A kind of carbon nine petroleum resin and preparation method thereof
Through the alkylation and copolymerization of hydroxyl compounds and methylstyrene, combined with Lewis acid catalysts, the problem of insufficient performance of existing C9 petroleum resins is solved, and C9 petroleum resins with high performance and good stability are prepared to meet the needs of high-end market demand.
Patent Information
- Application Number
- CN202310675684.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-06-08
AI Technical Summary
The existing carbon-9 petroleum resin thermal polymerization process cannot obtain high-quality resin products. The hue and compatibility properties of the resin are generally poor, and cannot meet the needs of the high-end market.
After the alkylation reaction between hydroxyl compounds and methylstyrene, methylstyrene and styrene are added for copolymerization, a Lewis acid catalyst is used to control the reaction conditions, and filtration and post-processing are performed to obtain high-performance C9 petroleum resin.
The prepared C9 petroleum resin has high hydroxyl value, good compatibility, wide adaptability, light color, stable product quality, and is suitable for high-end markets.
Smart Images

Figure BDA0004274507460000101 
Figure BDA0004274507460000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of petroleum resins, and in particular to a carbon nine petroleum resin and a preparation method thereof. Background Art
[0002] Petroleum resin is a solid or viscous liquid polymer with a low relative molecular weight obtained by polymerization with C5 / C9 fraction, a by-product of ethylene plant, as the main raw material. According to the monomer and molecular structure of the resin, it can be roughly divided into aromatic petroleum resin, aliphatic petroleum resin and alicyclic petroleum resin.
[0003] Aromatic petroleum resin, also known as C9 petroleum resin, is obtained by polymerizing the above-mentioned ethylene by-product C9 fraction as raw material. Its production raw material is mainly the cracked C9 fraction oil by-product of ethylene plant, which accounts for about 10% to 20% of the ethylene production. The fraction oil has a complex composition and is rich in unsaturated hydrocarbons such as styrene, methyl styrene, dicyclopentadiene, indene, methylcyclopentadiene dimer, etc.
[0004] At present, there are two main methods for producing petroleum resin using C9 fraction: one is the low-temperature polymerization method with cationic catalysis (referred to as cold polymerization method), and the other is the free radical polymerization method initiated by heating (referred to as hot polymerization method). The hot polymerization process of C9 petroleum resin has the advantages of simple process, high conversion rate and output, and stable product performance. Its main drawback is that it is impossible to obtain high-quality resin products. The hue and compatibility of the resin are generally poor, which cannot meet the needs of the high-end market. It is generally only used in the fields of alkyd paint and rubber mixing, and the product added value is low.
[0005] Cold-polymerized C9 petroleum resin is a resin with a certain softening point obtained by copolymerizing the polymerizable olefin components in the C9 fraction under the conditions of a catalyst or a peroxide initiator. The main polymerizable components in the C9 fraction all contain large conjugated electron cloud structures, which are easy to copolymerize with certain monomers with electrophilic groups; in addition, the aromatic ring is also an ideal electrophilic substitution reaction substrate, and it is easy to introduce polar groups on the aromatic ring for chemical modification. For example, in patent CN1091751A, polar molecules such as acrylic acid and maleic anhydride are used to copolymerize with C9 fraction oil in a solution free radical copolymerization or free radical emulsion polymerization under the initiation of peroxide or azo compounds to prepare water-soluble C9 petroleum resin. Therefore, it is urgent to find a new method for preparing C9 petroleum resin. Therefore, the existing technology needs to be further developed. Summary of the invention
[0006] The purpose of the present invention is to overcome the above technical deficiencies and provide a carbon nine petroleum resin and a preparation method thereof.
[0007] In order to achieve the above technical objectives, the present invention adopts the following technical scheme: a method for preparing a carbon nine petroleum resin is provided, a hydroxy compound is subjected to an alkylation reaction with methyl styrene, and after the reaction, methyl styrene, a carbon nine fraction and styrene are added for copolymerization reaction, and the carbon nine petroleum resin is obtained by post-treatment of filtering and removing impurities.
[0008] Furthermore, when the hydroxy compound and methyl styrene undergo alkylation reaction, the molar ratio of the hydroxy compound to methyl styrene is (1-3):1.
[0009] Furthermore, the mass ratio of the total amount of methylstyrene added during the alkylation reaction and the copolymerization reaction to styrene is (1-5):1.
[0010] Furthermore, the reaction temperature of the alkylation reaction is 40-80°C, and the reaction temperature of the copolymerization reaction is 10-25°C.
[0011] Furthermore, the specific process of the alkylation reaction is as follows: the hydroxyl compound and methyl styrene are mixed in a xylene and / or toluene solvent and then a Lewis acid catalyst is added; the specific process of the copolymerization reaction is as follows: methyl styrene, carbon nine fraction, and Lewis acid catalyst are added again, and then styrene is added dropwise to react for 1-2 hours, and calcium hydroxide and sodium hydroxide are added to react again for 30-60 minutes before terminating the reaction.
[0012] Furthermore, the ratio of the solvent mass to the total mass of the first olefin is greater than 1:1, and the first olefin includes methylstyrene and styrene added in the alkylation reaction and the copolymerization reaction respectively; the mass of the calcium hydroxide is 2% of the total mass of the hydroxyl compound, methylstyrene added in the alkylation reaction, the mass of the methylstyrene added in the copolymerization reaction, the carbon nine fraction, and styrene; the mass of the sodium hydroxide is 10% of the mass of the calcium hydroxide.
[0013] Furthermore, the mass of the hydroxyl compound is m1, which is 15% of the total mass of the product C9 petroleum resin; the total mass of the second olefin is m2, which is m2=m1 / 0.15-m1; the second olefin includes methylstyrene added in the alkylation reaction, methylstyrene added in the copolymerization reaction, and components and styrene in the C9 fraction participating in the copolymerization reaction; the mass of the components in the C9 fraction participating in the copolymerization reaction is m3, which is m3=m2×(40% to 60%); the mass of the Lewis acid catalyst added in the alkylation reaction is 0.1 to 0.2% of the total mass of the hydroxyl compound and methylstyrene added in the alkylation reaction; the mass of the Lewis acid catalyst added in the copolymerization reaction is 0.1 to 0.2% of the total mass of the components, methylstyrene and styrene in the C9 fraction added in the copolymerization reaction.
[0014] Furthermore, the hydroxy compound is benzyl alcohol or p-tert-butylphenol.
[0015] Furthermore, the post-treatment also includes distillation at 220° C. to remove the solvent and unreacted low molecular weight substances.
[0016] In addition, the present invention also provides a carbon nine petroleum resin prepared by the above method.
[0017] Beneficial effects:
[0018] 1. The present invention utilizes the carbon nine fraction and also adds hydroxyl compounds, methylstyrene and styrene. The methylstyrene and styrene adjust the content of related components in the carbon nine fraction; the hydroxyl compound undergoes an alkylation reaction with the introduced methylstyrene and styrene, and the prepared carbon nine petroleum resin has a high hydroxyl value, good compatibility with EVA, alkyd, etc., and the product has a wide adaptability.
[0019] 2. The carbon nine petroleum resin prepared by the present invention has light color and stable product quality. DETAILED DESCRIPTION
[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0021] According to an embodiment of the present invention, a method for preparing a carbon nine petroleum resin is provided, wherein a hydroxyl compound and methyl styrene undergo an alkylation reaction, and after the reaction, methyl styrene, a carbon nine fraction and styrene are added for copolymerization, and the carbon nine petroleum resin is obtained by post-treatment of filtering and removing impurities. Hydroxyl compounds, methyl styrene and styrene are added while utilizing the carbon nine fraction, and the added methyl styrene and styrene adjust the content of related components in the carbon nine fraction, so that methyl styrene and styrene increase during the entire reaction process; the hydroxyl compound undergoes an alkylation reaction with the introduced methyl styrene and styrene, and the prepared carbon nine petroleum resin has a high hydroxyl value, good compatibility with EVA, alkyd, etc., and a wide range of product adaptability. Methyl styrene is not added at one time, but is added separately during the alkylation reaction and the copolymerization reaction. If an excessive amount is added at one time, it is easy to cause methyl styrene to self-polymerize.
[0022] The carbon nine fraction is prepared by the following process: using carbon nine aromatic hydrocarbons as raw materials, the carbon nine aromatic hydrocarbons are first treated as follows: the distillation range cut out by atmospheric distillation is a fraction between 180 and 200°C. The contents of the components in the fraction are as follows: 0 styrene, 9% methyl styrene, 33% indene, 12% methyl indene, 0.3% naphthalene, 54.3% of the components involved in the copolymerization reaction in the carbon nine fraction, and 45.7% of the rest.
[0023] In some embodiments, the amount of hydroxyl compound added can be calculated based on the expected final output of C9 petroleum resin, and the amount of hydroxyl compound added is 15% of the total mass of C9 petroleum resin, where the total mass of C9 petroleum resin is the expected final output of C9 petroleum resin.
[0024] In some embodiments, the amount of the catalyst used in the alkylation reaction is 0.1% to 0.2% of the hydroxy compound and methyl styrene in the alkylation reaction.
[0025] In some embodiments, the mass proportion of the carbon nine fraction participating in the copolymerization reaction in the carbon nine fraction is 54.3%.
[0026] In some embodiments, the Lewis acid catalyst may be boron trifluoride, and may also be aluminum trichloride or ferric chloride, but is not limited to boron trifluoride.
[0027] The following is an explanation through specific embodiments.
[0028] Embodiment 1:
[0029] Step 101: Add 450 g of solvent xylene, 108.1 g of hydroxy compound benzyl alcohol, and 118.2 g of methyl styrene into a reactor in sequence, stirring continuously during the addition of the materials, and the molar ratio of benzyl alcohol to methyl styrene is 1:1;
[0030] Step 102: nitrogen is charged into the reactor, and the temperature is raised to 40° C. using a constant temperature water bath to keep the temperature of the initial material in the reactor constant;
[0031] Step 103: After the initial temperature is constant, 0.34 g of boron trifluoride is introduced successively, and the reaction temperature is controlled to 60° C. by adjusting the water bath temperature;
[0032] Step 104: After the temperature stops rising, stop introducing boron trifluoride, continue stirring for 0.5 h, and lower the temperature in the reactor to 5° C.;
[0033] Step 105: 137.8 g of methyl styrene and 500 g of the treated carbon nine fraction are added in sequence, and the materials are continuously stirred during the addition process;
[0034] Step 106: Add 0.74 g of boron trifluoride again;
[0035] Step 107: slowly dropwise add 85.31 g of styrene, stir, and control the material temperature in the reactor to be 15° C.;
[0036] Step 108: After the material becomes obviously viscous, continue stirring for 1 hour;
[0037] Step 109: add 19 g of calcium hydroxide with a particle size of 400 mesh, and stir for 30 min; then add 1.9 g of sodium hydroxide with a concentration of 10%, and continue stirring for 30 min;
[0038] Step 110: sampling and testing the pH value to be 7.2, the neutralization reaction is completed, stirring is stopped, and the polymerization reaction is terminated;
[0039] Step 111: Filter to remove solid materials;
[0040] Step 112: distill the filtered liquid material to 220° C. under normal pressure to remove the solvent and unreacted low molecular weight substances, i.e., C9 petroleum resin.
[0041] Among them, the mass ratio of the total amount of methyl styrene used to styrene in the whole process is 3:1.
[0042] In addition, the flask was kept in a nitrogen or boron trifluoride environment throughout the entire process until neutralization.
[0043] Example 2
[0044] Step 101: 550 g of solvent xylene, 150.2 g of hydroxy compound p-tert-butylphenol (PTBP), and 118.2 g of methyl styrene are added into a reactor in sequence, and the materials are continuously stirred during the addition process, and the molar ratio of benzyl alcohol to methyl styrene is 1:1;
[0045] Step 102: nitrogen is charged into the reactor, and the temperature is raised to 40° C. using a constant temperature water bath to keep the temperature of the initial material in the reactor constant;
[0046] Step 103: After the initial temperature is constant, 0.40 g of boron trifluoride is introduced successively, and the reaction temperature is controlled to 60° C. by adjusting the water bath temperature;
[0047] Step 104: After the temperature stops rising, stop introducing boron trifluoride, continue stirring for 0.5 h, and lower the temperature in the reactor to 0° C.;
[0048] Step 105: 173.9 g of methyl styrene and 850 g of the treated carbon nine fraction are added in sequence, and stirring is continued during the addition of the materials;
[0049] Step 106: 1.1 g of boron trifluoride is introduced again;
[0050] Step 107: slowly dropwise add 97.4 g of styrene, stir, and control the material temperature in the reactor to 20° C.;
[0051] Step 108: After the material becomes obviously viscous, continue stirring for 1 hour;
[0052] Step 109: add 27.8 g of calcium hydroxide with a particle size of 400 mesh, and stir for 30 min; then add 2.78 g of sodium hydroxide with a concentration of 10%, and continue stirring for 30 min;
[0053] Step 110: sampling and testing the pH value to be 7.2, the neutralization reaction is completed, stirring is stopped, and the polymerization reaction is terminated;
[0054] Step 111: Filter to remove solid materials;
[0055] Step 112: distill the filtered liquid material to 220° C. under normal pressure to remove the solvent and unreacted low molecular weight substances to obtain C9 petroleum resin.
[0056] Among them, the mass ratio of the total amount of methyl styrene used to styrene in the whole process is 3:1.
[0057] In addition, the flask was kept in a nitrogen or boron trifluoride environment throughout the entire process until neutralization.
[0058] Example 3
[0059] Step 101: 400 g of solvent toluene, 108.1 g of hydroxy compound benzyl alcohol, and 118.2 g of methyl styrene are added into a reactor in sequence, and the materials are continuously stirred during the addition process, and the molar ratio of benzyl alcohol to methyl styrene is 1:1;
[0060] Step 102: nitrogen is charged into the reactor, and the temperature is raised to 60° C. using a constant temperature water bath to keep the temperature of the initial material in the reactor constant;
[0061] Step 103: After the initial temperature is constant, 0.34 g of boron trifluoride is introduced successively, and the reaction temperature is controlled to 80° C. by adjusting the water bath temperature;
[0062] Step 104: After the temperature stops rising, stop introducing boron trifluoride, continue stirring for 0.5 h, and lower the temperature in the reactor to 3° C.;
[0063] Step 105: 137.8 g of methyl styrene and 500 g of the treated carbon nine fraction are added in sequence, and the materials are continuously stirred during the addition process;
[0064] Step 106: Add 0.74 g of boron trifluoride again;
[0065] Step 107: slowly dropwise add 85.31 g of styrene, stir, and control the material temperature in the reactor to 25° C.;
[0066] Step 108: After the material becomes obviously viscous, continue stirring for 1 hour;
[0067] Step 109: add 19 g of calcium hydroxide with a particle size of 400 mesh, and stir for 30 min; then add 1.9 g of sodium hydroxide with a concentration of 10%, and continue stirring for 30 min;
[0068] Step 110: sampling and testing the pH value to be 7.3, the neutralization reaction is completed, stirring is stopped, and the polymerization reaction is terminated;
[0069] Step 111: Filter to remove solid materials;
[0070] Step 112: distill the filtered liquid material to 220° C. under normal pressure to remove the solvent and unreacted low molecular weight substances to obtain C9 petroleum resin.
[0071] Among them, the mass ratio of the total amount of methyl styrene used to styrene in the whole process is 3:1.
[0072] In addition, the flask was kept in a nitrogen or boron trifluoride environment throughout the entire process until neutralization.
[0073] Embodiment 4:
[0074] Step 101: 500 g of solvent xylene, 150.2 g of hydroxy compound p-tert-butylphenol (PTBP), and 118.2 g of methyl styrene are added into a reactor in sequence, and the materials are continuously stirred during the addition process, and the molar ratio of p-tert-butylphenol to methyl styrene is 1:1;
[0075] Step 102: nitrogen is charged into the reactor, and the temperature is raised to 40° C. using a constant temperature water bath to keep the temperature of the initial material in the reactor constant;
[0076] Step 103: After the initial temperature is constant, 0.4 g of boron trifluoride is introduced successively, and the reaction temperature is controlled to 60° C. by adjusting the water bath temperature;
[0077] Step 104: After the temperature stops rising, stop introducing boron trifluoride, continue stirring for 0.5 h, and lower the temperature in the reactor to 5° C.;
[0078] Step 105: 94.6 g of methyl styrene and 783.7 g of the treated carbon nine fraction are added in sequence, and stirring is continued during the addition of the materials;
[0079] Step 106: 1.1 g of boron trifluoride is introduced again;
[0080] Step 107: slowly dropwise add 212.8 g of styrene, stir, and control the material temperature in the reactor to 20° C.;
[0081] Step 108: After the material becomes obviously viscous, continue stirring for 1 hour;
[0082] Step 109: add 27.2 g of calcium hydroxide with a particle size of 400 mesh, and stir for 30 min; then add 2.72 g of sodium hydroxide with a concentration of 10%, and continue stirring for 30 min;
[0083] Step 110: sampling and testing the pH value to be 7.1, the neutralization reaction is completed, stirring is stopped, and the polymerization reaction is terminated;
[0084] Step 111: Filter to remove solid materials;
[0085] Step 112: distill the filtered liquid material to 220° C. under normal pressure to remove the solvent and unreacted low molecular weight substances to obtain C9 petroleum resin.
[0086] Among them, the mass ratio of the total amount of methyl styrene used and styrene in the whole process is 1:1.
[0087] In addition, the flask was kept in a nitrogen or boron trifluoride environment throughout the entire process until neutralization.
[0088] Embodiment 5:
[0089] Step 101: 500 g of solvent xylene, 150.2 g of hydroxy compound p-tert-butylphenol (PTBP), and 236.4 g of methyl styrene are added into a reactor in sequence, and the materials are continuously stirred during the addition process. The molar ratio of p-tert-butylphenol to methyl styrene is 2:1;
[0090] Step 102: nitrogen is charged into the reactor, and the temperature is raised to 40° C. using a constant temperature water bath to keep the temperature of the initial material in the reactor constant;
[0091] Step 103: After the temperature is constant, 0.58 g of boron trifluoride is introduced successively, and the reaction temperature is controlled to 60° C. by adjusting the water bath temperature;
[0092] Step 104: After the temperature stops rising, stop introducing boron trifluoride, continue stirring for 0.5 h, and lower the temperature in the reactor to 5° C.;
[0093] Step 105: 82.8 g of methyl styrene and 783.7 g of the treated carbon nine fraction are added in sequence, and stirring is continued during the addition of the materials;
[0094] Step 106: Add 0.92 g of boron trifluoride again;
[0095] Step 107: slowly dropwise add 106.4 g of styrene, stir, and control the material temperature in the reactor to be 15° C.;
[0096] Step 108: After the material becomes obviously viscous, continue stirring for 1 hour;
[0097] Step 109: add 27.2 g of calcium hydroxide with a particle size of 400 mesh, and stir for 30 min; then add 2.72 g of sodium hydroxide with a concentration of 10%, and continue stirring for 30 min;
[0098] Step 110: sampling and testing the pH value to be 7.1, the neutralization reaction is completed, stirring is stopped, and the polymerization reaction is terminated;
[0099] Step 111: Filter to remove solid materials;
[0100] Step 112: distill the filtered liquid material to 220° C. under normal pressure to remove the solvent and unreacted low molecular weight substances, thereby obtaining a carbon nine petroleum resin with a high hydroxyl value, light color, and high softening point.
[0101] Among them, the mass ratio of the total amount of methyl styrene used to styrene in the whole process is 3:1.
[0102] In addition, the flask was kept in a nitrogen or boron trifluoride environment throughout the entire process until neutralization.
[0103] Embodiment 6:
[0104] Step 101: 550 g of solvent xylene, 150.2 g of hydroxy compound p-tert-butylphenol (PTBP), and 354.6 g of methyl styrene are added into a reactor in sequence, and the materials are continuously stirred during the addition process. The molar ratio of p-tert-butylphenol to methyl styrene is 3:1;
[0105] Step 102: nitrogen is charged into the reactor, and the temperature is raised to 40° C. using a constant temperature water bath to keep the temperature of the material in the reactor constant;
[0106] Step 103: After the temperature is constant, 0.76 g of boron trifluoride is introduced successively, and the reaction temperature is controlled to 60° C. by adjusting the water bath temperature;
[0107] Step 104: After the temperature stops rising, stop introducing boron trifluoride, continue stirring for 0.5 h, and lower the temperature in the reactor to 0° C.;
[0108] Step 105: 70.95 g of methyl styrene and 627 g of the treated carbon nine fraction are added in sequence, and stirring is continued during the addition of the materials;
[0109] Step 106: Add 0.74 g of boron trifluoride again;
[0110] Step 107: Slowly drop 85.11 g of styrene, stir, and control the material temperature in the reactor to be 15° C.;
[0111] Step 108: After the material becomes obviously viscous, continue stirring for 1 hour;
[0112] Step 109: add 25.8 g of calcium hydroxide with a particle size of 400 mesh, and stir for 30 min; then add 2.58 g of sodium hydroxide with a concentration of 10%, and continue stirring for 30 min;
[0113] Step 110: sampling and testing the pH value to be 7.1, the neutralization reaction is completed, stirring is stopped, and the polymerization reaction is terminated;
[0114] Step 111: Filter to remove solid materials;
[0115] Step 112: distill the filtered liquid material to 220° C. under normal pressure to remove the solvent and unreacted low molecular weight substances to obtain C9 petroleum resin.
[0116] Among them, the mass ratio of the total amount of methyl styrene used to styrene in the whole process is 5:1.
[0117] In addition, the flask was kept in a nitrogen or boron trifluoride environment throughout the entire process until neutralization.
[0118] Comparative Example 1:
[0119] Compared with Example 4, no p-tert-butylphenol, methylstyrene and styrene were added, and only the carbon nine fraction was used as a raw material for the reaction. The other steps were exactly the same.
[0120] The Example 6 and the Comparative Example 1-2 were analyzed and tested, and the test and analysis methods were as follows:
[0121] Wax fog point: The mass ratio of EVA, wax, and resin is 6:6:8. After melting, pour into a 25ml colorimetric tube and insert a thermometer in the middle of the liquid. Stir gently until fog appears and covers the mercury ball of the thermometer. Read the temperature on the thermometer, which is the wax fog point.
[0122] Alkyd miscibility: First, mix the solvent with the petroleum resin in a 1:1 ratio. After dissolving, mix the long oil alkyd resin with the mixed and dissolved petroleum resin solution in a 1:1 mass ratio, apply it to a transparent slide, leave it for 24 hours, and observe whether it is clear. If it is clear, it is good.
[0123] Volatile matter: Use a dry beaker to weigh about 5g of petroleum resin, place it in an oven at 185℃, take it out after 4 hours, place it in a desiccator to cool to room temperature, and weigh it. The percentage of the lost weight to the weight of the weighed petroleum resin is the volatile matter.
[0124] The test results are shown in Table 1.
[0125] Table 1 Performance test results of C9 petroleum resin
[0126]
[0127]
[0128] From the performance test results of carbon nine petroleum resin in Table 1, it can be seen that, first, for Examples 1-6, compared with Example 1 and Example 2, the effect of using PTBP as the hydroxyl compound in Example 2 is slightly better, ensuring that the hydroxyl value and softening point are high at the same time; compared with Example 1 and Example 3, under the same material conditions, the reaction temperature of the first feeding of methyl styrene in Example 3 increases (step 102), the softening point decreases with the increase of temperature, the reaction is more complete, and the bromine value decreases; compared with Example 2 and Example 4, both are PTBP, the styrene content is appropriately increased, the softening point increases, the reaction is more complete, and the bromine value decreases; compared with Example 2 and Example 5, for the same material, the first methyl styrene content increases, the softening point decreases, the reaction is not complete, and the bromine value is relatively high; compared with Example 2 and Example 6, the amount of styrene decreases, the first methyl styrene feeding increases, the softening point decreases more than Example 5, and the bromine value decreases more. It can be seen from the above that the first methyl styrene feeding ratio can affect the bromine value and softening point of carbon nine petroleum resin. The first addition of methyl styrene increases, the softening point decreases, and the bromine value increases; the first addition of methyl styrene decreases, and the softening point increases and the bromine value decreases. The feed ratio of styrene to methyl styrene can affect the softening point and bromine value of C9 petroleum resin. When the amount of styrene increases, the reaction is relatively violent, the softening point increases relatively, and the bromine value decreases. When the amount of styrene decreases, the softening point decreases and the bromine value increases. The reaction temperature when methyl styrene is first fed can affect the softening point and bromine value of C9 petroleum resin. When the temperature increases, the softening point decreases and the bromine value decreases. When the temperature decreases, the softening point increases and the bromine value increases.
[0129] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a carbon nine petroleum resin, characterized in that: The hydroxy compound and methyl styrene undergo an alkylation reaction, and after the alkylation reaction, methyl styrene, a carbon nine fraction and styrene are added to undergo a copolymerization reaction to obtain a carbon nine petroleum resin; When the hydroxy compound and methyl styrene undergo an alkylation reaction, the molar ratio of the hydroxy compound to the methyl styrene is (1-3):1; The mass ratio of the total amount of methylstyrene added during the alkylation reaction and the copolymerization reaction to styrene is (1-5):1; The reaction temperature of the alkylation reaction is 40-80°C; The reaction temperature of the copolymerization reaction is 10-25°C; The specific process of the alkylation reaction is as follows: a hydroxy compound and methyl styrene are mixed in a xylene and / or toluene solvent, and then a Lewis acid catalyst is added; the specific process of the copolymerization reaction is as follows: methyl styrene, carbon nine fraction, and Lewis acid catalyst are added again, and then styrene is added dropwise to react for 1-2 hours, and calcium hydroxide and sodium hydroxide are added to react again for 30-60 minutes before terminating the reaction; The hydroxy compound is benzyl alcohol or p-tert-butylphenol.
2. The method for preparing carbon nine petroleum resin according to claim 1, characterized in that: The ratio of the solvent mass to the total mass of the first olefin is greater than 1:1, and the first olefin is methylstyrene and styrene added in the alkylation reaction and the copolymerization reaction, respectively; The mass of calcium hydroxide is 2% of the total mass of the hydroxyl compound, methyl styrene added in the alkylation reaction, the mass of methyl styrene added in the copolymerization reaction, the carbon nine fraction, and styrene; The mass of sodium hydroxide is 10% of the mass of calcium hydroxide.
3. The method for preparing a carbon nine petroleum resin according to claim 1, characterized in that: The mass of the hydroxy compound is m1, which is 15% of the total mass of the product C9 petroleum resin; The total mass of the second olefin is m2, m2= m1 / 0.15-m1; the second olefin includes methyl styrene added in the alkylation reaction, methyl styrene added in the copolymerization reaction, and the components and styrene in the carbon nine fraction participating in the copolymerization reaction; The mass of the components participating in the copolymerization reaction contained in the carbon nine fraction is m3, m3 = m2 × (40% to 60%); The mass of the Lewis acid catalyst added to the alkylation reaction is 0.1 to 0.2% of the total mass of the hydroxy compound and methylstyrene added to the alkylation reaction; The mass of the Lewis acid catalyst added to the copolymerization reaction is 0.1 to 0.2% of the total mass of the components participating in the copolymerization reaction in the carbon nine fraction added to the copolymerization reaction, methylstyrene and styrene.
4. The method for preparing a carbon nine petroleum resin according to claim 1, characterized in that: After the copolymerization reaction, the mixture was filtered to remove impurities and distilled at 220°C.
5. A carbon nine petroleum resin, characterized in that: The invention is prepared by the preparation method of the carbon nine petroleum resin according to any one of claims 1 to 4.
Citation Information
Patent Citations
Water-soluble carbon pellet petroleum resin
CN1091751A
C9 liquid petroleum resin and preparation method thereof
CN112646076A