A thermally conductive filler with modified lignin surface and its preparation method and application

By wrapping lignin on conductive and thermally conductive fillers, the problems of complex preparation process, high cost and poor insulation performance of thermally conductive composite materials are solved, and the thermal conductivity and electrical insulation properties are improved. The process is simple, low-cost and takes advantage of green environmental protection. of lignin material.

CN116554713BActive Publication Date: 2024-10-22GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310516520.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-10-22
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

Existing thermally conductive composite materials have complex preparation processes, high costs, and poor electrical insulation properties, making them difficult to apply in harsh environments such as electronic packaging.

Method used

Lignin is used as a surface modifier, which is evenly dispersed with electrically conductive and thermally conductive fillers, and wrapped on the surface of electrically conductive and thermally conductive fillers through an anti-solvent method to reduce the electrical conductivity of the thermally conductive fillers and improve the thermal conductivity and insulation properties of the composite material.

Benefits of technology

It achieves good thermal conductivity and improved electrical insulation performance of thermally conductive composite materials. The process is simple and low-cost, and the cheap and easily available green environmentally friendly material lignin is used to promote its high-value utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116554713B_ABST
    Figure CN116554713B_ABST
Patent Text Reader

Abstract

The present invention provides a lignin surface-modified thermally conductive filler and a preparation method and application thereof. The present invention encapsulates an electrically conductive thermally conductive filler in lignin by an anti-solvent method to prepare a surface-modified thermally conductive filler. The modified thermally conductive filler is then mixed with an epoxy resin and cured by hot pressing to obtain a thermally conductive insulating composite material. The present invention uses lignin as a surface modifier, utilizes the electrical insulation of the lignin coating layer to effectively enhance the electrical insulation performance of the composite material, and synthesizes a composite material with good thermal conductivity and electrical insulation, and the thermal conductivity coefficient is 0.83-13.42 W·m ‑1 ·K ‑1 , volume resistivity up to 10 9 Ω·cm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermally conductive composite materials and relates to a thermally conductive filler with modified lignin surface and a preparation method and application thereof. Background Art

[0002] With the rapid development of technologies such as electronic packaging and 5G communications, modern electronic devices are gradually tending towards miniaturization and integration. The power density of electronic devices is growing rapidly, and the heat generated by the equipment working for a long time accumulates, causing the equipment to be in an ultra-high temperature state, seriously affecting the performance and service life of the equipment. Therefore, achieving effective thermal management of electronic devices has become an urgent problem to be solved, and the development of thermally conductive polymer composite materials for heat dissipation of equipment will be a feasible method.

[0003] Polymer materials are widely used in the preparation of thermally conductive composite materials due to their good chemical stability, easy processing and low cost. Traditional thermally conductive polymer composite materials mainly add thermally conductive fillers with high thermal conductivity to the polymer matrix to improve the thermal conductivity of the entire composite material. These high thermal conductivity thermally conductive fillers are usually some metal particles with electrical conductivity (such as silver nanowires, copper nanowires, aluminum powder, etc.) and carbon-based materials (such as graphene nanosheets, carbon nanotubes, expanded graphite, etc.). Although the introduction of these thermally conductive fillers can improve the thermal conductivity of the composite material, it will also reduce the electrical insulation ability of the material, which is not conducive to the application of composite materials in harsh environments such as electronic packaging and integrated circuits that require electrical insulation.

[0004] At present, the method for preparing thermally conductive insulating composite materials is mainly to modify the surface of thermally conductive fillers. For example, patent application CN201910015535.9 loads nano-γ-alumina on carbon nanotubes through an electrostatic self-assembly process, and then adds the above-mentioned modified filler to silicone rubber to prepare a thermal interface elastomer composite material with good thermal conductivity and electrical insulation capabilities. Patent application CN202210817058.X mixes insulating thermally conductive fillers (such as boron nitride, aluminum nitride, etc.) with conductive thermally conductive fillers (such as graphene, nanographite sheets, etc.) through processes such as melt blending and cooling granulation to obtain modified thermally conductive fillers, and finally combines with thermoplastic materials to prepare high thermal conductivity insulating composite materials. However, the above-mentioned modification method has high equipment requirements, complex preparation process, and high cost. Summary of the invention

[0005] The purpose of the present invention is to solve the problems existing in the prior art of preparing thermally conductive composite materials, such as complex preparation process, high cost, poor insulation performance, etc., thereby providing a method for preparing a thermally conductive composite material by modifying a thermally conductive filler with lignin, which can significantly improve the electrical insulation performance of the thermally conductive composite material and effectively improve its thermal conductivity.

[0006] To achieve the above object, the present invention is achieved by the following means:

[0007] The first aspect of the present invention provides a method for preparing a lignin surface-modified thermally conductive filler, comprising the following steps:

[0008] (1) placing a hydrogen bond donor compound and a hydrogen bond acceptor compound in a container, and stirring at room temperature until the solution becomes uniform and transparent, thereby preparing a DES solvent;

[0009] (2) Purifying a lignin raw material to obtain a purified lignin raw material, adding the purified lignin raw material to the DES solvent obtained in step (1), stirring at room temperature until the lignin raw material is completely dissolved, and then adding a conductive and thermally conductive filler to uniformly disperse the lignin raw material to obtain a mixed system;

[0010] (3) adding the mixed system obtained in step (2) dropwise into ultrapure water at room temperature while stirring continuously, then filtering and washing the precipitate with ultrapure water, and finally drying to obtain a lignin surface-modified thermal conductive filler.

[0011] Preferably, the hydrogen bond donor compound in step (1) is selected from one or more of phenol, resorcinol, hydroquinone or ethylene glycol; and the hydrogen bond acceptor compound is one or more of maleic anhydride, glutaric anhydride and citraconic anhydride.

[0012] Preferably, in step (1), the mass ratio of the hydrogen bond donor compound to the hydrogen bond acceptor compound is 0.5-2.5.

[0013] Preferably, the stirring time in step (1) is 1-2 h.

[0014] Preferably, the lignin raw material in step (2) is selected from one or more of alkali lignin, enzymatically hydrolyzed lignin or sodium lignin sulfonate.

[0015] Preferably, in step (2), the mass volume ratio of the purified lignin raw material to the DES solvent is 1:1-5.

[0016] It should be understood that, unless otherwise specified, the "mass volume ratio" in the context of the present invention should be understood in a conventional manner in the art, that is, the ratio of the mass of the solid substance (in g) to the liquid volume (in mL). For example, when the "mass volume ratio of the purified lignin raw material to the DES solvent is 1:2", if the added amount of the purified lignin raw material is 1 g, the added amount of the DES solvent is 2 mL.

[0017] Preferably, the purification in step (2) specifically comprises the following steps:

[0018] (a) adding a lignin raw material into ultrapure water, and then adding an alkaline solution to adjust the pH of the solution so that the lignin raw material is completely dissolved;

[0019] (b) filtering to remove the filter residue and then adding an acidic solution to further adjust the pH of the solution;

[0020] (c) performing vacuum filtration under constant temperature conditions, discarding the filtrate, collecting the precipitated lignin raw material, washing it repeatedly with ultrapure water, and freeze-drying it to obtain the purified lignin raw material.

[0021] Preferably, in step (a), the mass ratio of the lignin raw material to ultrapure water is 1:5-20.

[0022] Preferably, the alkaline solution in step (a) is selected from a NaOH solution; more preferably, the alkaline solution is selected from a NaOH solution with a concentration of 10-30 wt%.

[0023] Preferably, in step (a), an alkaline solution is added to adjust the pH of the solution to 12-13.5.

[0024] Preferably, the acidic solution in step (b) is selected from HCl solution; more preferably, the acidic solution is selected from HCl solution with a concentration of 10-20 vol%.

[0025] Preferably, an acidic solution is added in step (b) to further adjust the pH of the solution to 1.5-3.

[0026] Preferably, the constant temperature in step (c) is 60-70°C.

[0027] Preferably, in step (c), ultrapure water is used for repeated washing until the pH value of the washing filtrate is 6.8-7.2.

[0028] Preferably, the freeze-drying time in step (c) is 36-72 hours.

[0029] Preferably, the conductive and thermally conductive filler in step (2) is selected from one or more of aluminum powder (Al), copper nanowires (CuNWs), silver nanowires (AgNWs), natural graphite (NG), expanded graphite (EG), graphene nanosheets (GNPs), carbon nanotubes (CNTs) or MXene.

[0030] Preferably, the average size of the aluminum powder is 25 μm, the average size of the copper nanowires is 40 μm, the average size of the silver nanowires is 20 μm, the average size of the natural graphite is 100 μm, the average size of the expanded graphite is 150 μm, the average size of the graphene nanosheets is 3 μm, the average size of the carbon nanotubes is 6 μm, and the average size of the MXene is 150 nm.

[0031] Preferably, in step (2), the mass ratio of the purified lignin raw material to the electrically conductive and thermally conductive filler is 1:2-4.

[0032] Preferably, the volume ratio of the mixed system to ultrapure water in step (3) is 1:200-300.

[0033] Preferably, the washing is performed 2-3 times in step (3).

[0034] Preferably, the drying in step (3) is carried out under vacuum conditions, the drying temperature is 40-55° C., and the drying time is 24-48 h.

[0035] The second aspect of the present invention provides a lignin surface-modified thermally conductive filler prepared according to the above preparation method.

[0036] A third aspect of the present invention provides a thermally conductive insulating composite material, comprising an epoxy resin, a curing agent, and a thermally conductive filler with a surface modified with lignin prepared according to the above method.

[0037] Preferably, the epoxy resin is selected from one or more of E44, E51, and E54.

[0038] Preferably, the curing agent is selected from one or more of 4,4'-diaminodiphenylmethane (DDM) and 4,4'-diaminodicyclohexylmethane (PACM).

[0039] Preferably, the amount of the lignin surface modified thermal conductive filler is 10-50% of the total mass of the lignin surface modified thermal conductive filler, the curing agent and the epoxy resin.

[0040] Preferably, the mass ratio of the epoxy resin to the curing agent is 3.0-5.0.

[0041] A fourth aspect of the present invention provides a method for preparing the above-mentioned thermally conductive insulating composite material, comprising the following steps:

[0042] After the lignin surface-modified thermal conductive filler and epoxy resin are mixed and stirred evenly, a curing agent is added and stirred to obtain a uniform mixed liquid, and then the mixed liquid is placed in a mold and subjected to three-stage hot pressing curing.

[0043] Preferably, the curing agent is added and stirred for 5-20 minutes.

[0044] Preferably, the conditions for the three-stage hot pressing curing are as follows: the temperature of the first stage is 80-100°C and the time is 1-3h; the temperature of the second stage is 110-130°C and the time is 1-3h; the temperature of the third stage is 140-160°C and the time is 1-3h.

[0045] The lignin surface modified thermal conductive filler involved in the present invention first purifies the industrial lignin raw material, then selects a suitable compound with hydrogen bond donors and acceptors according to the properties of the lignin used to prepare a DES solvent and dissolve the lignin, and then the conductive thermal conductive filler (such as Al, CuNWs, AgNWs, NG, EG, GNP, CNTs or MXene, etc.) is uniformly dispersed in the above-mentioned DES system, and then the above-mentioned mixture is added drop by drop into excess ultrapure water by an anti-solvent method, and the lignin surface modified thermal conductive filler is obtained by filtration and drying. Compared with other modification methods, the present invention provides a simple and low-cost surface insulation modification method, which wraps lignin on the surface of the conductive thermal conductive filler, reduces the electrical conductivity of the filler, and improves the thermal conductivity and electrical insulation of the polymer composite material. Lignin is cheap and easy to obtain, green and environmentally friendly, and using it as a surface modifier further promotes the high-value utilization of lignin.

[0046] Compared with the existing technology, the present invention has the following beneficial effects:

[0047] (1) The present invention creatively uses lignin as a surface modifier and uses an anti-solvent method to wrap lignin on a conductive and thermally conductive filler to reduce the conductivity of the thermally conductive filler. The prepared composite material has good thermal conductivity and electrical insulation properties.

[0048] (2) The preparation method of the lignin surface modified thermal conductive filler described in the present invention has mild reaction conditions and a simple process; the surface modifier used is industrial lignin, which has a wide source, low cost, and is green and environmentally friendly. Using it as a surface insulation modifier can achieve high-value utilization of lignin. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 The scanning electron microscope images and mapping images of the AL@Al thermally conductive filler prepared in Example 1 and the pure aluminum powder thermally conductive filler in Comparative Example 1.

[0050] Figure 2 This is the X-ray diffraction pattern of the AL@Al thermally conductive filler prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0052] Unless otherwise defined, all technical terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The technical terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or can be prepared by existing methods.

[0053] Example 1

[0054] A lignin surface-modified thermal conductive filler, the preparation method of which specifically comprises the following steps:

[0055] (1) 23.528 g of phenol and 24.514 g of maleic anhydride were placed in a 500 mL covered wide-mouth bottle and stirred at room temperature for 1 h until the solution became homogeneous and transparent, thereby obtaining a DES solvent of the phenol-maleic anhydride system.

[0056] (2) 10 g of alkali lignin (AL) was placed in a 500 mL beaker, 100 mL of ultrapure water was added, and then a 10 wt % NaOH solution was added to adjust the pH to 12 so that AL was completely dissolved. After filtering out the residue, a 10 vol % HCl solution was added to adjust the pH value of the system to 1.5. The temperature was maintained at 60° C., vacuum filtered, and the filtrate was discarded. The precipitated AL was collected and repeatedly washed with ultrapure water until the pH value of the washing filtrate was 6.8, and freeze-dried for 36 h to obtain purified AL. 2 g of purified AL was added to 5 mL of the DES solvent obtained in step (1), stirred at room temperature until AL was completely dissolved, and then 4 g of aluminum powder (Al, average size of 25 μm) was added to disperse it evenly to obtain a mixed system.

[0057] (3) The mixed system obtained in step (2) was added dropwise into 1000 mL of ultrapure water at room temperature with continuous stirring, and then filtered and the precipitate was washed with ultrapure water for 2-3 times, and finally vacuum dried at 40° C. for 24 h to obtain a modified thermal conductive filler of Al encapsulated in Al, which was named AL@Al.

[0058] Furthermore, the modified thermally conductive filler of Al wrapped in Al prepared by the above method is used to prepare a thermally conductive composite material, which specifically includes the following steps:

[0059] 0.4 g AL@Al and 2.956 g E44 were mixed and stirred, 0.644 g DDM was added and stirred for 5 min to obtain a uniform mixed solution, and then the mixed solution was placed in a 25×25×5 mm mold and hot-pressed and cured at 80, 110 and 140 °C for 1 h to obtain a thermally conductive composite material, named AL@Al / E44 / DDM.

[0060] Example 2

[0061] A lignin surface-modified thermal conductive filler, the preparation method of which specifically comprises the following steps:

[0062] (1) 23.528 g of resorcinol and 49.029 g of citraconic anhydride were placed in a 500 mL covered wide-mouth bottle and stirred at room temperature for 2 h until the solution became uniform and transparent, thereby obtaining a DES solvent of the resorcinol-citraconic anhydride system.

[0063] (2) 10 g of enzymatically hydrolyzed lignin (EHL) was placed in a 500 mL beaker, 100 mL of ultrapure water was added, and then a 20 wt % NaOH solution was added to adjust the pH to 12.5 so that the EHL was completely dissolved. After filtering out the residue, a 15 vol % HCl solution was added to adjust the pH value of the system to 2, and the temperature was maintained at 65° C. The filtrate was vacuum filtered and the filtrate was discarded. The precipitated AL was collected and repeatedly washed with ultrapure water until the pH value of the washing filtrate was 7.0, and freeze-dried for 72 h to obtain purified EHL; 2 g of purified EHL was added to 5 mL of the DES solvent obtained in step (1), stirred at room temperature until the EHL was completely dissolved, and then 6 g of natural graphite (NG, with an average size of 100 μm) was added to disperse it evenly to obtain a mixed system.

[0064] (3) The mixed system obtained in step (2) was added dropwise into 1200 mL of ultrapure water at room temperature with continuous stirring, and then filtered and the precipitate was washed with ultrapure water for 2-3 times, and finally vacuum dried at 45°C for 24 h to obtain a modified thermal conductive filler of EHL-encapsulated NG, which was named EHL@NG.

[0065] Furthermore, the preparation of a thermally conductive composite material using the modified thermally conductive filler of NG wrapped in EHL prepared by the above method specifically includes the following steps:

[0066] 0.8 g EHL@NG and 2.524 g E51 were mixed and stirred, 0.676 g PACM was added and stirred for 10 min to obtain a uniform mixture, and then the mixture was placed in a 25×25×5 mm mold and hot-pressed and cured at 90, 120 and 150 °C for 2 h to obtain a thermally conductive composite material, named EHL@NG / E51 / PACM.

[0067] Example 3

[0068] A lignin surface-modified thermal conductive filler, the preparation method of which specifically comprises the following steps:

[0069] (1) 47.056 g of hydroquinone and 49.029 g of glutaric anhydride were placed in a 500 mL wide-mouth bottle with a cap and stirred at room temperature for 2 h until the solution became uniform and transparent, thereby obtaining a DES solvent of the hydroquinone-glutaric anhydride system.

[0070] (2) 10 g of sodium lignin sulfonate (LS) was placed in a 500 mL beaker, 100 mL of ultrapure water was added, and then a 30 wt % NaOH solution was added to adjust the pH to 13.5 so that the LS was completely dissolved. After filtering out the residue, a 20 vol % HCl solution was added to adjust the pH value of the system to 2, and the temperature was maintained at 70° C. The filtrate was removed by vacuum filtration, and the filtrate was discarded. The precipitated LS was collected and repeatedly washed with ultrapure water until the pH value of the washing filtrate was 7.2, and freeze-dried for 45 h to obtain purified LS; 2 g of the purified LS was added to 5 mL of the DES solvent obtained in step (1), and stirred at room temperature until the LS was completely dissolved, and then 6 g of expanded graphite (EG, with an average size of 150 μm) was added to disperse it evenly to obtain a mixed system.

[0071] (3) The mixed system obtained in step (2) was added dropwise into 1500 mL of ultrapure water at room temperature with continuous stirring, and then filtered and the precipitate was washed with ultrapure water for 2-3 times, and finally vacuum dried at 55° C. for 48 h to obtain a modified thermal conductive filler of EG encapsulated by LS, which was named LS@EG.

[0072] Furthermore, the modified thermally conductive filler of EG encapsulated by LS prepared by the above method is used to prepare a thermally conductive composite material, which specifically includes the following steps:

[0073] 1.2 g LS@EG and 2.209 g E54 were mixed and stirred, 0.591 g DDM was added and stirred for 15 min to obtain a uniform mixture, and then the mixture was placed in a 25×25×5 mm mold and hot-pressed and cured at 100, 130 and 160 °C for 3 h to obtain a thermally conductive composite material, named LS@EG / E54 / DDM.

[0074] Example 4

[0075] A lignin surface-modified thermally conductive filler, the preparation method of which specifically comprises the following steps:

[0076] (1) 47.056 g of butanediol and 24.514 g of maleic anhydride were placed in a 500 mL covered wide-mouth bottle and stirred at room temperature for 1.5 h until the solution became uniform and transparent, thereby obtaining a DES solvent of a butanediol-maleic anhydride system.

[0077] (2) 10 g of alkali lignin (AL) was placed in a 500 mL beaker, 100 mL of ultrapure water was added, and then a 10 wt % NaOH solution was added to adjust the pH to 12 so that AL was completely dissolved. After filtering out the residue, a 10 vol % HCl solution was added to adjust the pH value of the system to 1.5. The temperature was maintained at 60° C., vacuum filtered, and the filtrate was discarded. The precipitated AL was collected and repeatedly washed with ultrapure water until the pH value of the washing filtrate was 6.8. The precipitated AL was freeze-dried for 36 h to obtain purified AL. 2 g of purified AL was added to 5 mL of the DES solvent obtained in step (1), stirred at room temperature until AL was completely dissolved, and then 8 g of MXene (average size of 150 nm) was added to disperse it evenly to obtain a mixed system.

[0078] (3) The mixed system obtained in step (2) was added dropwise into 1000 mL of ultrapure water at room temperature with continuous stirring, and then filtered and the precipitate was washed with ultrapure water for 2-3 times, and finally vacuum dried at 40 °C for 24 h to obtain a modified thermal conductive filler of AL-wrapped MXene, which was named AL@MXene.

[0079] Furthermore, the modified thermally conductive filler of MXene wrapped in AL prepared by the above method is used to prepare a thermally conductive composite material, which specifically includes the following steps:

[0080] 1.6 g AL@MXene and 1.950 g E44 were mixed and stirred, 0.450 g PACM was added and stirred for 20 min to obtain a uniform mixture. The mixture was then placed in a 25×25×5 mm mold and hot-pressed and cured at 80, 120 and 150 °C for 2 h to obtain a thermally conductive composite material, named AL@MXene / E44 / PACM.

[0081] Example 5

[0082] A lignin surface-modified thermally conductive filler, the preparation method of which specifically comprises the following steps:

[0083] (1) 23.528 g of hydroquinone and 49.029 g of maleic anhydride were placed in a 500 mL covered wide-mouth bottle and stirred at room temperature for 1 h until the solution became uniform and transparent, thereby obtaining a DES solvent of the hydroquinone-maleic anhydride system.

[0084] (2) 10 g of enzymatically hydrolyzed lignin (EHL) was placed in a 500 mL beaker, 100 mL of ultrapure water was added, and then a 20 wt % NaOH solution was added to adjust the pH to 13.5 so that the EHL was completely dissolved. After filtering out the residue, a 15 vol % HCl solution was added to adjust the pH value of the system to 3, and the temperature was maintained at 65° C. The filtrate was vacuum filtered and the filtrate was discarded. The precipitated AL was collected and repeatedly washed with ultrapure water until the pH value of the washing filtrate was 7.2, and freeze-dried for 36 h to obtain purified EHL; 2 g of purified EHL was added to 5 mL of the DES solvent obtained in step (1), stirred at room temperature until the EHL was completely dissolved, and then 6 g of graphene nanosheets (GNP, with an average size of 3 μm) were added to disperse it evenly to obtain a mixed system.

[0085] (3) The mixed system obtained in step (2) was added dropwise into 1500 mL of ultrapure water at room temperature with continuous stirring, and then filtered and the precipitate was washed with ultrapure water for 2-3 times, and finally vacuum dried at 55 °C for 48 h to obtain the modified thermal conductive filler of EHL-encapsulated GNP, which was named EHL@GNP.

[0086] Furthermore, the preparation of a thermally conductive composite material using the modified thermally conductive filler of EHL encapsulated GNP prepared by the above method specifically includes the following steps:

[0087] 2 g of EHL@GNP was mixed with 1.642 g of E44, and 0.358 g of DDM was added and stirred for 10 min to obtain a uniform mixture. The mixture was then placed in a 25×25×5 mm mold and hot-pressed and cured at 100, 120 and 160 °C for 2 h to obtain a thermally conductive composite material named EHL@GNP / E44 / DDM.

[0088] Example 6

[0089] A lignin surface-modified thermally conductive filler, the preparation method of which specifically comprises the following steps:

[0090] (1) 47.056 g of resorcinol and 24.514 g of glutaric anhydride were placed in a 500 mL covered wide-mouth bottle and stirred at room temperature for 1 h until the solution became uniform and transparent, thereby obtaining a DES solvent of the resorcinol-glutaric anhydride system.

[0091] (2) 10 g of sodium lignin sulfonate (LS) was placed in a 500 mL beaker, 100 mL of ultrapure water was added, and then a 10 wt % NaOH solution was added to adjust the pH to 12 so that the LS was completely dissolved. After filtering out the residue, a 10 vol % HCl solution was added to adjust the pH value of the system to 1.5, and the temperature was maintained at 65° C. The filtrate was removed by vacuum filtration, and the filtrate was discarded. The precipitated LS was collected and repeatedly washed with ultrapure water until the pH value of the washing filtrate was 6.8, and freeze-dried for 36 h to obtain purified LS; 2 g of purified LS was added to 5 mL of the DES solvent obtained in step (1), and stirred at room temperature until the LS was completely dissolved, and then 8 g of carbon nanotubes (CNTs, with an average size of 6 μm) were added to disperse them evenly to obtain a mixed system.

[0092] (3) The mixed system obtained in step (2) was added dropwise into 1300 mL of ultrapure water at room temperature with continuous stirring, and then filtered and the precipitate was washed with ultrapure water for 2-3 times, and finally vacuum dried at 50° C. for 36 h to obtain a modified thermal conductive filler of LS-wrapped CNTs, which was named LS@CNTs.

[0093] Furthermore, the modified thermal conductive filler of LS encapsulated CNTs prepared by the above method is used to prepare a thermal conductive composite material, which specifically includes the following steps:

[0094] 2 g LS@CNTs and 1.597 g E51 were mixed and stirred, 0.403 g DDM was added and stirred for 8 min to obtain a uniform mixed solution, and then the mixed solution was placed in a 25×25×5 mm mold and hot-pressed and cured at 100, 130 and 160 °C for 3 h to obtain a thermally conductive composite material, named LS@CNTs / E51 / DDM.

[0095] Comparative Example 1

[0096] The preparation of the thermally conductive composite material using pure aluminum powder as a thermally conductive filler specifically includes the following steps:

[0097] 0.4 g of pure aluminum powder (average size of 25 μm) was mixed with 2.956 g of E44, 0.644 g of DDM was added and stirred for 5 min to obtain a uniform mixed solution, and then the mixed solution was placed in a 25×25×5 mm mold and hot-pressed and cured at 80, 110 and 140°C for 1 h to obtain a thermally conductive composite material, named Al / E44 / DDM.

[0098] Comparative Example 2

[0099] The preparation of a thermally conductive composite material using pure natural graphite as a thermally conductive filler specifically includes the following steps:

[0100] 0.8 g of pure natural graphite (average size of 100 μm) was mixed with 2.524 g of E51, 0.676 g of PACM was added and stirred for 10 min to obtain a uniform mixed solution, and then the mixed solution was placed in a 25×25×5 mm mold and hot-pressed and cured at 90, 120 and 150°C for 2 h to obtain a thermally conductive composite material, named NG / E51 / PACM.

[0101] Comparative Example 3

[0102] The preparation of a thermally conductive composite material using graphene nanosheets as a thermally conductive filler specifically includes the following steps:

[0103] 2 g of graphene nanosheets (average size of 3 μm) were mixed with 1.642 g of E44, 0.358 g of DDM was added and stirred for 10 min to obtain a uniform mixture, and then the mixture was placed in a 25×25×5 mm mold and hot-pressed and cured at 100, 120 and 160°C for 2 h to obtain a thermally conductive composite material, named GNP / E44 / DDM.

[0104] Verification Example 1

[0105] The modified thermal conductive filler AL@Al coated with Al prepared in Example 1 and the pure aluminum powder thermal conductive filler in Comparative Example 1 were respectively taken and their morphologies were characterized by scanning electron microscopy. The results are as follows: Figure 1 As shown. Figure 1 (a)-(c) are scanning electron microscope images of pure aluminum powder thermal conductive filler in comparative example 1. Figure 1 (d)-(f) are scanning electron microscope images of AL@Al thermal conductive filler in Example 1. Figure 1 (g) and Figure 1 (h) are mapping diagrams of the thermal conductive fillers of comparative example 1 and embodiment 1. Subsequently, the AL@Al thermal conductive filler prepared in embodiment 1 was tested using an X-ray diffractometer. The results are as follows: Figure 2 shown.

[0106] Furthermore, the thermal conductive composite materials prepared in Examples 1-6 and Comparative Examples 1-3 were respectively tested for thermal conductivity and insulation properties. The test results are shown in Table 1 below.

[0107] Table 1 Thermal conductivity and volume resistivity of thermally conductive composite materials prepared in Examples 1-6

[0108]

[0109]

[0110] The results show that the thermally conductive composite materials Al / E44 / DDM, NG / E51 / PACM and GNP / E44 / DDM prepared in Comparative Examples 1-3 respectively use traditional aluminum powder, natural graphite and graphene nanosheets as thermally conductive fillers. Due to the poor interface compatibility between the thermally conductive filler and the resin matrix, there is a large interface thermal resistance between the thermally conductive filler and the resin matrix, resulting in relatively poor thermal conductivity of the entire composite material. The thermal conductivity coefficients of the composite materials prepared in Comparative Examples 1-2 are only 0.47 and 0.58 W·m -1 ·K -1 The thermal conductivity of the composite material of Comparative Example 3 reaches 6.88 W·m -1 ·K -1 , but it is still much lower than the composite material prepared at the same filler loading in Example 5. In addition, the volume resistivity of the composite materials prepared in Comparative Examples 1-3 is only 10 5 Ω·cm, that is, it has no electrical insulation. The thermally conductive composite material prepared according to the embodiment of the present invention, by wrapping lignin on the conductive and thermally conductive filler, can promote the interface compatibility of the thermally conductive filler and the resin matrix, effectively reduce the interface thermal resistance between the filler and the matrix, significantly improve the thermal conductivity of the thermally conductive composite material, and at the same time reduce the electrical conductivity of the thermally conductive filler, so that the composite material has excellent electrical insulation performance.

[0111] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.

Claims

1. A method for preparing a thermally conductive filler with modified lignin surface, characterized in that: The steps include: (1) placing a hydrogen bond donor compound and a hydrogen bond acceptor compound in a container, stirring at room temperature until the solution becomes uniform and transparent, thereby preparing a low eutectic solvent; the hydrogen bond donor compound is selected from one or more of phenol, resorcinol, hydroquinone or ethylene glycol; the hydrogen bond acceptor compound is one or more of maleic anhydride, glutaric anhydride, and citraconic anhydride; (2) Purifying a lignin raw material to obtain a purified lignin raw material, adding the purified lignin raw material to the DES solvent obtained in step (1), stirring at room temperature until the lignin raw material is completely dissolved, and then adding a conductive and thermally conductive filler to disperse it evenly to obtain a mixed system; the lignin raw material is selected from one or more of alkali lignin, enzymatically hydrolyzed lignin or sodium lignin sulfonate; the conductive and thermally conductive filler is selected from one or more of aluminum powder, copper nanowires, silver nanowires, natural graphite, expanded graphite, graphene nanosheets, carbon nanotubes or MXene; The purification specifically comprises the following steps: (a) adding lignin raw material into ultrapure water, and then adding alkaline solution to adjust the pH of the solution so that the lignin raw material is completely dissolved; (b) filtering to remove the residue and then adding an acidic solution to further adjust the pH of the solution; (c) performing vacuum filtration under constant temperature conditions, discarding the filtrate, collecting the precipitated lignin raw material and repeatedly washing it with ultrapure water, and freeze-drying it to obtain the purified lignin raw material; (3) Adding the mixed system obtained in step (2) dropwise into ultrapure water at room temperature while stirring continuously, then filtering and washing the precipitate with ultrapure water, and finally drying to obtain a lignin surface-modified thermal conductive filler.

2. The thermally conductive filler with surface modified lignin prepared according to the preparation method of claim 1.

3. A thermally conductive insulating composite material, characterized in that: The invention comprises epoxy resin, curing agent and a lignin surface-modified thermal conductive filler prepared according to the preparation method of claim 1.

4. The thermally conductive insulating composite material according to claim 3, characterized in that: The epoxy resin is selected from one or more of E44, E51, and E54.

5. The thermally conductive insulating composite material according to claim 3, characterized in that: The curing agent is selected from one or more of 4,4'-diaminodiphenylmethane and 4,4'-diaminodicyclohexylmethane.

6. The method for preparing the thermally conductive insulating composite material according to any one of claims 3 to 5, characterized in that: The method comprises the following steps: mixing and stirring the lignin surface-modified thermal conductive filler and epoxy resin evenly, adding a curing agent and stirring to obtain a uniform mixed liquid, and then placing the mixed liquid in a mold and performing three-stage hot pressing curing to obtain the obtained product.