Aqueous acrylic polymer dispersant and preparation method and application thereof

Through the polymerization of alkyl glycoside modified acrylate monomers and acrylate monomers, the dispersion performance of aqueous polyacrylate polymer dispersants is enhanced, and the problem of low dispersion performance in the prior art is solved, thereby achieving high efficiency and low viscosity and stable pigment dispersion effect, suitable for water-based coatings and inks.

CN116554395BActive Publication Date: 2024-11-01CHONGQING KOOPPER CHEM IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310588184.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-01
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

The dispersion performance of existing aqueous polyacrylate polymer dispersants is relatively low, and it is difficult to meet the requirements of high efficiency and environmentally friendly in coatings and inks.

Method used

Polymerized with alkyl glycoside modified acrylate monomers and acrylate monomers, providing strong anchoring and steric hindrance functions through the polyhydroxy groups and ring structures in alkyl glycosides, enhancing the dispersion performance of non-polar pigments .

Benefits of technology

It significantly improves the efficiency of water-based dispersants, which are characterized by excellent dispersion performance, low viscosity, fluidity and stability, and greatly improves the dispersion capacity of pigments such as carbon black, phthalocyanine blue, iron oxide red, etc., and is suitable for water-based coatings. and ink.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0005007989150000011
    Figure FDA0005007989150000011
  • Figure FDA0005007989150000012
    Figure FDA0005007989150000012
  • Figure GDA0004933785650000021
    Figure GDA0004933785650000021
Patent Text Reader

Abstract

The present invention belongs to the technical field of dispersants, and specifically relates to a method for preparing a water-based acrylic ester polymer dispersant, comprising the following steps: S1, esterification reaction of acrylic acid (ester) monomers with alkyl glycoside to obtain alkyl glycoside modified acrylic acid ester monomers; S2, mixing the alkyl glycoside modified acrylic acid ester monomers in step S1 with acrylic acid (ester) monomers, a part of initiator, and chain transfer aid, and then dropping into 60-90°C deionized water, adding another part of initiator after constant temperature reaction for 2h, continuing constant temperature reaction for more than 4h, cooling after the reaction, and neutralizing with a pH regulator to obtain a water-based acrylic acid ester polymer dispersant. The water-based acrylic acid ester polymer dispersant in the present invention is suitable for dispersing pigments such as carbon black, phthalocyanine blue, red iron oxide, titanium dioxide, etc., has high efficiency, has excellent color development for pigments, and the obtained color paste has low viscosity and excellent stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of dispersants, and in particular relates to an aqueous acrylate polymer dispersant and a preparation method and application thereof. Background Art

[0002] As one of the key additives in coatings / inks, water-based dispersants have been widely studied by experts and scholars at home and abroad. Among them, due to the diversity of monomers of water-based polyacrylate polymer dispersants, such as acrylic acid (ester), styrene, hydroxyethyl acrylate, etc., it provides a variety of possibilities for molecular design, thus meeting various needs in practical applications. Dispersants based on water-based polyacrylate polymers provide excellent dispersion / stabilization properties for pigments and fillers such as carbon black, phthalocyanine blue, red iron oxide, and titanium dioxide.

[0003] With the increasing requirements for environmental protection of coatings / inks, water-based dispersant products tend to be more efficient, that is, water-based dispersants have more effective dispersing effects at the same usage content, or less usage at the same dispersing effect; in addition, water-based dispersants are also required to have better environmental friendliness. Therefore, as an important branch of water-based dispersants, water-based polyacrylate polymer dispersants have higher requirements.

[0004] The excellent dispersibility of waterborne polyacrylate polymer dispersants mainly comes from the fact that their molecular chains contain anchoring groups that have different effects on pigment and filler particles, such as carboxyl, hydroxyl and amide groups; at the same time, the special structure on the molecular chain provides different degrees of hydrophobic effect, such as aromatic hydrocarbons, aliphatic hydrocarbon ring structures, C4-C12 long-chain alkanes, etc.; in addition, the molecular chain also improves dispersibility by providing different degrees of steric hindrance effect. At present, the monomers introduced into the molecular chain of the dispersant often have relatively simple functions. For example, the Chinese patent document CN106397656A (publication date: February 15, 2017) improves the dispersibility of polymer dispersants by introducing aromatic hydrocarbon-containing monomers. The patent document introduces that aromatic hydrocarbon monomers mainly provide a certain degree of hydrophobic effect; another example is the Chinese patent document CN109181402A (publication date: January 11, 2019) obtained by polymerizing vinyl monomers to obtain a solution and then compounding. As such, the degree of improvement in the dispersibility of aqueous dispersant products is low, and the requirement for high efficiency of aqueous dispersant products is difficult to meet. Summary of the invention

[0005] The present invention is intended to provide a method for preparing an aqueous acrylic ester polymer dispersant, so as to solve the problem that the introduction of a monomer with a single function leads to a low degree of improvement in the dispersibility of an aqueous dispersant product.

[0006] In order to achieve the above object, the scheme of the present invention is: a method for preparing an aqueous acrylic ester polymer dispersant, comprising the following steps:

[0007] S1. Preparation of alkyl glycoside modified acrylate monomer:

[0008] (1) adding a catalyst and hydroquinone to an alkyl polyglycoside at 70-85° C. and stirring to obtain a mixed system I;

[0009] (2) dropping acrylic acid (ester) monomers into the mixed system I, reacting at a constant temperature for 4 to 7 hours after the dropping is completed, taking samples to test the acid value until the acid value remains unchanged, thereby obtaining an alkyl glycoside-modified acrylic acid ester monomer;

[0010] S2. Preparation of water-based acrylic polymer dispersant:

[0011] (1) The initiator is divided into two parts, and the alkyl glycoside modified acrylate monomer obtained in step S1 is mixed with an acrylic acid (ester) monomer, a part of the initiator, and a chain transfer aid, and stirred to obtain a mixed system II, and the mixed system II is added dropwise to deionized water at 60 to 90° C. After the addition is completed, the temperature is raised to 80 to 100° C. and the reaction is carried out at a constant temperature for 2 hours, and another part of the initiator is added, and the reaction is continued at a constant temperature for more than 4 hours;

[0012] (2) After the isothermal reaction is completed, the temperature is lowered to 40° C., and the pH value is adjusted to 7-8 using a pH adjuster to obtain an aqueous acrylate polymer dispersant.

[0013] Optionally, the structural formula of the alkyl glycoside used in step S1 is as shown in formula (I):

[0014]

[0015] Wherein, R1 is a C1-C18 alkane or a derivative thereof.

[0016] Optionally, the acrylic acid (ester) monomer used in step S1 is one or both of methacrylic acid and acrylic acid; the structure of the alkyl glycoside-modified acrylic acid ester monomer obtained in step S1 is shown in formula (II):

[0017]

[0018] Wherein, R2 is H or CH3.

[0019] Optionally, in step S1, the acrylic acid (ester) monomer, the alkyl glycoside, the hydroquinone and the catalyst are respectively 14 to 26 parts, 73 to 86 parts, 0.05 to 0.1 parts and 0.2 to 2.0 parts by weight.

[0020] Optionally, the catalyst used in step S1 is one or both of p-toluenesulfonic acid and dodecylbenzenesulfonic acid.

[0021] Optionally, the acrylic acid (ester) monomer used in step S2 is one or more of acrylic acid, methyl acrylate, methacrylic acid, methacrylate, acrylamide, hydroxyethyl acrylate, hydroxyethyl methacrylate, butyl acrylate, butyl methacrylate, glycidyl methacrylate, lauryl acrylate, 2-acrylamide-2-methylpropane sulfonic acid, sodium p-styrene sulfonate, sodium methacrylic acid, maleic acid, maleic anhydride and itaconic acid.

[0022] Optionally, the initiator used in step S2 is one of ammonium sulfate, azobisisoheptanitrile and azobisisobutyronitrile.

[0023] Optionally, the chain transfer aid used in step S2 is one or two of dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid and isopropanol.

[0024] Optionally, the pH adjuster used in step S2 is adjusted to one or more of ammonia water, monoethanolamine, diethanolamine, sodium hydroxide, potassium hydroxide, triethanolamine, N,N-dimethylethanolamine and 2-amino-2-methyl-1-propanol.

[0025] Optionally, in step S2, the amount of acrylic acid (ester) monomer used is 55-90% of the total mass of the reactants in step S2.

[0026] Optionally, in step S2, the amount of the alkyl glycoside-modified acrylate monomer used is 10-60% of the total mass of the reactants in step S2.

[0027] Optionally, in step S2, the amount of the initiator used is 1.0 to 6.0% of the total mass of the reactants in step S2.

[0028] Optionally, in step S2, the amount of the chain transfer aid is 0.5-10.0% of the total mass of the reactants in step S2.

[0029] The present invention also provides an aqueous acrylate polymer dispersant prepared by the above preparation method, and the aqueous acrylate polymer dispersant is applied to aqueous coating dispersants and ink dispersants.

[0030] The working principle and beneficial effects of this solution are as follows: the water-based acrylic polymer dispersant of this solution is obtained by polymerizing alkyl glycoside-modified acrylic monomers with acrylic acid (ester) monomers, wherein the polyhydroxyl groups in the alkyl glycoside structure provide strong and effective anchoring ability, the cyclic structure provides efficient steric hindrance function, and the alkyl or its derivative structure (R1) enhances the steric hindrance ability and provides a solvation chain effect. Under the above effects, the water-based acrylic polymer dispersant of this solution has excellent dispersibility for non-polar pigment filler carbon black, and improves the high efficiency of water-based dispersant products.

[0031] Moreover, since the polyhydroxyl groups in the glycoside structure of the aqueous acrylic polymer dispersant and the carboxyl groups in the acrylic acid monomer have a strong adsorption effect on the carbon black particles, and at the same time, the glycoside structure forms a strong steric hindrance between the carbon black particles, the color paste prepared by the aqueous acrylic polymer dispersant in this scheme has excellent fluidity and low viscosity. At the same dispersant dosage, its viscosity is lower than that without the glycoside structure, the fluidity is excellent, and the color development and stability are greatly improved. Its efficient dispersing ability is obvious. Similarly, the aqueous acrylic polymer dispersant in this scheme has an efficient dispersing ability for dispersing pigments such as phthalocyanine blue, red iron oxide, and titanium dioxide, and also has excellent color development. The prepared color paste has the properties of low viscosity, high color concentration, and excellent stability, and can be widely used in water-based coatings, inks and other fields. DETAILED DESCRIPTION

[0032] The following is further described in detail through specific implementation methods:

[0033] Example 1

[0034] This embodiment provides a method for preparing an aqueous acrylate polymer dispersant, which specifically comprises the following steps:

[0035] S1. Preparation of alkyl glycoside modified acrylate monomer:

[0036] (1) 50 kg of methyl glucoside was added to a reaction kettle, N2 was introduced, the mixture was ventilated three times, and the mixture was heated to 70±1°C. After the vacuum pump was turned on to remove water, 0.073 kg of hydroquinone and 0.73 kg of p-toluenesulfonic acid were added and stirred evenly to obtain a mixed system I.

[0037] (2) 23.8 kg of methacrylic acid was slowly added dropwise to the reaction kettle (i.e., methacrylic acid was slowly added dropwise to the mixed system I), and the dripping was completed within 90 minutes. After the reaction was carried out at a constant temperature for 4 hours, samples were taken every 0.5 hours to test the acid value until the acid value remained unchanged. The material was discharged to obtain an alkyl glycoside-modified acrylate monomer, methyl methacrylate glucoside.

[0038] S2. Preparation of water-based acrylic polymer dispersant:

[0039] (1) 20 kg of methyl methacrylate methyl glucoside, 5 kg of styrene, 10 kg of methacrylic acid, 15 kg of acrylic acid, 1.8 kg of azobisisobutyronitrile and 2 kg of dodecyl mercaptan are added to a stirring kettle in sequence and mixed evenly to obtain a mixed system II for standby use; at the same time, 20 kg of deionized water is added to the reaction kettle, heated to 70°C under a N2 atmosphere, and then the mixed system II in the stirring kettle is slowly added dropwise under stirring. The addition is completed within 120 minutes, and after the addition is completed, the reaction system is heated to 85°C, and the reaction is carried out at a constant temperature for 2 hours under stirring, and then 0.2 kg of azobisisobutyronitrile is added and the reaction is continued at a constant temperature for 4 hours.

[0040] (2) After the constant temperature reaction is completed, the temperature in the reactor is lowered to 40° C., 30 wt % NaOH solution is added to the reactor, stirred, the pH value is adjusted to 7-8, filtered, and the filtrate is collected to obtain an aqueous acrylate polymer dispersant.

[0041] The aqueous acrylate polymer dispersant obtained in step S2 was sampled, and the conversion rate was measured to be 99.5%. The effective ingredient content of the aqueous acrylate polymer dispersant obtained in step S2 was calculated according to the conversion rate. 16.7 kg of deionized water was added to the aqueous acrylate polymer dispersant obtained in step S2 to obtain an aqueous acrylate polymer dispersant product a with an effective ingredient content of 50±1%.

[0042] Example 2

[0043] This embodiment provides a method for preparing an aqueous acrylate polymer dispersant, which specifically comprises the following steps:

[0044] S1. Preparation of alkyl glycoside modified acrylate monomer:

[0045] (1) 50 kg of lauryl glucoside was added to a reaction kettle, N2 was introduced, the mixture was ventilated three times, and the mixture was heated to 70±1°C. After the vacuum pump was turned on to remove water, 0.063 kg of hydroquinone and 0.63 kg of p-toluenesulfonic acid were added and stirred evenly to obtain a mixed system I.

[0046] (2) 12.6 kg of methacrylic acid was slowly added dropwise to the reaction kettle (i.e., methacrylic acid was slowly added dropwise to the mixed system I), and the dripping was completed within 90 minutes. After the reaction was carried out at a constant temperature for 4 hours, samples were taken every 0.5 hours to test the acid value until the acid value remained unchanged. The material was discharged to obtain methacrylate lauryl glucoside ester.

[0047] S2. Preparation of water-based acrylic polymer dispersant:

[0048] (1) 15 kg of lauryl glucoside methacrylate, 5 kg of styrene, 5 kg of methacrylic acid, 10 kg of acrylic acid, 1.4 kg of azobisisobutyronitrile and 1.75 kg of dodecyl mercaptan are sequentially added into a stirring kettle and mixed evenly to obtain a mixed system II for standby use; at the same time, 10 kg of deionized water is added into the reaction kettle, heated to 60°C under N2 atmosphere, and then the mixed system II in the stirring kettle is slowly added dropwise under stirring. The addition is completed within 120 minutes, and after the addition is completed, the reaction system is heated to 85°C, and reacted at a constant temperature for 2 hours under stirring, and then 0.35 kg of azobisisobutyronitrile is added, and the constant temperature reaction is continued for 4 hours.

[0049] (2) After the constant temperature reaction is completed, the temperature in the reactor is lowered to 40° C., 30 wt % NaOH solution is added to the reactor, stirred, the pH value is adjusted to 7-8, filtered, and the filtrate is collected to obtain an aqueous acrylate polymer dispersant.

[0050] The aqueous acrylate polymer dispersant obtained in step S2 was sampled, and the conversion rate was measured to be 99.2%. The effective ingredient content of the aqueous acrylate polymer dispersant obtained in step S2 was calculated according to the conversion rate. 17.65 kg of deionized water was added to the aqueous acrylate polymer dispersant obtained in step S2 to obtain an aqueous acrylate polymer dispersant product b with an effective ingredient content of 50±1%.

[0051] Example 3

[0052] This embodiment provides a method for preparing an aqueous acrylate polymer dispersant, which specifically comprises the following steps:

[0053] S1. Preparation of alkyl glycoside modified acrylate monomer:

[0054] (1) 50 kg of lauryl glucoside was added to a reaction kettle, N2 was introduced, the mixture was ventilated three times, and the mixture was heated to 70±1°C. After the vacuum pump was turned on to remove water, 0.061 kg of hydroquinone and 0.61 kg of dodecylbenzene sulfonic acid were added and stirred evenly to obtain a mixed system I.

[0055] (2) 10.86 kg of acrylic acid was slowly added dropwise to the reaction kettle (i.e., acrylic acid was slowly added dropwise to the mixed system I), and the dripping was completed within 90 minutes. After the reaction was carried out at a constant temperature for 4 hours, samples were taken every 0.5 hours to test the acid value until the acid value remained unchanged. The material was discharged to obtain lauryl glucoside acrylate.

[0056] S2. Preparation of water-based acrylic polymer dispersant:

[0057] (1) 15 kg of lauryl glucoside acrylate, 5 kg of methacrylic acid, 5 kg of butyl methacrylate, 10 kg of acrylic acid, 1.4 kg of azobisisobutyronitrile and 1.75 kg of thioglycolic acid were added to a stirring kettle in sequence and mixed evenly to obtain a mixed system II for standby use; at the same time, 10 kg of deionized water was added to the reaction kettle, heated to 60°C under N2 atmosphere, and then the mixed system II in the stirring kettle was slowly added dropwise under stirring. The addition was completed within 120 minutes, and after the addition was completed, the reaction system was heated to 85°C, and the reaction was carried out at a constant temperature for 2 hours under stirring, and then 0.35 kg of azobisisobutyronitrile was added and the reaction was continued at a constant temperature for 4 hours.

[0058] (2) After the constant temperature reaction is completed, the temperature in the reactor is lowered to 40° C., diethanolamine is added to the reactor, stirred, the pH value is adjusted to 7-8, filtered, and the filtrate is collected to obtain an aqueous acrylate polymer dispersant.

[0059] The aqueous acrylate polymer dispersant obtained in step S2 was sampled, and the conversion rate was measured to be 99.3%. The effective ingredient content of the aqueous acrylate polymer dispersant obtained in step S2 was calculated according to the conversion rate. 7.45 kg of deionized water was added to the aqueous acrylate polymer dispersant obtained in step S2 to obtain an aqueous acrylate polymer dispersant product c with an effective ingredient content of 50±1%.

[0060] Example 4

[0061] This embodiment provides a method for preparing an aqueous acrylate polymer dispersant, which specifically comprises the following steps:

[0062] S1. Preparation of alkyl glycoside modified acrylate monomer:

[0063] (1) 50 kg of n-octyl glucoside was added to a reaction kettle, N2 was introduced, the mixture was ventilated three times, and the mixture was heated to 70±1°C. After the vacuum pump was turned on to remove water, 0.063 kg of hydroquinone and 0.63 kg of dodecylbenzenesulfonic acid were added and stirred evenly to obtain a mixed system I.

[0064] (2) 12.71 kg of acrylic acid was slowly added dropwise to the reaction kettle (i.e., acrylic acid was slowly added dropwise to the mixed system I), and the dripping was completed within 90 minutes. After the reaction was carried out at a constant temperature for 4 hours, samples were taken every 0.5 hours to test the acid value until the acid value remained unchanged. The material was discharged to obtain n-octyl glucoside of acrylic acid.

[0065] S2. Preparation of water-based acrylic polymer dispersant:

[0066] (1) 25 kg of octyl glucoside acrylate, 4.5 kg of butyl methacrylate, 3.79 kg of acrylic acid, 0.83 kg of azobisisobutyronitrile and 2.23 kg of mercaptopropionic acid were added to a stirring kettle in sequence and mixed evenly to obtain a mixed system II for standby use; at the same time, 10 kg of deionized water was added to the reaction kettle, heated to 60°C under N2 atmosphere, and then slowly added dropwise to the mixed system II in the stirring kettle under stirring. The addition was completed over 120 minutes, and after the addition was completed, the reaction system was heated to 85°C, and reacted at a constant temperature for 2 hours under stirring, and then 0.23 kg of azobisisobutyronitrile was added and the constant temperature reaction was continued for 4 hours.

[0067] (2) After the constant temperature reaction is completed, the temperature in the reactor is lowered to 40° C., 2-amino-2-methyl-1-propanol is added to the reactor, stirred, the pH value is adjusted to 7-8, filtered, and the filtrate is collected to obtain an aqueous acrylate polymer dispersant.

[0068] The aqueous acrylate polymer dispersant obtained in step S2 was sampled, and the conversion rate was measured to be 99.7%. The effective ingredient content of the aqueous acrylate polymer dispersant obtained in step S2 was calculated according to the conversion rate. 21.52 kg of deionized water was added to the aqueous acrylate polymer dispersant obtained in step S2 to obtain an aqueous acrylate polymer dispersant product d with an effective ingredient content of 50±1%.

[0069] Example 5

[0070] This embodiment provides a method for preparing an aqueous acrylate polymer dispersant, which specifically comprises the following steps:

[0071] S1. Preparation of alkyl glycoside modified acrylate monomer:

[0072] (1) 50 kg of decyl glucoside was added to a reaction kettle, N2 was introduced, the mixture was ventilated three times, and the mixture was heated to 70±1°C. After the vacuum pump was turned on to remove water, 0.062 kg of hydroquinone and 0.62 kg of p-toluenesulfonic acid were added and stirred evenly to obtain a mixed system I.

[0073] (2) 13.85 kg of methacrylic acid was slowly added dropwise to the reaction kettle (i.e., acrylic acid was slowly added dropwise to the mixed system I), and the dripping was completed within 90 minutes. After the reaction was carried out at a constant temperature for 4 hours, samples were taken every 0.5 hours to test the acid value until the acid value remained unchanged. The material was discharged to obtain methacrylate decyl glucoside.

[0074] S2. Preparation of water-based acrylic polymer dispersant:

[0075] (1) 8 kg of decyl glucoside methacrylate, 4.5 kg of acrylic acid, 15 kg of methacrylic acid, 0.69 kg of azobisisobutyronitrile and 1.93 kg of thioglycolic acid were added to a stirring kettle in sequence and mixed evenly to obtain a mixed system II for standby use; at the same time, 10 kg of deionized water was added to the reaction kettle, heated to 60°C under a N2 atmosphere, and then the mixed system II in the stirring kettle was slowly added dropwise under stirring. The addition was completed within 120 minutes, and after the addition was completed, the reaction system was heated to 85°C, and the reaction was carried out at a constant temperature for 2 hours under stirring, and then 0.28 kg of azobisisobutyronitrile was added and the reaction was continued at a constant temperature for 4 hours.

[0076] (2) After the constant temperature reaction is completed, the temperature in the reactor is lowered to 40° C., 30 wt % NaOH solution is added to the reactor, stirred, the pH value is adjusted to 7-8, filtered, and the filtrate is collected to obtain an aqueous acrylate polymer dispersant.

[0077] The aqueous acrylate polymer dispersant obtained in step S2 was sampled, and the conversion rate was measured to be 99.4%. The effective ingredient content of the aqueous acrylate polymer dispersant obtained in step S2 was calculated according to the conversion rate. 7.85 kg of deionized water was added to the aqueous acrylate polymer dispersant obtained in step S2 to obtain an aqueous acrylate polymer dispersant product e with an effective ingredient content of 50±1%.

[0078] Experimental example

[0079] The aqueous acrylate polymer dispersant products a-e obtained in Examples 1-5 were applied to pigment and filler dispersion slurries and compared with Comparative Example 1 and Comparative Example 2. The formulas of the pigment and filler dispersion slurries are shown in Table 1, and the comparison results are shown in Table 2.

[0080] Table 1 Application of water-based acrylic polymer dispersants in the preparation of pigment and filler dispersions

[0081]

[0082] Note: Tego902W is a commercial defoamer, and the heat storage test adopts 50±1℃ condition, 7×24h; CabotREGAL99R is a commercial ink carbon black, CAS No.: 1333-86-4. Comparative Example 1 is a commercially available Disponer983 dispersant, and Comparative Example 2 is a commercially available B6012.

[0083] Table 2 Comparison of performance of water-based acrylic polymer dispersants used in pigment and filler dispersions

[0084]

[0085]

[0086] As shown in Table 2, the gloss of Formulas 1 to 5 is better than that of Formulas 7 and 8, and the stability of Formulas 1 to 5 is better than that of Formula 7. Moreover, Formulas 1 to 5, as well as Formulas 8 and 9, have no stratification or precipitation, which indicates that the aqueous acrylic polymer dispersant in the present invention has excellent gloss and stability under the same dosage conditions. When the dosage is reduced, such as when the dosage of Formulas 8 and 9 is reduced by 33.33%, they also show excellent performance, reflecting their high efficiency.

[0087] The above are only embodiments of the present invention. The invention is not limited to the fields involved in this implementation case. The common sense such as the known specific structures and characteristics in the scheme is not described in detail here. The ordinary technicians in the relevant field know all the common technical knowledge in the technical field to which the invention belongs before the application date or priority date, can obtain all the existing technologies in the field, and have the ability to apply the conventional experimental means before that date. The ordinary technicians in the relevant field can improve and implement this scheme in combination with their own abilities under the enlightenment given by this application. Some typical known structures or known methods should not become obstacles for ordinary technicians in the relevant field to implement this application. It should be pointed out that for those skilled in the art, without departing from the structure of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, which will not affect the effect of the implementation of the present invention and the practicality of the present invention. The protection scope required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to explain the content of the claims.

Claims

1. A method for preparing an aqueous acrylic polymer dispersant, characterized in that: The following steps are involved: S1. Preparation of alkyl glycoside modified acrylate monomer: (1) adding a catalyst and hydroquinone to an alkyl polyglycoside at 70-85° C. and stirring to obtain a mixed system I; (2) dropping acrylic acid monomer or acrylic acid ester monomer into the mixed system I, reacting at a constant temperature for 4 to 7 hours after the dropping is completed, taking samples to test the acid value until the acid value remains unchanged, thereby obtaining an alkyl glycoside-modified acrylic acid ester monomer; S2. Preparation of water-based acrylic polymer dispersant: (1) The initiator is divided into two parts, and the alkyl glycoside modified acrylate monomer obtained in step S1 is mixed with an acrylic monomer or an acrylate monomer, a part of the initiator, and a chain transfer aid, and stirred evenly to obtain a mixed system II, and the mixed system II is added dropwise to deionized water at 60 to 90° C. After the addition is completed, the temperature is raised to 80 to 100° C. and the reaction is carried out at a constant temperature for 2 hours, and another part of the initiator is added, and the reaction is continued at a constant temperature for more than 4 hours; (2) After the isothermal reaction is completed, the temperature is lowered to 40° C., and the pH value is adjusted to 7-8 using a pH adjuster to obtain an aqueous acrylate polymer dispersant.

2. The preparation method according to claim 1, characterized in that: The structural formula of the alkyl glycoside used in step S1 is shown in formula (I): Wherein, R1 is a C1-C18 alkane or a derivative thereof.

3. The preparation method according to claim 2, characterized in that: The acrylic monomer used in step S1 is one or both of methacrylic acid and acrylic acid; the structure of the alkyl glycoside modified acrylate monomer obtained in step S1 is shown in formula (II): Wherein, R2 is H or CH3.

4. The preparation method according to claim 1, characterized in that: In step S1, the acrylic monomer or acrylic ester monomer, alkyl glycoside, hydroquinone and catalyst are respectively 14-26 parts, 73-86 parts, 0.05-0.1 parts and 0.2-2.0 parts by weight.

5. The preparation method according to claim 1, characterized in that: The catalyst used in step S1 is one or both of p-toluenesulfonic acid and dodecylbenzenesulfonic acid.

6. The preparation method according to claim 1, characterized in that: The acrylic monomer used in step S2 is one or both of acrylic acid and methacrylic acid; the acrylic ester monomer used in step S2 is one or more of methyl acrylate, methacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, butyl acrylate, butyl methacrylate, glycidyl methacrylate and lauryl acrylate; And / or, the initiator used in step S2 is one of ammonium sulfate, azobisisoheptanitrile and azobisisobutyronitrile; And / or, the chain transfer aid used in step S2 is one or two of dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid and isopropanol.

7. The preparation method according to claim 1, characterized in that: The pH adjuster used in step S2 is adjusted to one or more of ammonia water, monoethanolamine, diethanolamine, sodium hydroxide, potassium hydroxide, triethanolamine, N,N-dimethylethanolamine and 2-amino-2-methyl-1-propanol.

8. The preparation method according to claim 1, characterized in that: In step S2, the amount of acrylic acid monomer or acrylic ester monomer used is 55-90% of the total mass of the reactants in step S2; and / or, in step S2, the amount of the alkyl glycoside-modified acrylate monomer used is 10 to 60% of the total mass of the reactants in step S2; and / or, in step S2, the amount of the initiator used is 1.0 to 6.0% of the total mass of the reactants in step S2; And / or, in step S2, the amount of the chain transfer aid is 0.5-10.0% of the total mass of the reactants in step S2.

9. An aqueous acrylic polymer dispersant, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the aqueous acrylate polymer dispersant according to claim 9 in aqueous coating dispersants and ink dispersants.