A kind of water-based coating for greenhouse ground film paper and preparation method thereof

Through the use of water-based coatings for greenhouse plastic film paper, the problems of low light transmittance, insufficient strength, poor water resistance and too fast biodegradation of greenhouse plastic film paper are solved, and efficient and environmentally friendly coating technology is achieved, which improves the paper Physical performance and environmental friendliness.

CN116556100BActive Publication Date: 2024-11-19BEIJING FORESTRY UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310705410.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-14
Publication Date
2024-11-19
Estimated Expiration
2043-06-14

AI Technical Summary

Technical Problem

The existing greenhouse mulberry paper has shortcomings in terms of low light transmittance, insufficient strength, poor water resistance and too fast biodegradation. It has complex production processes and high cost, making it difficult to effectively utilize resources, resulting in environmental pollution.

Method used

Use water-based coatings for low-quantity greenhouse mulch paper, including black pulp, styrene butadiene latex or water-based polyurethane adhesives, PVDC and EAA waterproof and moisture-repellent, carboxymethyl cellulose and modified chitosan dry strength agent, polyether defoaming The agent and sodium hypophosphite hydrophobic agent are prepared by stirring a high-speed disperser. The solid content is 20%-30%, and the coating amount is 4g/m2-6g/m2 to improve the opacity and physical strength of the paper.

Benefits of technology

It significantly improves the opacity, moisture resistance and water resistance of greenhouse plastic film paper, reduces water vapor transmission and light transmittance, extends biodegradation time, reduces environmental pollution, reduces production costs, and improves paper resistance Break index and wet intensity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004285795940000061
    Figure BDA0004285795940000061
  • Figure BDA0004285795940000071
    Figure BDA0004285795940000071
  • Figure HDA0004285795950000011
    Figure HDA0004285795950000011
Patent Text Reader

Abstract

The present invention relates to the technical field of papermaking coatings and greenhouse ground film paper, and specifically to a low-quantity special coating for greenhouse ground film paper and a preparation method thereof. The coating comprises the following raw materials by weight: 20 to 30 parts of black color paste; 25 to 35 parts of styrene-butadiene latex and water-based polyurethane adhesive, 5 to 8 parts of PVDC and EAA waterproof and moisture-blocking agents, 1 to 2 parts of carboxymethyl cellulose and modified chitosan dry strength agents, 0.1 to 0.5 parts of polyether defoamers, 0.5 to 1 parts of sodium hexametaphosphate dispersants, 1 to 2 parts of sodium hypophosphite hydrophobic agents, and 100 parts of distilled water. The coating of the present invention has a simple preparation process, low production cost, is soluble in water, has controllable viscosity, and is suitable for producing greenhouse ground film paper by coating or sizing processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of papermaking coatings and greenhouse mulch paper, and in particular to a low-quantity special coating for greenhouse mulch paper and a preparation method thereof, which is mainly used for surface coating of greenhouse mulch paper. Background Art

[0002] Paper coating is an engineering material that is coated on the surface of paper and can form a firmly attached film. Paper coating is an important component of coated paper. It is a mixed system composed of pigment dispersion, adhesive and other additives. It can play a good protective role on paper and give paper certain special functions such as moisture resistance, water resistance and antibacterial, and can improve the physical strength of paper to a certain extent.

[0003] Greenhouse mulch films are widely used and play an important role in increasing crop yields and improving agricultural production efficiency. However, current mulch films are mainly made of plastics such as PE, which are difficult to degrade. The development of biodegradable and environmentally friendly paper-based materials has important practical significance for alleviating plastic pollution in my country. At present, the coating method for producing greenhouse mulch paper has become a research hotspot because of its simple preparation process and ability to effectively reduce environmental pollution. However, the current black paper-based films have the disadvantages of low light transmittance, insufficient strength, poor water resistance, and rapid biodegradation (Guo Shuai, Long Zhu, Zhao Yu, et al. Preparation and strength properties of waste cotton fiber paper-based films [J]. New Chemical Materials, 2016, 44(2): 3. DOI: CNKI: SUN: HGXC.0.2016-02-046.; Li Hui. Degradable cellulose-based Preparation and performance research of ground film [D]. Qilu University of Technology, 2019.; Lv Guohua, Bai Wenbo, Guo Jinyi, Song Jiqing. Analysis of research status and development trend of paper ground film in my country [J]. Agricultural Mechanization Research, 2012, 34(09): 249-252. DOI: 10.13427 / j.cnki.njyi.2012.09.003.; Zhou Jinghui, Zhu Hongwei. Overview of research and application of paper ground film [J]. China Papermaking, 2002(05): 58-60.).

[0004] Therefore, preparing a coating that can effectively utilize resources, has a simple process flow and reduces production costs will become the first choice for producing greenhouse mulch paper by coating method. Summary of the invention

[0005] In view of the above problems, the present invention aims to provide a low-quantity special coating for greenhouse mulch paper and a preparation method thereof, so as to solve the technical problems in the production of greenhouse mulch paper by coating method.

[0006] The invention provides a water-based coating for greenhouse ground film paper, which comprises the following raw materials in parts by weight: 20 to 30 parts of black color paste; 25 to 35 parts of styrene-butadiene latex or water-based polyurethane adhesive, 5 to 8 parts of PVDC and EAA waterproof and moisture-blocking agents, 1 to 2 parts of carboxymethyl cellulose and modified chitosan dry strength agent (the mass ratio of carboxymethyl cellulose to modified chitosan dry strength agent is 4-6:1), 0.1 to 0.5 parts of polyether defoaming agent, 0.5 to 1 parts of sodium hexametaphosphate dispersant, 1 to 2 parts of sodium hypophosphite hydrophobic agent, and 100 parts of distilled water.

[0007] The present invention provides a method for preparing the water-based coating for greenhouse mulch paper, which comprises the following steps:

[0008] Step (1): stirring distilled water and sodium hexametaphosphate using a high-speed disperser to dissolve the dispersant;

[0009] Step (2): add black color paste and slowly pour it into a disperser to continue dispersing to obtain a uniformly mixed pigment dispersion;

[0010] Step (3): Add PVDC or EAA waterproof and moisture-blocking agent to the pigment dispersion, and continue to stir with a high-speed disperser to mix evenly;

[0011] Step (4): adding carboxymethyl cellulose and modified chitosan, mixing and dispersing, observing the coating state, and dropping a polyether defoamer;

[0012] Step (5): weighing styrene-butadiene latex or water-based polyurethane adhesive and continuing to stir;

[0013] Step (6): Finally, add sodium hypophosphite hydrophobic agent and mix well to obtain the target coating.

[0014] Specifically, in step (1), the high-speed disperser stirs at a speed of 800-1200 r / min for 5-15 min.

[0015] Preferably, in step (2), a high-speed shear disperser is used to stir the mixture at a speed of 4000-6000 r / min for 20-30 min.

[0016] In addition, preferably, in the step (3), PVDC or EAA is first stirred at a speed of 2500-3500 r / min for 15-25 min using a high-speed disperser, and after uniform mixing, carboxymethyl cellulose and modified chitosan are added and then mixed and dispersed at a speed of 2000-3000 r / min for 15-25 min, the coating state is observed, and a polyether defoamer is added dropwise.

[0017] Preferably, in step (4), stirring is performed at a speed of 2500-3500 r / min for 10-20 min using a high-speed shearing disperser; and in step (5), stirring is performed at a speed of 1500-2500 r / min for 5-15 min using a high-speed shearing disperser.

[0018] More preferably, the main component of the black color paste is high-pigment carbon black, which is beneficial to increase the surface strength of the coating, improve the opacity of the coated paper, and reduce the cost of the coating raw materials.

[0019] Specifically, the prepared target coating has a solid content of 20%-30%.

[0020] In a specific example of the present invention, the preparation method comprises the following steps:

[0021] Step (1): Stir the above-mentioned distilled water and sodium hexametaphosphate in parts by weight at a speed of 1000 r / min for 10 minutes using a high-speed disperser to dissolve the dispersant;

[0022] Step (2): slowly pour the above-mentioned black color paste in parts by weight into a disperser and stir at a speed of 5000 r / min for 25 minutes to obtain a uniformly mixed pigment dispersion;

[0023] Step (3): After the pigment is dispersed, add the above-mentioned weight portions of PVDC and EAA waterproof and moisture-blocking agent, stir at a speed of 3000 r / min for 20 minutes using a high-speed disperser, add the above-mentioned weight portions of carboxymethyl cellulose and modified chitosan after mixing evenly, mix and disperse at a speed of 2500 r / min for 20 minutes, observe the coating state, and add an appropriate amount of polyether defoamer.

[0024] Step (4): Weigh the above-mentioned weight portions of styrene-butadiene latex and water-based polyurethane adhesive, and continue stirring at a speed of 3000 r / min for 15 minutes.

[0025] Step (5): Finally, add the above-mentioned weight portion of sodium hypophosphite hydrophobic agent, stir at a speed of 2000 r / min for 10 minutes, and mix evenly to obtain the target coating.

[0026] The invention provides a water-based coating for greenhouse ground film paper obtained according to the preparation method.

[0027] Furthermore, the use of the water-based coating for greenhouse mulch paper in the preparation of greenhouse mulch paper is provided. Preferably, the coating amount of the water-based coating for greenhouse mulch paper applied to the greenhouse mulch paper is 4 g / m 2 -6g / m 2 , making the opacity of greenhouse mulch paper ≥95.0%.

[0028] Beneficial effects of the present invention:

[0029] (1) The low-quantity greenhouse ground film paper special coating of the present invention uses black color paste instead of carbon black powder as the pigment component, which is beneficial to prevent the impact of dust on the production environment, increase the service life of production equipment, effectively improve the utilization rate of carbon black, prevent resource waste and reduce environmental pollution.

[0030] (2) The present invention uses styrene-butadiene latex and water-based polyurethane as adhesives. Styrene-butadiene latex has excellent water and oil resistance and can be uniformly mixed with pigments. Both adhesives can increase the viscosity of the coating, reduce the foam generated during the coating preparation process, and make the coating have better fiber coverage and higher air permeability.

[0031] (3) The present invention adds PVDC and EAA waterproof and moisture-blocking agents, both of which are ideal materials with high barrier, strong toughness and good chemical stability. They have excellent moisture barrier and waterproof properties, can reduce water vapor transmission, and are unique in the coating, packaging and anti-corrosion industries. They have been widely used in surface coatings, food, drug packaging, mechanical parts, military strategic materials, and other fields. They are currently a very vital polymer material in the global coating, packaging and anti-corrosion industries. Carboxymethyl cellulose and modified chitosan dry strength agents help to improve the strength of the finished paper.

[0032] (4) The water-based coating for greenhouse ground film paper of the present invention has a simple preparation process and low production cost. The coating is soluble in water and has controllable viscosity. It is suitable for producing greenhouse ground film paper by coating or sizing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The following is an example coating prepared according to the present invention.

[0034] Figure 2 The greenhouse mulch paper sample was prepared by coating the example coating on ordinary kraft paper.

[0035] Figure 3 The coated paper was prepared by knife coating. DETAILED DESCRIPTION

[0036] The present invention is further described below in conjunction with the examples. Figure 1 .

[0037] Example 1

[0038] (1) 200 g of distilled water and 1 g of sodium hexametaphosphate were stirred at a speed of 1000 r / min for 10 min using a high-speed disperser to dissolve the dispersant.

[0039] (2) Add 47.5 g of carbon black in turn and continue stirring at 5000 r / min for 25 min to fully disperse the pigment.

[0040] (3) Add 33.34 g of EAA emulsion (solid content 30%) and stir at 3000 r / min for 20 min.

[0041] (4) Add 2 g of carboxymethyl cellulose and 0.4 g of modified chitosan, mix and disperse at a speed of 2500 r / min for 20 min, and add an appropriate amount of polyether defoamer.

[0042] (5) Add 120.11 g of styrene-butadiene latex (solid content 50%) and stir at a speed of 3000 r / min for 15 min.

[0043] (6) Add 1.5 g of sodium hypophosphite hydrophobic agent, stir at a speed of 2000 r / min for 10 min, and mix well to obtain the target coating.

[0044] Example 2

[0045] (1) 200 g of distilled water and 1 g of sodium hexametaphosphate were stirred at a speed of 1000 r / min for 10 min using a high-speed disperser to dissolve the dispersant.

[0046] (2) Add 47.5 g of carbon black in turn and continue stirring at 5000 r / min for 25 min to fully disperse the pigment.

[0047] (3) Add 16.67 g PVDC emulsion (solid content 60%) and stir at 3000 r / min for 20 min.

[0048] (4) Add 2 g of carboxymethyl cellulose and 0.4 g of modified chitosan, mix and disperse at a speed of 2500 r / min for 20 min, and add an appropriate amount of polyether defoamer.

[0049] (5) Add 120.11 g of styrene-butadiene latex (solid content 50%) and stir at a speed of 3000 r / min for 15 min.

[0050] (6) Add 1.5 g of sodium hypophosphite hydrophobic agent, stir at a speed of 2000 r / min for 10 min, and mix well to obtain the target coating.

[0051] Example 3

[0052] (1) 200 g of distilled water and 1 g of sodium hexametaphosphate were stirred at 1000 r / min for 10 min using a high-speed disperser to dissolve the dispersant.

[0053] (2) Add 47.5 g of carbon black in turn and continue stirring at 5000 r / min for 25 min to fully disperse the pigment.

[0054] (3) Add 16.67 g of EAA emulsion (solid content 30%) and 8.34 g of PVDC emulsion (solid content 60%) and stir at a speed of 3000 r / min for 20 min.

[0055] (4) Add 2 g of carboxymethyl cellulose and 0.4 g of modified chitosan, mix and disperse at a speed of 2500 r / min for 20 min, and add an appropriate amount of polyether defoamer.

[0056] (5) Add 120.11 g of styrene-butadiene latex (solid content 50%) and stir at a speed of 3000 r / min for 15 min.

[0057] (6) Add 1.5 g of sodium hypophosphite hydrophobic agent, stir at a speed of 2000 r / min for 10 min, and mix well to obtain the target coating.

[0058] Properties performance test

[0059] Serial number Paint Name Solid content (%) Viscosity (mPa.s) 1 Example 1 30.2 5328 2 Example 2 31.5 6770 3 Example 3 30.8 6213

[0060] Application Examples

[0061] The coatings of Example 1, Example 2 and Example 3 and the method of scraper coating (see attached Figure 3 ) was coated on 60g of ordinary kraft paper. The sample was Figure 2 .

[0062] (1) Water vapor transmission rate test

[0063] The test is carried out on a water vapor permeability tester according to GB / T 16928-1997. The specific test steps are as follows:

[0064] ① Paper sample pretreatment: Before the experiment, the paper sample should be processed according to the provisions of GB / T2918 to ensure that the paper sample has no wrinkles, pinholes, or stains; meet the minimum size requirements of the sample to facilitate cutting and sealing; the thickness of the paper sample should be uniform.

[0065] ② Sampling and clamping: Place the paper sample flat on the cutting pad, cut the sample with a sampler, and clamp the paper sample on the standard moisture permeable cup in order.

[0066] ③Test: Use the weight loss method to test the water vapor permeability of the paper sample.

[0067] (2) Cobb value determination

[0068] The test is carried out on the absorbency tester according to GB / T 1540-2002. The specific test steps are as follows:

[0069] ① Sample collection, treatment and preparation: Samples were collected according to GB / T450, and temperature and humidity treatment was performed according to GB / T10739. The treated paper samples were cut into (125±5) mm square specimens. ② Test: The water absorption of the paper samples was tested by flipping method, and the cobb value was calculated.

[0070] (3) Tear strength measurement

[0071] The test was carried out on a tear tester (Sichuan Changjiang J-SLY1000) according to GB / T455-2002. The specific test steps are as follows:

[0072] ① Sample collection, processing and preparation: Samples shall be collected according to GB / T450, ensuring that the sample has no creases, wrinkles or other obvious defects, and temperature and humidity treatment shall be carried out according to GB / T10739. The size of the sample shall be (63±0.5)mm×(50±2)mm, and the sample shall be cut in the longitudinal and transverse directions. If the longitudinal direction of the paper is parallel to the short side of the sample, a transverse test shall be carried out, otherwise a longitudinal test shall be carried out. At least 5 valid tests shall be carried out in each direction.

[0073] ②Test: Use a tear tester to test the tear strength of the paper sample and calculate the tear index.

[0074] (4) Determination of longitudinal fracture length

[0075] The test was carried out on a tensile strength tester (Sichuan Changjiang DCP-KZ300) according to GB / T12914-2018. The specific test steps are as follows:

[0076] ① Paper sample collection, processing and preparation: Samples are collected according to GB / T450 and temperature and humidity treatment is performed according to GB / T10739. From undamaged paper and cardboard samples, cut a sample strip with a width of (15±0.1) mm and a length sufficient to be clamped between the two clamps. Avoid touching the sample part between the two clamps with your hands. The two long sides of the sample should be straight, and the parallelism error should not exceed ±0.1mm within the entire clamping length. The sample cut should be neat and undamaged. Cut a sufficient number of sample strips at one time.

[0077] ② Adjust the chuck distance to the specified initial test length and clamp the specimen on the chuck. Be careful not to touch the test area between the two clamping lines of the specimen with your hands. Straighten and clamp the specimen without any slack or obvious strain. Ensure that the specimen is parallel to the direction of the applied tension.

[0078] ③Test: Start the test until the sample breaks. Record the maximum applied tension and elongation (in mm), and calculate the tensile strength and longitudinal breaking length.

[0079] (5) Wet strength measurement

[0080] According to GB / T 465.2-2008, the test was carried out on a tensile strength tester (Sichuan Changjiang DCP-KZ300). The specific test steps are as follows:

[0081] ① Sample collection, processing and preparation: Collect samples according to GB / T450, immerse the samples in water that meets the requirements of GB / T10739 for 10 minutes, take the samples out of the pan, and gently absorb the water on the surface of the samples with filter paper or blotting paper.

[0082] ②Test: Soak the sample in water, absorb the surface moisture, and quickly place it on the tensile strength tester to measure the tensile strength and calculate the wet strength.

[0083] (6) Transmittance measurement

[0084] The test was carried out on a UV spectrophotometer. The specific test steps are as follows:

[0085] ① Paper sample collection, processing and preparation: Cut sample strips with a width of (15±0.1) mm and a length of (40±0.1) mm from undamaged paper and paperboard samples.

[0086] ②Test: Using the integrating sphere mode, the transmittance of the sample was measured at fixed points at wavelengths of 550nm and 850nm.

[0087] The results are shown in Table 1.

[0088] Table 1 Quantitative 60g ordinary kraft paper experimental data

[0089]

[0090]

[0091] As can be seen from the table, it can significantly improve the moisture resistance, water resistance and light transmittance of the base paper, and all indicators of the coated paper at low coating amounts meet the standard requirements of Class A natural color ground film paper. When the single-sided coating amounts of Example 1, Example 2 and Example 3 are 3.48g / m2, 6.51g / m2 and 5.83g / m2 respectively, the water vapor permeability of samples No. 1, No. 4 and No. 7 is reduced from 1987g / (m2.24h) of the base paper to 393, 548 and 499g / (m2.24h), respectively, which meets the moisture resistance requirements of Class A ground film paper; and the 120s Cobb value is 9-16g / m2, meeting the requirement of a water resistance value of less than 20. In the research experiment, in order to more accurately reflect the light-shielding performance of the sample, the transmittance of the paper sample at 550nm and 850nm was measured by an ultraviolet spectrophotometer. From the test results, it can be seen that the light transmittance of the paper coated with the coatings of Example 1, Example 2 and Example 3 at 550nm and 850nm is only 0-1.6%, which is lower than 5% and meets the light-shielding requirements.

[0092] Increasing the coating amount can further reduce water vapor transmission and light transmittance, but the Cobb value increases with the increase of coating amount and the water resistance decreases.

[0093] In addition, coating improves the bursting index and wet strength of the base paper. After coating with the coatings of Example 1, Example 2 and Example 3, the bursting index of the base paper is increased by 0.5 to 38%, and the wet strength is increased by 3 to 4.4 times.

[0094] From the analysis table data, it can be seen that the performance improvement effect of the coatings of Example 1, Example 2 and Example 3 on offset paper is equivalent to that of ordinary kraft paper, and the influence of the coating amount on various indicators of paper is similar to that of kraft paper. After coating, the water vapor permeability decreases from 2207g / (m2.24h) to 412-784g / (m2.24h), the Cobb value is 6-24g / m2, the light transmittance is 0-2.1%, the bursting index is increased by 7-21%, and the wet strength is increased by 0.7-4.71 times.

[0095] In summary, when the coating schemes of Example 1, Example 2 and Example 3 are used with low coating amounts, the water vapor transmission rate, Cobb value (120s), paper bursting index, wet strength and light transmittance are all improved.

Claims

1. A water-based coating for greenhouse mulch paper, characterized by: The invention comprises the following raw materials in parts by weight: 20-30 parts of black color paste; 25-35 parts of styrene-butadiene latex or water-based polyurethane adhesive; 5-8 parts of PVDC and EAA waterproof and moisture-blocking agents; 1-2 parts of a mixture of carboxymethyl cellulose and modified chitosan dry strength agent in a mass ratio of 4-6:1; 0.1-0.5 parts of polyether defoaming agent; 0.5-1 parts of sodium hexametaphosphate dispersant; 1-2 parts of sodium hypophosphite hydrophobic agent; and 100 parts of distilled water.

2. The method for preparing the water-based coating for greenhouse mulch paper according to claim 1, characterized in that The steps include: Step (1): Stir distilled water and sodium hexametaphosphate using a high-speed disperser to dissolve the dispersant; Step (2): add black color paste and slowly pour it into the disperser to continue dispersing to obtain a uniformly mixed pigment dispersion; Step (3): Add PVDC or EAA waterproof and moisture-blocking agent to the pigment dispersion, and continue to stir with a high-speed disperser to mix evenly; Step (4): add carboxymethyl cellulose and modified chitosan, mix and disperse, observe the coating state, and add polyether defoamer dropwise; Step (5): Weigh styrene-butadiene latex or water-based polyurethane adhesive and continue stirring; Step (6): Finally, add sodium hypophosphite hydrophobic agent and mix evenly to obtain the target coating.

3. The preparation method according to claim 2, wherein: In the step (1), the high-speed disperser is stirred at a speed of 800-1200 r / min for 5-15 minutes.

4. The preparation method according to claim 2, wherein: In the step (2), a high-speed shearing disperser is used to stir the mixture at a speed of 4000-6000 r / min for 20-30 min.

5. The preparation method according to claim 2, wherein: In step (3), PVDC or EAA is first stirred at a speed of 2500-3500 r / min for 15-25 min using a high-speed disperser. After uniform mixing, carboxymethyl cellulose and modified chitosan are added and then mixed and dispersed at a speed of 2000-3000 r / min for 15-25 min. The coating state is observed and a polyether defoamer is added dropwise.

6. The preparation method according to claim 2, wherein: In the step (4), the mixture is stirred at a speed of 2500-3500 r / min for 10-20 min using a high-speed shearing disperser; and in the step (5), the mixture is stirred at a speed of 1500-2500 r / min for 5-15 min using a high-speed shearing disperser.

7. The preparation method according to claim 2, wherein: The main component of the black color paste is high-pigment carbon black.

8. The preparation method according to claim 2, wherein: The target solid content of the prepared coating is 20%-30%.

9. A water-based coating for greenhouse mulch paper obtained according to the preparation method according to any one of claims 2 to 8.

10. Use of the water-based coating for greenhouse mulch paper according to claim 9 in the preparation of greenhouse mulch paper.

11. The use according to claim 10, characterized in that The coating amount of the water-based coating applied to the greenhouse film paper is 4g / m 2 -6g / m 2 , making the opacity of greenhouse film paper ≥95.0%.