monomer of the present invention, in a preferred case, in the mixture of the organic solvent and water, the volume ratio of the organic solvent to water can be 2-10:1, preferably 4-6:1, the pH value under the alkaline condition can be 8-12, preferably 9-11, and the alkaline condition can be achieved by adding an alkaline compound (such as NaOH, KOH, etc.) to the mixture, as long as the required pH value range can be reached; the molar ratio of the organic solvent to the total amount of the aliphatic amine or aromatic amine and the alkali metal salt of the halogenated alkyl sulfonic acid can be 20-50:1, preferably 30-40:1.

[0069] The organic solvent may be at least one selected from ethanol, isopropanol, tetrahydrofuran, ether, chloroform, ethyl acetate, dimethylformamide, benzene and toluene, preferably one or more of ethanol, isopropanol and tetrahydrofuran.

[0070] According to the present invention, the intermediate can be obtained by cooling at room temperature and then filtering.

[0071] Since the intermediate in the present invention is prepared by the dehydrohalogenation reaction between a halogenated hydrocarbon and an organic amine, and this reaction is a very conventional and well-studied reaction in the field of organic chemistry, the solid product after the aliphatic amine having 3 to 18 carbon atoms or the aromatic amine having 3 to 18 carbon atoms is contacted with the alkali metal salt of the halogenated alkylsulfonic acid represented by the general formula (1) does not need any special structural characterization to prove that it has the structure represented by formula (2), but it can also be characterized, such as by nuclear magnetic resonance and infrared spectrum.

[0072] The conditions for contacting the aliphatic amine with 3-18 carbon atoms or the aromatic amine with 3-18 carbon atoms with the alkali metal salt of halogenated alkyl sulfonate and the intermediate with acryloyl chloride include the contact temperature and contact time. The contact temperature can be selected in a wide temperature range, for example, the temperature for contacting the aliphatic amine with 3-18 carbon atoms or the aromatic amine with 3-18 carbon atoms with the alkali metal salt of halogenated alkyl sulfonate can be 40-90°C, preferably 60-85°C. The extension of the contact time is conducive to the improvement of the reaction yield, but the yield improvement is not obvious when the contact time is too long. Therefore, under generally preferred conditions, the contact time can be 10-20 hours, preferably 10-14 hours; the temperature for contacting the intermediate with acryloyl chloride can be 1-10°C, preferably 2-5°C.

[0073] The preparation method of the amphiphilic polymerizable monomer also includes filtering and vacuum drying after the contacting is completed to obtain the amphiphilic polymerizable monomer of the present invention. The filtering, vacuum drying, and recrystallization methods or methods can all adopt methods or methods commonly used in the art, and the present invention has no special requirements. For example, the solvent for the recrystallization can be one or more of ethanol, acetone, isopropanol, and ethyl acetate.

[0074] Preparation method of water-soluble thermally cross-linked multipolymer:

[0075] The water-soluble heat-crosslinked multi-polymer of the present invention is synthesized by copolymerization, and the copolymerization reaction can be random copolymerization or block copolymerization, preferably random copolymerization. The initiator of the polymerization includes peroxides such as di-tert-butyl peroxide, phthalide peroxide, persulfate such as potassium persulfate, ammonium persulfate, azo compounds such as azobisisobutyronitrile, etc. The copolymerization method adopts emulsion polymerization.

[0076] The reaction solvents that can be used include water, methanol, ethanol, n-propanol, isopropanol, butanol, acetone, methyl ethyl ketone, cyclohexanone,

[0077] Ethyl acetate, butyl acetate, tetrahydrofuran, 1, 4-dioxane, N, N-dimethylformamide, dimethylacetamideacetone, methyl ethyl ketone, cyclohexane, ethylene dichloride, toluene, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol dimethyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, acetylacetone, diacetone alcohol, ethylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, ethylene glycol isopropyl ether, ethylene glycol butyl ether acetate, 3-methoxypropanol, methoxymethoxyethanol, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, dimethyl sulfoxide, methyl lactate and ethyl lactate, or a mixture thereof. Preferably, a mixture of alcohol and water is used, preferably a mixture of n-propanol monowater or isopropanol monowater. The emulsion copolymerization temperature is preferably 40-100°C, and most preferably 60-90°C.

[0078] The water-soluble heat-crosslinked multipolymer described in the present invention is synthesized by adding part of the raw materials in a dripping manner. The particle size of the multipolymer particles can be controlled by changing the concentration of the reaction system and the dripping time. The diameter of the multipolymer particles decreases with the decrease of the concentration of the reaction system and the increase of the dripping time. The particle size of the multipolymer particles can be controlled at the nanometer level by adjusting the concentration of the reaction system and the dripping time.

[0079] The water-soluble heat-crosslinked multipolymer of the present invention has a weight average molecular weight of 2000-300000, preferably 10000-200000, more preferably 20000-180000, further preferably 30000-150000, and further preferably 40000-100000. The glass transition temperature is 30-400°C, preferably 30-300°C, more preferably 40-220°C, and further preferably 60-150°C.

[0080] Some useful water-soluble thermally crosslinked copolymers are present in particulate form. Such discrete particles may have an average particle size of at least 10 nm and up to and including 1500 nm, or typically at least 80 nm and up to and including 600 nm, and are generally uniformly distributed within the imageable layer sensitive to infrared radiation.

[0081] The lithographic printing plate precursor of the present invention is prepared having the structure and components as described below.

[0082] Imageable layer

[0083] The imageable layer includes one or more water-soluble heat-crosslinked copolymers, which can be selected from many materials known in the art, and can be composed of vinyl copolymer units containing branched hydrophilic groups, (meth) acrylonitrile copolymer units, amphiphilic polymerizable monomer copolymer units, (meth) acrylate copolymer units, or (meth) acrylate copolymer units with branched unsaturated double bonds amined, etc. Some useful multi-polymers contain repeating units with side chains containing sulfonic acid alkyl segments, etc. Other useful multi-polymers contain two or more types of repeating units, the repeating units having different side chains of amine segments containing unsaturated double bonds.

[0084] The water-soluble thermally cross-linked copolymer must include the water-soluble thermally cross-linked multipolymer described in the present application.

[0085] Some water-soluble thermally crosslinked copolymers are present in particulate form. Such discrete particles may have an average particle size of at least 10 nm and up to and including 1500 nm, or typically at least 80 nm and up to and including 600 nm, and are generally uniformly distributed in the imageable layer sensitive to infrared radiation.

[0086] The solid content of the water-soluble heat-crosslinked copolymer in the imaging layer of the planographic printing plate of the present invention is 10-60%, preferably 20-40%.

[0087] The imageable layer includes a polymerizable / crosslinkable component, which includes one or more free radical polymerizable / crosslinkable compounds, each of which contains one or more free radical polymerizable groups that can be polymerized using free radicals. In some embodiments, the imageable layer sensitive to infrared radiation includes two or more free radical polymerizable components, the components having different numbers of free radical polymerizable groups in each molecule.

[0088] Useful free radical polymerizable components may contain one or more free radical polymerizable monomers or oligomers having one or more ethylenically unsaturated polymerizable or crosslinkable groups which can be polymerized or crosslinked by free radical initiation. Thus, suitable polymerizable or crosslinkable ethylenically unsaturated compounds include ethylenically unsaturated polymerizable monomers having one or more polymerizable groups, including unsaturated esters of alcohols, such as (meth) acrylic esters of polyols. Oligomers and / or prepolymers may also be used, for example, urethane (meth) acrylates.

[0089] Similarly, crosslinkable polymers having such radically polymerizable groups may also be used. Oligomers or prepolymers such as urethane acrylates and methacrylates, epoxide acrylates and methacrylates, polyester acrylates and methacrylates, polyether acrylates and methacrylates, and unsaturated polyester resins may be used. In some embodiments, the radically polymerizable component comprises a carboxyl group.

[0090] Particularly useful free radical polymerizable components include free radical polymerizable monomers or oligomers containing addition polymerizable ethylenically unsaturated groups, including multiple acrylate and methacrylate groups and combinations thereof, or free radical crosslinkable polymers. More particularly useful free radical polymerizable compounds include urea urethane (meth) acrylates or urethane (meth) acrylates derived from having multiple polymerizable groups.

[0091] The polymerizable / crosslinkable component is present in the imaging layer of the lithographic printing plate of the present invention at a solids content of 10-70%, preferably 20-50%.

[0092] The imageable layer includes one or more infrared radiation absorbers, which can be cyanine dyes sensitive to near-infrared radiation or infrared radiation with a wavelength of 750 to 1200 nm, and the cyanine dyes contain a color-changing group and polymerizable / cross-linkable unsaturated double bonds. Due to the special structure of the cyanine dye, it has a good imaging contrast, and because the molecule contains polymerizable / cross-linkable double bonds, the dye residue can participate in the photopolymerization reaction during imaging, thereby improving the printing plate's printing durability.

[0093] The infrared radiation absorber may be a cyanine dye absorbing at 750-850 nm.

[0094] In addition to the infrared photothermal conversion material containing cyanine dyes, the initiation system capable of initiating polymerization / crosslinking of the present invention may also contain other suitable photothermal conversion dyes, such as methine, polymethine, arylmethine, cyanine, hemicyanine, chain cyanine, squarylium, pyranium, oxonium alcohol, naphthoquinone, anthraquinone, porphyrin, azo, croconium, triarylamine, thiazolium, indolium, oxonium, indigo, indigotricarbocyanine, oxatricarbocyanine, phthalocyanine, thiocyanine, thiotricarbocyanine, merocyanine, cryptocyanine, naphthalocyanine, polyaniline, polypyrrole, polythiophene, thiopyranoarylidene and bis(thiopyrrolo)polymethine, oxyindoxazine, pyrazoline azo, etc.

[0095] Preferably, at least one infrared radiation absorber in the imageable layer of the lithographic printing plate of the present invention is a cyanine dye comprising a tetraarylborate anion.

[0096] The structures of the cyanine dyes used in the present invention are exemplified below, but are not limited to these structures.

[0097]

[0098]

[0099] The total amount of infrared radiation absorbers in the imaging layer of the lithographic printing plate of the present invention is 1-30% solid content, preferably 1-15%.

[0100] The imageable layer also includes an initiator that provides free radicals to initiate polymerization of one or more free radical polymerizable components when the radiation-sensitive imageable layer is exposed to infrared radiation, selected from onium salts such as sulfonium salts, iodonium salts, etc. Suitable onium salts include sulfonium salts, oxysulfonium salts, oxosulfonium salts, sulfoxide onium salts, diazonium salts and halogen onium salts such as iodonium salts, etc. Specific examples of suitable onium salts include diphenyliodonium chloride, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, [4-[(2-hydroxytetradecyl-oxy]-phenyl]phenyliodonium hexafluoroantimonate, triphenylsulfonium iodonium tetrafluoroborate, triphenylsulfonium iodonium octylsulfate, 2-methoxy-4-aminophenyldiazonium hexafluorophosphate, phenoxyphenyldiazonium hexafluoroantimonate, and the like. The initiator is preferably an iodonium borate initiator compound.

[0101] The solid content of the initiator in the imaging layer of the lithographic printing plate of the present invention is 1-30%, preferably 3-20%.

[0102] In some embodiments, the secondary multipolymer is more hydrophilic than the primary multipolymer.Examples of such hydrophilic secondary multipolymers include, but are not limited to, cellulose derivatives, such as hydroxypropyl cellulose, carboxymethyl cellulose; and polyvinyl alcohols with various degrees of saponification.

[0103] Additionally, the imageable layer may include pigments / dyes and developers as known in the art. Useful pigments / dyes include, but are not limited to, phthalide and fluorane leuco dyes containing a lactone skeleton having acid dissociation properties.

[0104] The imageable layer of the lithographic printing plate of the present invention may also contain various materials in combination with the essential components of the present invention. For example, pigments, organic or inorganic particles, sensitized dyes, wetting agents, plasticizers, binders, surfactants, antioxidants, coating aids, stabilizers and brighteners, etc., may be used in the present invention without affecting its performance, or any other additives commonly used in the lithographic printing field, and the amount thereof is a conventional amount.

[0105] Protective layer

[0106] In some embodiments, the negative-working lithographic plate precursor does not have an outermost layer disposed on the imageable layer, but it is possible that the precursor can be designed with a hydrophilic protective layer (or oxygen barrier layer or topcoat) disposed directly on the imageable layer (with no intervening layers between the two layers). Such precursors can be developed on-press, as well as off-press using any suitable developer as described below.

[0107] The protective layer can prevent and hinder low molecular compounds such as oxygen and alkaline substances in the atmosphere from mixing into the photosensitive layer, affecting the image formation reaction caused by exposure in the photosensitive layer. Therefore, the characteristics required for this protective layer are low permeability of low molecular compounds such as oxygen, and it is required not to substantially hinder the transmission of light used in exposure and to have good adhesion to the photosensitive layer, and it can be easily removed during the on-machine development of the plate. In addition, other properties can also be given to the protective layer. For example, by adding a colorant (water-soluble dye, etc.) that has good light permeability of 780-850nm used in exposure and can effectively absorb light outside the range of 780-850nm, the platemaking safety of the lithographic plate under white light can be improved without causing a decrease in sensitivity.

[0108] For the materials that can be used for the protective layer, for example, it is preferred to use a water-soluble polymer compound with good crystallinity. Specifically, water-soluble polymers such as polyvinyl alcohol, polyvinyl pyrrolidone, acidic cellulose, gelatin, gum arabic, and polyacrylic acid are known. Among these substances, when polyvinyl alcohol is used as the main component, it can bring the best results for basic properties such as oxygen barrier properties and development removal properties. The polyvinyl alcohol used in the protective layer can contain unsubstituted vinyl alcohol units in an amount that can have the required oxygen barrier properties and water solubility, and part of them can be substituted by esters, ethers, and acetals. In addition, part of them can also have other copolymer components. For specific examples of polyvinyl alcohol, compounds with 71-100% hydrolysis and a molecular weight of 300-2400 can be cited. Specific examples include: PVA-105, PVA-110, PVA-117, PVA-117H. PVA-120, PVA-124. PVA-124H. PVA-CS. PVA-CST, PVA-HC. PVA-203, PVA-204, PVA-205, PVA-210, etc.

[0109] The composition of the protective layer (selection of PVA, use of additives), coating amount, etc., are selected in consideration of not only oxygen barrier properties and developer removability, but also fogging, adhesion, and scratch resistance. Generally, the higher the hydrolysis rate of the PVA used (the higher the content of unsubstituted vinyl alcohol units in the protective layer) and the thicker the film thickness, the higher the oxygen barrier properties become, which is beneficial to the sensitivity. In addition, the adhesion and scratch resistance to the image part are very important in the operation of the printing plate. That is, if a hydrophilic layer composed of a water-soluble polymer is laminated on a lipophilic polymer layer, film peeling caused by insufficient adhesion is likely to occur, and defects such as poor film curing will occur in the peeled portion due to the inhibition of oxygen.

[0110] When a protective layer is present, the dry coating weight of the protective layer is usually 0.1 -4g / m 2 , preferably 0.2-2.0g / m 2 In some embodiments, the dry coating weight is 0.1-0.9 g / m 2 , so that the hydrophilic protective layer is relatively thin for being easily removed during off-press development or on-press development.

[0111] Base

[0112] The substrate present in the precursor generally has a hydrophilic surface, or at least has a more hydrophilic surface than the imageable layer sensitive to infrared radiation applied on the imaging side of the substrate. The substrate comprises a support which can be composed of any material conventionally used for preparing lithographic printing plate precursors.

[0113] A useful plate base is composed of an aluminum support, which is a high-purity aluminum plate, and its aluminum content is preferably above 99%. The aluminum support can be treated using techniques known in the art, including roughening a certain type by physical (mechanical) grinding, electrochemical grinding or chemical grinding, and usually then anodizing. The electrolyte used for electrolytic roughening can be an aqueous solution of an acid, alkali or salt or an aqueous solution containing an organic solvent. Among them, an aqueous solution of hydrochloric acid, nitric acid or their salts is preferably used as the electrolyte. Typically, phosphoric acid or sulfuric acid is used and anodizing is performed using conventional procedures.

[0114] First, place the aluminum plate in a 1% to 30% aqueous solution of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, etc., and chemically etch it at a temperature of 20 to 80°C for 5 to 250 seconds. Then neutralize it in 10 to 30% nitric acid or sulfuric acid at a temperature of 20 to 70°C to remove the ash. The aluminum plate that has been cleaned in this way is then etched at a temperature of 10 to 60°C using a rectangular wave, a mezzanine wave, or a sine wave with alternating positive and negative currents at a rate of 5 to 100 A / dm 2The aluminum plate is electrolyzed in a nitric acid or hydrochloric acid electrolyte for 10 to 300 seconds at a current density of 10000 s. Then, the electrolyzed aluminum plate is anodized. Anodization is usually performed using sulfuric acid. The concentration of sulfuric acid used is 5 to 30%, and the current density is 1 to 15 A / dm 2 The oxidation temperature is 20-60°C and the oxidation time is 5-250 seconds to form 1-10 g / m 2 The oxide film formed in this way usually has a higher oxide film micropore, a stronger adsorption capacity, and is easy to adhere to dirt. Therefore, it is usually necessary to perform a pore sealing treatment. A variety of methods can be used for the pore sealing treatment, preferably to achieve 50% to 80% volume of the closed oxide film micropores. The anodized aluminum support can be further treated with a known post-anodic treatment (PAT) process to seal the oxide pores and make its surface hydrophilic, such as a treatment in an aqueous solution of the following substances: poly(vinylphosphonic acid) (PVPA), vinylphosphonic acid copolymers, poly[(meth)acrylic acid], or acrylic acid copolymers, a mixture of phosphates and fluoride salts, or sodium silicate.

[0115] The solution used for the plate substrate sealing treatment of the lithographic plate of the present invention preferably contains an aqueous solution of fluoride ions and phosphates.

[0116] Preparation of the lithographic printing plates of the present invention can be accomplished by applying an imageable layer to the hydrophilic surface of the lithographic substrate by conventional techniques. The imageable layer can be applied by any suitable method such as coating or lamination.

[0117] Usually, the components of the imageable layer are dispersed in or dissolved in a suitable coating solvent. For example, water, water and an organic solvent. For example, a mixture of methanol, ethanol, isopropanol, and / or acetone. A surfactant may be present, such as a fluorinated surfactant or a polyethoxylated dimethylpolysiloxane copolymer, or a mixture of surfactants to help other components to be dispersed in the coating solvent. The resulting mixture is applied to the lithographic substrate by conventional methods such as spin coating, bar coating, gravure coating, die coating, slot coating or roller coating. After coating, the imageable layer is dried to evaporate the solvent. The imageable layer can be air dried at room temperature or high temperature, such as in an oven. Alternatively, the imageable layer can be dried by blowing warm air over the imageable element.

[0118] After coating the imageable layer, a protective layer may be coated on top of this layer.

[0119] After the negative planographic plate precursor of the present invention is produced, it is exposed by a laser according to the image through digital data to give an undulating image opposite to the original plate. As a preferred exposure light source, for example, a solid-state laser and a semiconductor laser radiating infrared rays of 780-850nm are used. The infrared laser used in the present invention is preferably a laser capable of outputting 100mW or more, and the exposure time of each pixel is preferably not longer than 20 microseconds. The radiation energy is preferably 10-300mj / cm 2 .

[0120] After the lithographic printing plate precursor of the present invention is exposed imagewise, printing is performed by supplying printing ink and dampening liquid without receiving a developing process. Specifically, the lithographic printing plate precursor is exposed imagewise with a laser beam, and then the coating of the blank area is removed on a printing press by supplying printing ink and dampening liquid, and the image recording layer hardened by exposure forms a printing ink-receptive portion having an ink-receptive surface in the exposed portion of the image recording layer, the unhardened image recording layer is wetted and penetrated with the supplied dampening liquid to become loose, and then is removed by being transferred to paper by the printing ink, and a hydrophilic surface is exposed in the unexposed portion, thereby preparing a lithographic printing plate that can be printed. Subsequently, the dampening liquid adheres to the exposed hydrophilic surface, and the printing ink adheres to the image recording layer in the exposed portion, and the printing process begins.

[0121] During the machine development process, the plate surface should usually be pre-soaked with fountain solution for 10-60 seconds. The longer the time and the larger the amount of fountain solution, the more conducive it is to remove the coating in the blank area. Then, the ink is transferred to the surface of the lithographic plate precursor through the ink roller, and the coating in the blank area is peeled off by relying on the viscosity of the ink. The ink contact time is 10-30 seconds. The longer the time, the more conducive it is to remove the coating in the blank area.

[0122] In some cases, an aqueous washout may be used off-line to remove the unexposed areas and develop the imaged precursor, and to provide a protective layer or coating over the entire imaged and developed (washed) precursor printing surface. After off-line development, printing may be performed by placing the exposed and washed lithographic printing plate on a suitable printing press.

[0123] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that this embodiment is only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Technical personnel skilled in the art can make some non-essential improvements and adjustments based on the above-mentioned contents of the present invention.

[0124] Amphiphilic polymerizable monomers Raw materials used in the examples:

[0125] Aliphatic amine or aromatic amine Nanjing Chemical Reagent Factory

[0126] Alkali Metal Halogenated Alkyl Sulfonate Aladdin Reagents

[0127] Acrylamide Aladdin Reagent Company

[0128] Acrylic Acid Aladdin Reagent Company

[0129] 2-Acrylamido-2-Methylpropanesulfonic Acid Aladdin Reagent Company

[0130] Initiator Sinopharm Chemical Reagent Company

[0131] Preparation of amphiphilic polymerizable monomers:

[0132] Embodiment 1:

[0133] 1 mol of n-octylamine, 1 mol of sodium chloroethylsulfonate, 320 mL of ethanol and 80 mL of water (volume ratio of 4:1), and 20 g of sodium hydroxide were added to a 1 L three-necked flask, the pH value of the solution in the reactor was 10.2, and the mixture was reacted at 50°C for 12 hours. After cooling, the mixture was filtered to obtain a solid, which was determined to be an intermediate of sodium N-octylethylsulfonate by nuclear magnetic resonance analysis. 0.4 mol of the above sodium N-octylethylsulfonate intermediate was added to a 500 mL three-necked flask, 120 mL of water was added, and 10 g of sodium hydroxide was added. After the mixture was dissolved, 0.5 mol of acryloyl chloride was added dropwise within 2 hours, and the mixture was reacted at 5°C for 12 hours. After the solvent water was evaporated, the mixture was recrystallized with a mixed solvent of chloroform: methanol (volume ratio of 7:1), filtered, and dried to obtain a solid. The solid was confirmed to be the amphiphilic polymerizable monomer 2-octylacrylamidoethylsulfonate sodium D1 provided by the present invention by nuclear magnetic resonance analysis.

[0134] Embodiment 2:

[0135] 1 mol of dodecylamine, 1 mol of sodium chloroethylsulfonate, 300 mL of ethanol and 60 mL of water (volume ratio of 5:1), and 22 g of sodium hydroxide were added to a 1 L three-necked flask, the pH value of the solution in the reactor was 10.9, the mixture was reacted at 55° C. for 12 hours, and filtered after cooling to obtain a solid, which was determined to be an intermediate of sodium N-dodecylethylsulfonate by nuclear magnetic resonance analysis; 0.4 mol of the above sodium N-dodecylethylsulfonate intermediate was added to a 500 mL three-necked flask, 120 mL of water was added, 10 g of sodium hydroxide was added, and after dissolution, 0.52 mol of acryloyl chloride was added dropwise within 2 hours, the mixture was reacted at 8° C. for 12 hours, the solvent water was evaporated, and the mixture was recrystallized with a mixed solvent of chloroform: methanol (volume ratio of 7:1), filtered, and dried to obtain a solid, which was confirmed by nuclear magnetic resonance analysis to be the amphiphilic polymerizable monomer 2-dodecylacrylamidoethylsulfonate sodium D2 provided by the present invention.

[0136] Embodiment 3:

[0137] 1 mol of tetradecylamine, 1 mol of sodium chloroethylsulfonate, 240 mL of ethanol and 40 mL of water (volume ratio of 6:1), and 18 g of sodium hydroxide were added to a 1 L three-necked flask, the pH value of the solution in the reactor was 9.8, and the mixture was reacted at 60° C. for 14 hours. After cooling, the mixture was filtered to obtain a solid, and the solid was determined to be an N-tetradecyl sodium ethyl sulfonate intermediate by nuclear magnetic resonance analysis; 0.4 mol of the above-mentioned N-tetradecyl sodium ethyl sulfonate intermediate was added to a 500 mL three-necked flask, 120 mL of water was added, and 10 g of sodium hydroxide was added. After the mixture was dissolved, 0.55 mol of acryloyl chloride was added dropwise within 2 hours, and the mixture was reacted at 8° C. for 16 hours. After the solvent water was evaporated, the mixture was recrystallized with a mixed solvent of chloroform: methanol (volume ratio of 7:1), filtered, and dried to obtain a solid. The solid was confirmed by nuclear magnetic resonance analysis to be the amphiphilic polymerizable monomer 2-tetradecyl acrylamido sodium ethyl sulfonate D3 provided by the present invention.

[0138] Embodiment 4:

[0139] An amphiphilic monomer was prepared according to the method for preparing an amphiphilic monomer in Example 3, except that sodium chloroethyl sulfonate was replaced by potassium chloropropyl sulfonate, and the solvent ethanol was replaced by methanol, to obtain an amphiphilic monomer 2-tetradecyl acrylamidopropane sulfonate potassium D4.

[0140] Example 5

[0141] 1 mol of hexadecylamine, 1 mol of sodium chloroethylsulfonate, 280 mL of ethanol and 40 mL of water (volume ratio of 7:1), and 22 g of sodium hydroxide were added to a 1 L three-necked flask, the pH value of the solution in the reactor was 10.6, the mixture was reacted at 65°C for 14 hours, and filtered after cooling to obtain a solid, which was determined to be an N-hexadecyl sodium ethylsulfonate intermediate by nuclear magnetic resonance analysis; 0.4 mol of the above-mentioned N-hexadecyl sodium ethylsulfonate intermediate was added to a 500 mL three-necked flask, 120 mL of water was added, and 10 g of sodium hydroxide was added, and after dissolution, 0.58 mol of acryloyl chloride was added dropwise within 2 hours, the mixture was reacted at 5°C for 12 hours, the solvent water was evaporated, and the mixture was recrystallized with a mixed solvent of chloroform: methanol (volume ratio of 8:1), filtered, and dried to obtain a solid, which was confirmed by nuclear magnetic resonance analysis to be the amphiphilic polymerizable monomer 2-hexadecyl acrylamido sodium ethylsulfonate D5 provided by the present invention.

[0142] Raw materials used in the preparation examples of water-soluble heat-crosslinked multi-polymers:

[0143] Styrene Nanjing Chemical Reagent Factory

[0144] Ethyl Acrylate / Ethyl Methacrylate Aladdin Reagents

[0145] Example compound C1 / C2 Baoding Lucky Chemical Co., Ltd.

[0146] Example compounds D1 / D2 / D3 / D4 / D5 Baoding Lucky Chemical Co., Ltd.

[0147] Azobisisobutyronitrile Nanjing Chemical Reagent Factory

[0148] Potassium Persulfate Nanjing Chemical Reagent Factory

[0149] Preparation of water-soluble thermally cross-linked multipolymers:

[0150] Example 1 (multipolymer P01)

[0151] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 30 g of ethyl methacrylate and 30 g of example compound C1, heat and stir evenly, then add dropwise 20 g of styrene, 20 g of example compound D1 and 0.7 g of AIBN (azobisisobutyronitrile) at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for 12 hours before ending.

[0152] Example 2 (multipolymer P02)

[0153] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 1 g of ethyl methacrylate and 19 g of example compound C1, heat and stir evenly, then add dropwise 70 g of styrene, 10 g of example compound D1 and 0.7 g of AIBN (azobisisobutyronitrile) at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for 12 hours before ending.

[0154] Example 3 (multipolymer P03)

[0155] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 40 g of ethyl methacrylate and 25 g of example compound C1, heat and stir evenly, then add dropwise 25 g of styrene, 10 g of example compound D1 and 0.7 g of AIBN (azobisisobutyronitrile) at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0156] Example 4 (multipolymer P04)

[0157] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 29 g of ethyl methacrylate and 1 g of example compound C1, heat and stir evenly, then add dropwise 30 g of styrene, 40 g of example compound D1 and 0.7 g of potassium persulfate at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0158] Example 5 (multipolymer P05)

[0159] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 20 g of ethyl methacrylate and 40 g of example compound C1, heat and stir evenly, then add dropwise 39 g of styrene, 1 g of example compound D1 and 0.7 g of potassium persulfate at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0160] Example 6 (multi-polymer P06)

[0161] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 30 g of ethyl acrylate and 30 g of example compound C1, heat and stir evenly, add 20 g of styrene, 20 g of example compound D1 and 0.7 g of AIBN (azobisisobutyronitrile) dropwise at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0162] Example 7 (multipolymer P07)

[0163] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 19 g of ethyl acrylate and 1 g of example compound C1, heat and stir evenly, add 40 g of styrene, 40 g of example compound D1 and 0.7 g of potassium persulfate dropwise at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before termination.

[0164] Example 8 (multipolymer P08)

[0165] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 1 g of ethyl acrylate and 19 g of example compound C1, heat and stir evenly, add 70 g of styrene, 10 g of example compound D1 and 0.7 g of AIBN (azobisisobutyronitrile) dropwise at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0166] Example 9 (multipolymer P09)

[0167] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 30 g of ethyl methacrylate and 40 g of example compound C2, heat and stir evenly, then add dropwise 20 g of styrene, 10 g of example compound D1 and 0.7 g of AIBN (azobisisobutyronitrile) at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0168] Example 10 (Multi-polymer P10)

[0169] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 20 g of ethyl methacrylate and 10 g of example compound C2, heat and stir evenly, add 69 g of styrene, 1 g of example compound D1 and 0.7 g of potassium persulfate dropwise at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0170] Example 11 (multipolymer P11)

[0171] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 1 g of ethyl acrylate and 19 g of example compound C1, heat and stir evenly, then add dropwise 70 g of styrene, 10 g of example compound D2 and 0.7 g of AIBN (azobisisobutyronitrile) at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for 12 hours before ending.

[0172] Example 12 (multipolymer P12)

[0173] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 30 g of ethyl methacrylate and 40 g of example compound C2, heat and stir evenly, then add dropwise 20 g of styrene, 10 g of example compound D2 and 0.7 g of AIBN (azobisisobutyronitrile) at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0174] Example 13 (Multi-polymer P13)

[0175] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 20 g of ethyl methacrylate and 10 g of example compound C1, heat and stir evenly, then add dropwise 50 g of styrene, 20 g of example compound D2 and 0.7 g of potassium persulfate at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0176] Example 14 (Multi-component copolymer P14)

[0177] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 40 g of ethyl acrylate and 20 g of example compound C2, heat and stir evenly, then add dropwise 30 g of styrene, 10 g of example compound D3 and 0.7 g of AIBN (azobisisobutyronitrile) at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0178] Example 15 (multipolymer P15)

[0179] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 19 g of ethyl acrylate and 1 g of example compound C1, heat and stir evenly, add 40 g of styrene, 40 g of example compound D3 and 0.7 g of potassium persulfate dropwise at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before termination.

[0180] Example 16 (multipolymer P16)

[0181] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 30 g of ethyl methacrylate and 30 g of example compound C2, heat and stir evenly, then add dropwise 20 g of styrene, 20 g of example compound D4 and 0.7 g of AIBN (azobisisobutyronitrile) at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for 12 hours before ending.

[0182] Example 17 (multi-polymer P17)

[0183] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 20 g of ethyl acrylate and 20 g of example compound C1, heat and stir evenly, add dropwise 50 g of styrene, 10 g of example compound D4 and 0.7 g of potassium persulfate at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before termination.

[0184] Example 18 (multipolymer P18)

[0185] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 1 g of ethyl acrylate and 19 g of example compound C2, heat and stir evenly, add 70 g of styrene, 10 g of example compound D5 and 0.7 g of AIBN (azobisisobutyronitrile) dropwise at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0186] Example 19 (Multi-polymer P03)

[0187] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 10 g of ethyl acrylate and 40 g of example compound C1, heat and stir evenly, then add dropwise 30 g of styrene, 20 g of example compound D5 and 0.7 g of AIBN (azobisisobutyronitrile) at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0188] Example 20 (multipolymer P20)

[0189] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 15 g of ethyl methacrylate and 15 g of example compound C1, heat and stir evenly, add dropwise 30 g of styrene, 40 g of example compound D5 and 0.7 g of potassium persulfate at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0190] Comparative Example 21 (Multi-component Copolymer P21)

[0191] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 15 g of ethyl acrylate and 15 g of example compound C2, heat and stir evenly, add 10 g of styrene, 60 g of example compound D2 and 0.7 g of AIBN (azobisisobutyronitrile) dropwise at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0192] Comparative Example 22 (Multi-component copolymer P22)

[0193] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 10 g of ethyl methacrylate and 5 g of example compound C1, heat and stir evenly, then add dropwise 80 g of styrene, 5 g of example compound D1 and 0.7 g of potassium persulfate at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0194] Comparative Example 23 (Multi-component copolymer P23)

[0195] In a 1000 ml four-necked flask equipped with temperature-controlled heating, mechanical stirring, condensation reflux and nitrogen protection, add 500 g of isopropanol, 150 g of deionized water, 10 g of ethyl methacrylate and 55 g of example compound C2, heat and stir evenly, then add dropwise 20 g of styrene, 15 g of example compound D1 and 0.7 g of potassium persulfate at 60°C for 2.5 hours, add 0.3 g of AIBN (azobisisobutyronitrile) after reacting for 7.5 hours, and continue to react for another 12 hours before ending.

[0196] Raw materials used in the formulation examples of the imageable layer formulation:

[0197] Multi-component copolymer with structure P Lucky Huaguang Printing Technology Co., Ltd.

[0198] Polyurethane acrylic prepolymer Baoding Lucky Chemical Co., Ltd.

[0199] Sartomer 399 Sartomer Co., Inc.

[0200] Ionium Salt Initiator Lucky Research Institute

[0201] Infrared Absorption Dye IR Lucky Research Institute

[0202] BYK-330 BYK

[0203] 1-Methoxy-2-propanol Nanjing Oriental Pearl Industry and Trade Co., Ltd.

[0204] The multi-polymer of structure P is a 25.0% DMF solution (weight percentage), and DMF is a common solvent in organic synthesis. Structure P is the water-soluble thermally cross-linked multi-polymer P1-P23 obtained in the above examples and comparative examples.

[0205] The prepolymer is a 50% MEK solution (weight percentage), and MEK is a common solvent in organic synthesis.

[0206] The structure of the iodonium salt initiator is as follows:

[0207]

[0208] The structure of infrared absorbing dye IR is as follows:

[0209]

[0210] Terminology Note:

[0211] Start-up tolerance: The adaptability of the machine-developed plate to the printing press status, the amount of fountain solution, the water contact time and the ink during the development process on the printing press. A large start-up tolerance of the plate indicates that it has good adaptability to the printing press, fountain solution and ink, and the printing press has a large operating space.

[0212] Number of papers lost from the start of paper feeding to the time when the blank is clean and the ink color is balanced.

[0213] Solvent resistance: After coating, drying and exposure on the plate base, the coating loss is measured by soaking in solvents such as isopropyl alcohol for a certain period of time. If the coating loss is large, it means that the plate has poor solvent resistance and low UV ink resistance during printing.

[0214] Preparation of the plate base: A1050 rolled aluminum plate with a diameter purity of 99.5% and a thickness of 0.3 mm was heated to 70°C in a 5% mass fraction sodium hydroxide aqueous solution. OC for 20 seconds, rinse with running water, and immediately neutralize with a 1% nitric acid aqueous solution. Then, in a 1% hydrochloric acid aqueous solution, 40 O C with a sine wave AC current of 40A / dm 2 The current density was used for electrolytic roughening for 16 seconds. Then 40 O C, neutralize with 5% sodium hydroxide aqueous solution for 10 seconds. Wash with water. Finally, O C, use a 20% sulfuric acid aqueous solution at 15A / dm 2 The current density was 200 ppm, and the anodization was carried out for 20 seconds. Washed with water. The pores were sealed with 200 ppm sodium fluoride and 6% sodium dihydrogen phosphate aqueous solution at 60°C for 20 seconds. Washed with water. Drying. The plate substrate thus obtained had an average center line roughness of 0.40 μm and an oxide film weight of 3.0 g / m 2 .

[0215] Photosensitive layer coating: Use a rod coater to coat the following photosensitive liquid formulation on the hydrophilized substrate, and then dry at 100°C for 60 seconds. 2 The dry weight of the coating is 100% to form a negative-working lithographic plate precursor sensitive to infrared radiation. The photosensitive layer here is the imageable layer. The photosensitive liquid is mixed with the following components (each component is calculated by weight) to obtain a photosensitive liquid formulation.

[0216] Example 1 (Printing Plate A1)

[0217] Water-soluble thermally cross-linked multipolymer P01 0.79

[0218] Polyurethane acrylic oligomer 4.62

[0219] Multifunctional acrylic monomer (Sartomer 399) 0.90

[0220] Ionium salt initiator 0.70

[0221] 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine 0.09

[0222] Infrared absorbing dye IR 0.71

[0223] BYK-330 0.28

[0224] 1-Methoxy-2-propanol 92.40

[0225] Example 2 (Printing Plate A2)

[0226] Water-soluble thermally cross-linked multipolymer P02 4.72

[0227] Polyurethane acrylic oligomer 0.69

[0228] Multifunctional acrylic monomer (Sartomer 399) 0.10

[0229] Ionium salt initiator 1.50

[0230] 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine 0.27

[0231] Infrared absorbing dye IR 0.39

[0232] BYK-330 0.20

[0233] 1-Methoxy-2-propanol 92.40

[0234] Example 3 (Printing Plate A3)

[0235] Water-soluble thermally cross-linked multipolymer P03 3.15

[0236] Polyurethane acrylic oligomer 1.17

[0237] Multifunctional acrylic monomer (Sartomer 399) 0.80

[0238] Ionium salt initiator 1.90

[0239] 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine 0.46

[0240] Infrared absorbing dye IR 0.12

[0241] BYK-330 0.28

[0242] 1-Methoxy-2-propanol 92.40

[0243] Example 4 (Printing Plate A4)

[0244] Water-soluble thermally cross-linked multipolymer P04 1.97

[0245] Polyurethane acrylic oligomer 1.95

[0246] Multifunctional acrylic monomer (Sartomer 399) 1.20

[0247] Ionium salt initiator 0.10

[0248] 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine 0.02

[0249] Infrared absorbing dye IR 2.36

[0250] BYK-330 0.28

[0251] 1-Methoxy-2-propanol 92.40

[0252] Example 5 (Printing Plate A5)

[0253] Water-soluble thermally cross-linked multipolymer P05 3.15

[0254] Polyurethane acrylic oligomer 1.80

[0255] Multifunctional acrylic monomer (Sartomer 399) 0.95

[0256] Ionium salt initiator 0.90

[0257] 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine 0.32

[0258] Infrared absorbing dye IR 0.48

[0259] BYK-330 0.28

[0260] 1-Methoxy-2-propanol 92.40

[0261] Example 6 (Printing Plate A6)

[0262] Water-soluble thermally cross-linked multipolymer P06 2.75

[0263] Polyurethane acrylic oligomer 2.05

[0264] Multifunctional acrylic monomer (Sartomer 399) 1.10

[0265] Ionium salt initiator 0.80

[0266] 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine 0.42

[0267] Infrared absorbing dye IR 0.48

[0268] BYK-330 0.28

[0269] 1-Methoxy-2-propanol 92.40

[0270] Example 7 (Printing Plate A7)

[0271] Water-soluble thermally cross-linked multipolymer P07 3.15

[0272] Polyurethane acrylic oligomer 1.17

[0273] Multifunctional acrylic monomer (Sartomer 399) 0.80

[0274] Ionium salt initiator 2.06

[0275] 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine 0.30

[0276] Infrared absorbing dye IR 0.12

[0277] BYK-330 0.28

[0278] 1-Methoxy-2-propanol 92.40

[0279] Example 8 (Printing Plate A8)

[0280] Water-soluble thermally cross-linked multipolymer P08 1.97

[0281] Polyurethane acrylic oligomer 1.95

[0282] Multifunctional acrylic monomer (Sartomer 399) 1.20

[0283] Ionium salt initiator 0.10

[0284] 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine 0.02

[0285] Infrared absorbing dye IR 2.36

[0286] BYK-330 0.28

[0287] 1-Methoxy-2-propanol 92.40

[0288] Except for the water-soluble heat-crosslinked multipolymer, the other ingredients and amounts of the photosensitive liquid formulations in the following embodiments are the same. When the water-soluble heat-crosslinked multipolymers are P9-P20, the corresponding printing plate embodiments A9-A20 are obtained in sequence, and when the water-soluble heat-crosslinked multipolymers are P21-P23, the corresponding printing plate comparison examples A21-A23 are obtained.

[0289] Water-soluble thermally cross-linked multipolymer P 3.05

[0290] Polyurethane acrylic oligomer 2.25

[0291] Multifunctional acrylic monomer (Sartomer 399) 0.85

[0292] Ionium salt initiator 0.81

[0293] 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine 0.18

[0294] Infrared absorbing dye IR 0.48

[0295] BYK-330 0.28

[0296] 1-Methoxy-2-propanol 92.40

[0297] The plate obtained in this way is exposed on a Kodak Thermal CTP plate-making machine to determine the appropriate exposure energy. Then, according to the corresponding exposure energy, the exposed plate is directly installed on the Heidelberg SpeedMaster74 printing press, the printing press is turned on, 50% of the fountain solution is used to wet the entire plate surface for 10 seconds, and then the paper is supplied to start printing. Its performance is listed in the following Table 1, and the number of plates passed is listed in the following Table 1 Start-up Method ①.

[0298] The plate obtained by the above method was exposed on a Kodak Thermal CTP plate-making machine to determine the appropriate exposure energy. Then, according to the corresponding exposure energy, the exposed plate was directly installed on the Manroland 700 printing press, and the printing press was turned on. The water volume of the dampening solution was 35%, and the entire plate surface was moistened for 90 seconds, and then the paper was supplied to start printing. The number of plates passed is listed in the following Table 1 Start-up Method ②.

[0299] Table 1

[0300]

[0301] The above description is only a preferred embodiment of the present invention, but the protection scope of the present invention is not limited thereto. It should be pointed out that for those skilled in the art and any technician familiar with the technical field, without departing from the overall concept of the present invention, the technical solution and the inventive concept of the present invention are equivalently replaced or changed, and several changes and improvements are made, which should also be regarded as the protection scope of the present invention.

Claims

1. A water-soluble thermally cross-linked multipolymer, characterized in that: The water-soluble thermally cross-linked copolymer contains at least the following copolymer units: -ABCD-; A represents a styrene copolymer unit; B represents an ethyl (meth)acrylate copolymer unit; C represents a copolymer unit having an amined unsaturated double bond branch: R1 is a H atom or a methyl group, and R2 is a CH2=C(CH3)COOCH2CH2NHCO- group; D represents an acrylamide copolymer unit containing a sulfonic acid alkyl group: Wherein, n is an integer of 0-8, R is an alkyl or aryl group having 3-18 carbon atoms, and M is an alkali metal element; The weight percentage content of the styrene copolymer unit A in the water-soluble heat-crosslinked multipolymer is 20%-70%; the weight percentage content of the (meth) ethyl acrylate copolymer unit B in the water-soluble heat-crosslinked multipolymer is 1%-40%; the weight percentage content of the copolymer unit C having amined unsaturated double bond side chains in the water-soluble heat-crosslinked multipolymer is 1%-40%; the weight percentage content of the acrylamide copolymer unit D containing sulfonic acid alkyl in the water-soluble heat-crosslinked multipolymer is 1%-40%.

2. The water-soluble heat-crosslinked multipolymer according to claim 1, characterized in that: For the acrylamide copolymer unit D containing a sulfonic acid alkyl group, wherein n is an integer of 1 to 4, R is any one selected from n-hexyl, n-octyl, n-nonyl, n-decyl, n-dodecyl, n-tetradecyl, p-octylphenyl and p-dodecylphenyl, and M is sodium or potassium; The weight average molecular weight of the water-soluble heat-crosslinked copolymer is 2000-300000; and the glass transition temperature is 30-400°C.

3. The water-soluble heat-crosslinked multipolymer according to claim 1, characterized in that: For the acrylamide copolymer unit D containing a sulfonic acid alkyl group, wherein n is 1 or 2, R is any one selected from n-octyl, n-dodecyl, n-tetradecyl, p-dodecylphenyl and n-hexadecyl, and M is sodium; The weight average molecular weight of the water-soluble heat-crosslinked copolymer is 10,000-200,000; the glass transition temperature is 40-300°C; The weight percentage content of the styrene copolymer unit A in the water-soluble heat-crosslinked multipolymer is 30%-60%; the weight percentage content of the (meth) ethyl acrylate copolymer unit B in the water-soluble heat-crosslinked multipolymer is 1%-30%; the weight percentage content of the copolymer unit C with amined unsaturated double bond side chains in the water-soluble heat-crosslinked multipolymer is 1%-30%; the weight percentage content of the acrylamide copolymer unit D containing sulfonic acid alkyl in the water-soluble heat-crosslinked multipolymer is 1%-30%.

4. The method for preparing the water-soluble heat-crosslinked multipolymer according to any one of claims 1 to 3, characterized in that: The random copolymerization method is adopted, the polymerization initiator contains at least one of benzoyl peroxide, persulfate or azo compound, and the copolymerization mode is emulsion polymerization.

5. A negative lithographic printing plate precursor, characterized in that: The imageable layer comprises a water-soluble heat-crosslinked copolymer, a polymerizable / crosslinked component, an infrared radiation absorber and an initiator. The water-soluble heat-crosslinked copolymer comprises the water-soluble heat-crosslinked multipolymer according to any one of claims 1 to 3.

6. The negative lithographic printing plate precursor according to claim 5, characterized in that: The water-soluble heat-crosslinked copolymer accounts for 10%-60% by weight of the imageable layer, the polymerizable / crosslinked component accounts for 10%-70% by weight of the imageable layer, the infrared radiation absorber accounts for 1%-30% by weight of the imageable layer, and the initiator accounts for 1%-30% by weight of the imageable layer.

7. The negative lithographic printing plate precursor according to claim 6, characterized in that: The water-soluble heat-crosslinked copolymer accounts for 20%-40% by weight of the imageable layer, the polymerizable / crosslinked component accounts for 20%-50% by weight of the imageable layer, the infrared radiation absorber accounts for 1%-15% by weight of the imageable layer, and the initiator accounts for 3%-20% by weight of the imageable layer.

8. The negative lithographic printing plate precursor according to any one of claims 5 to 7, characterized in that: The weight average molecular weight of the water-soluble heat-crosslinked multi-polymer is 30,000-150,000; the glass transition temperature is 60-150°C; The weight percentage content of the styrene copolymer unit A in the water-soluble heat-crosslinked multi-polymer is 40%-60%; the weight percentage content of the (meth) ethyl acrylate copolymer unit B in the water-soluble heat-crosslinked multi-polymer is 1%-25%; the weight percentage content of the copolymer unit C having amined unsaturated double bond side chains in the water-soluble heat-crosslinked multi-polymer is 5%-20%; the weight percentage content of the acrylamide copolymer unit D containing sulfonic acid alkyl in the water-soluble heat-crosslinked multi-polymer is 5%-25%; The polymerizable / cross-linkable component is composed of at least one of an ethylenically unsaturated free radical polymerizable monomer or a free radical cross-linkable polymer; the infrared radiation absorber is a cyanine dye absorbing at 750-850nm; and the initiator is selected from one or more of iodonium salts, sulfonium salts, phosphonium salts, and selenium salts.

9. The negative lithographic printing plate precursor according to claim 5, characterized in that: The imageable layer further comprises at least one of a pigment, an organic or inorganic particle, a sensitized dye, a wetting agent, a plasticizer, a binder, a surfactant, an antioxidant, a coating aid, an anti-stabilizer and a brightener.

10. The method for preparing a negative lithographic printing plate precursor according to any one of claims 5 to 9, characterized in that: The raw materials of the imageable layer are mixed to obtain a photosensitive liquid preparation, which is then coated on a hydrophilized plate substrate using a rod coater or other equipment or method, and then dried in a suitable manner to obtain a negative-working lithographic plate precursor.

Citation Information

Cited By

  • Cleaning agent for treatment-free CTP plate as well as preparation method and application of cleaning agent

    CN121379234A