A kind of blue-veined gold-spotted glaze and preparation method thereof

Through the one-time glazing preparation method of blue-grained gold-dappled glaze, using a specific proportion of glaze and firing process, the problem of complex ceramic glaze preparation process and low yield rate is solved, and energy-saving and efficient ceramic preparation is achieved. Smooth and wear-resistant, improving market competitiveness.

CN116589186BActive Publication Date: 2024-10-25SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310536384.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-10-25
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

The existing ceramic glaze preparation process is complex, the yield is low, and the kiln transformation mechanism is uncertain, resulting in a waste of mineral resources, and the artistic effect of the gold spot pattern is difficult to control.

Method used

A one-time glazing method is used to prepare the blue-grained gold-dappled glaze, through a combination of specific proportions of feldspar, quartz, kaolin, cobalt black, iron oxide, sodium tripolyphosphate and sodium carboxymethyl cellulose, combined with oxidation flame and reduction Flame firing, lowering the firing temperature, controlling the size of the spots and the smoothness of the glaze.

Benefits of technology

It achieves energy-saving and efficient preparation of artistic ceramics. The glaze surface is smooth and wear-resistant, the yield is improved, and the market competitiveness is enhanced. The cumbersome problem of two-stage glazing is avoided, and the stability of the process and the quality of the finished product are controllable.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a blue-veined gold-spotted glaze and a preparation method thereof, comprising the following steps: (1) preparing a glaze; wherein, by weight, the glaze comprises: 20-40 parts of feldspar, 10-21 parts of quartz, 10-30 parts of kaolin, 1-4 parts of cobalt black, 6-10 parts of iron oxide, 0.2-0.8 parts of sodium tripolyphosphate, and 0.5-1.5 parts of sodium carboxymethyl cellulose; (2) dipping a bisque-fired body in the glaze and then drying it; (3) firing the dried body in step (2) at 25°C-900°C using an oxidizing flame and at 900°C-1280°C using a reducing flame to obtain a blue-veined gold-spotted glaze. The present invention adopts one-time glazing, reduces the firing temperature of the glaze, effectively saves the firing time of the product, and makes the preparation process of the artistic ceramics energy-saving and efficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic production, and in particular relates to a blue-veined gold-spotted glaze and a preparation method thereof. Background Art

[0002] Traditional ceramics are widely used in people's lives, and people's aesthetic needs are constantly growing. Glazes that have a decorative effect on daily-use porcelain and artistic porcelain have become the key to solving this problem.

[0003] CN103224411A discloses a method for preparing a tiger skin glaze, which requires two glazings of base glaze and top glaze, and has a complex process and high requirements on the accuracy of the instrument; the base glaze prepared by the tiger skin glaze formula is white, and the yellow glaze pattern is dim, which needs further improvement to meet market demand. CN106396385A discloses a method for preparing a tiger skin glaze, which is a kiln-changing mechanism, with gold spots distributed on black and dark brown. The uncertainty of kiln changing is large, and the artistic effect of the gold spots cannot be controlled, so the yield is not high, which wastes mineral resources to a certain extent. CN102442841B discloses a method for preparing a leopard glaze, which is an artistic glaze with a circle-shaped brown ring on the surface of the yellow base glaze, and the artistic effect is different from the gold spot glaze. Summary of the invention

[0004] In order to solve the above-mentioned problems of the prior art, the present invention provides a blue-veined gold-spotted glaze and a preparation method thereof, which adopts one-time glazing and reduces the firing temperature of the glaze, effectively saving the product firing time and making the preparation process of artistic ceramics energy-saving and efficient.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for preparing a blue-veined gold-spotted glaze comprises the following steps:

[0007] (1) preparing a glaze; wherein the glaze comprises, by weight, 20-40 parts of feldspar, 10-21 parts of quartz, 10-30 parts of kaolin, 1-4 parts of cobalt black, 6-10 parts of iron oxide, 0.2-0.8 parts of sodium tripolyphosphate, and 0.5-1.5 parts of sodium carboxymethyl cellulose;

[0008] (2) dipping the fired body into the glaze and then drying it;

[0009] (3) The green body dried in step (2) is fired at 25° C.-900° C. using an oxidizing flame, and at 900° C.-1280° C. using a reducing flame to obtain a blue-veined gold-spotted glaze.

[0010] Preferably, step (1) is specifically as follows: feldspar, quartz, kaolin, cobalt black, iron oxide, sodium tripolyphosphate and sodium carboxymethyl cellulose are mixed with ball stone, and water is added, wet ball milled, and then sieved to obtain a glaze.

[0011] Furthermore, the ball milling time is 30-40 min.

[0012] Furthermore, the sieving is specifically sieving with 80-mesh and 150-mesh sieves.

[0013] Preferably, step (2) specifically comprises: dipping the bisque-fired body into the glaze so that the glaze thickness is 1-3 mm, and then drying.

[0014] Furthermore, in step (3), the firing system is: heating from room temperature to 300°C at a heating rate of 5°C / min, then heating to 900°C at a heating rate of 3°C / min, then heating to 1280°C at a heating rate of 1.5°C / min, and keeping at 1280°C for 30 minutes.

[0015] Furthermore, in step (3), the firing is carried out at 900°C-1280°C using a reducing flame, specifically: when the temperature rises to 900°C, 300 parts to 600 parts of charcoal are added into the firing furnace for firing.

[0016] The blue-veined gold-spotted glaze is obtained by the preparation method.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The glaze formula of the blue-veined gold-spotted glaze of the present invention includes feldspar, quartz, kaolin, cobalt black, iron oxide, sodium tripolyphosphate, sodium carboxymethyl cellulose, and a specific ratio is defined to obtain the blue-veined gold-spotted glaze. Cobalt oxide and iron oxide are added as colorants to form the blue-veined gold-spotted glaze. The addition of cobalt ions makes the glaze surface show blue. Iron oxide, quartz and feldspar are sintered at high temperature to generate reddish-brown snowflake-shaped hematite crystals and yellow dendrites of calcium magnesium iron silicon. The crystals precipitate from the blue glaze surface like golden flowers on the glaze surface. This gold-spotted glaze can adjust the size of the pattern by adjusting the iron oxide content. Quartz and feldspar form pyroxene crystals that are neatly arranged and interwoven during calcination, which effectively enhances the structural stability and wear resistance of the blue-veined gold-spotted glaze. Feldspar and more kaolin are not only conducive to crystal formation, but also reduce the firing temperature of the glaze, effectively saving the firing time of the product, and making the preparation process of artistic ceramics energy-saving and efficient. The present invention uses sodium tripolyphosphate and sodium carboxymethyl cellulose to adjust the slurry viscosity to control the glazing thickness, and the iron-based crystallization glaze surface requires a thicker glaze layer. The blue-veined gold-spotted glaze of the present invention is an iron-based crystallization glaze that is glazed and fired once, which effectively avoids the problems of low yield and complicated process caused by the current two-stage glazing and firing. The glaze surface of high-temperature crystallization has high bonding, smooth and wear-resistant glaze surface, stable mechanical properties, and high market competitiveness. DETAILED DESCRIPTION

[0019] In order to further understand the present invention, the present invention is described below in conjunction with embodiments. These descriptions are only to further explain the features and advantages of the present invention and are not intended to limit the claims of the present invention.

[0020] The blue-veined gold-spotted glaze of the present invention comprises, by weight, 20-40 parts of feldspar, 10-21 parts of quartz, 10-30 parts of kaolin, 1-4 parts of cobalt black, 6-10 parts of iron oxide, 0.2-0.8 parts of sodium tripolyphosphate, and 0.5-1.5 parts of sodium carboxymethyl cellulose. The blue-veined gold-spotted glaze fired by this glaze formula is dark blue in color as a whole, and rose-shaped golden spots are distributed on the glaze surface. The blue glaze surface is a glass phase, and the golden spots are caused by the yellow dendrites precipitated on the glaze surface and the red-brown snowflake-shaped crystals. The size of the spots can be controlled according to the precise raw material ratio and the thickness of the glaze layer. At the same time, the firing of the blue-veined gold-spotted glaze needs to ensure a strict firing system. The present invention details the firing temperature control information of the flower glaze, and provides a guarantee for the batch and industrial production of the blue-veined gold-spotted artistic flower glaze, so that it can reduce costs and increase efficiency, and has market competitiveness.

[0021] The preparation process of the blue-veined gold-spotted glaze specifically comprises the following steps:

[0022] (1) The raw materials are mixed with 200 parts of ball stones of different particle sizes, and water is added for wet ball milling for 30-40 minutes, the rotation speed is maintained at 300r / min, and the material ratio during wet ball milling is ensured to be ball stone: water: raw material = 200g: 70ml: 100g. When the glaze concentration (solid content) reaches 60%, sieve with 80 mesh and 150 mesh sieves to obtain a glaze with uniform and fine texture of blue-veined gold-spotted glaze.

[0023] (2) Dip the fired body in glaze for 5-15 seconds, ensuring that the glaze thickness reaches 1-3 mm, and then dry it at room temperature overnight.

[0024] (3) The firing system of the blue-veined gold-spotted glaze is: 25℃-300℃, heating rate 5℃ / min; 300℃-900℃, heating rate 3℃ / min; 900℃-1280℃, heating rate 1.5℃ / min, heating to 1280℃ and keeping warm for 30 minutes, and cooling down to room temperature with the furnace after firing. The firing of the blue-veined gold-spotted glaze must be carried out in a reducing atmosphere, specifically using an oxidizing flame at 25℃-900℃. The high-temperature firing of the glaze uses a reducing flame. When the temperature in the furnace is 900℃, the plug must be pulled out and 300g-600g of charcoal must be added to ensure the firing of the reducing flame.

[0025] The present invention uses quartz, feldspar and kaolin as main raw materials. The silicon dioxide in feldspar and quartz plays a skeleton role in the blue-veined gold-spotted glaze, mainly increasing the glossiness of the glaze. The magnesium oxide contained in more feldspar not only reduces the sintering temperature of the glaze, but also provides conditions for the formation of magnesium-iron pyroxene crystalline glaze. The aluminum oxide introduced by kaolin forms aluminum oxide octahedron in the glaze, and forms a glaze skeleton with silicon oxide tetrahedron, thereby improving the adhesion and wear resistance of the glaze. Sodium tripolyphosphate and sodium hydroxymethyl cellulose adjust the viscosity of the slurry for easy glazing. Cobalt black and iron oxide as colorants can effectively control the glaze color and the size of the pattern, thereby ensuring the preparation of the blue-veined gold-spotted glaze. The glaze is fired in a reducing atmosphere, which is conducive to the decomposition and precipitation of iron oxide, thereby preparing a smooth golden diopside glaze.

[0026] Example 1

[0027] A raw material formula for a blue-veined gold-spotted glaze: 8g iron oxide, 3g cobalt black, 35g feldspar, 27g kaolin, 21g quartz, 0.5g sodium tripolyphosphate, and 0.8g sodium carboxymethyl cellulose.

[0028] The preparation process of the blue-veined gold-spotted glaze specifically comprises the following steps:

[0029] (1) The raw materials are mixed with 200 g of ball stones of different particle sizes, and 70 mL of water is added for wet ball milling for 40 min. The rotation speed is maintained at 300 r / min. During wet ball milling, the material ratio is ensured to be ball stone: raw material: water = 200 g: 95.3 g: 70 mL. The glaze concentration reaches 60%. Sieve with 80 mesh and 150 mesh sieves to obtain a glaze with uniform and fine texture of blue-veined gold-spotted glaze.

[0030] (2) Dip the fired body in glaze for 10 seconds, ensuring that the glaze thickness reaches 2 mm, and then dry it at room temperature overnight.

[0031] (3) The firing system of the blue-veined gold-spotted glaze is: 25℃-300℃, heating rate 5℃ / min; 300℃-900℃, heating rate 3℃ / min; 900℃-1280℃, heating rate 1.5℃ / min, heating to 1280℃ and keeping warm for 30 minutes, and cooling down to room temperature with the furnace after firing. The firing of the blue-veined gold-spotted glaze must be carried out in a reducing atmosphere, specifically using an oxidizing flame at 25℃-900℃, and the high-temperature firing of the glaze uses a reducing flame. When the temperature in the furnace is 900℃, the plug must be pulled out and 400g of charcoal must be added to ensure the firing of the reducing flame.

[0032] A higher concentration of cobalt black is added to the raw materials and fired in a reducing atmosphere, resulting in a blue-black glaze. The glaze is smooth, crystal clear, and bright in color. It has different artistic effects when combined with the precipitated yellow dendrite diopside. The cobalt oxide in the glass phase is stably present in the silica skeleton, ensuring that the ceramic products are safe and stable when used. Accurate raw material ratios and specific firing processes are prerequisites for the formation of blue-veined gold-spotted glazes. Reasonable modification formulas within the allowable range will have slightly different effects based on the glaze color.

[0033] Example 2

[0034] A raw material formula for a blue-veined gold-spotted glaze: 6g iron oxide, 2g cobalt black, 40g feldspar, 30g kaolin, 21g quartz, 0.5g sodium tripolyphosphate, and 0.8g sodium carboxymethyl cellulose.

[0035] The preparation process of the blue-veined gold-spotted glaze specifically comprises the following steps:

[0036] (1) The raw materials are mixed with 200 g of ball stones of different particle sizes, and 70 mL of water is added for wet ball milling for 40 min. The rotation speed is maintained at 300 r / min. During wet ball milling, the material ratio is ensured to be ball stone: raw material: water = 200 g: 101.3 g: 70 mL. The glaze concentration reaches 60%. Sieve with 80 mesh and 150 mesh sieves to obtain a glaze with uniform and fine texture of blue-veined gold-spotted glaze.

[0037] (2) Dip the fired body in glaze for 10 seconds, ensuring that the glaze thickness reaches 2 mm, and then dry it at room temperature overnight.

[0038] (3) The firing system of the blue-veined gold-spotted glaze is: 25℃-300℃, heating rate 5℃ / min; 300℃-900℃, heating rate 3℃ / min; 900℃-1280℃, heating rate 1.5℃ / min, heating to 1280℃ and keeping warm for 30 minutes, and cooling down to room temperature with the furnace after firing. The firing of the blue-veined gold-spotted glaze must be carried out in a reducing atmosphere, specifically using an oxidizing flame at 25℃-900℃, and the high-temperature firing of the glaze uses a reducing flame. When the temperature in the furnace is 900℃, the plug must be pulled out and 400g of charcoal must be added to ensure the firing of the reducing flame.

[0039] Example 3

[0040] A raw material formula for a blue-veined gold-spotted glaze: 7g iron oxide, 2g cobalt black, 35g feldspar, 30g kaolin, 16g quartz, 0.8g sodium tripolyphosphate, and 1g sodium carboxymethyl cellulose.

[0041] The preparation process of the blue-veined gold-spotted glaze specifically comprises the following steps:

[0042] (1) The raw materials are mixed with 200 g of ball stones of different particle sizes, and 70 mL of water is added for wet ball milling for 30 min. The rotation speed is maintained at 300 r / min. During wet ball milling, the material ratio is ensured to be ball stone: raw material: water = 200 g: 91.8 g: 70 mL. The glaze concentration reaches 60%. Sieve with 80 mesh and 150 mesh sieves to obtain a glaze with uniform and fine texture of blue-veined gold-spotted glaze.

[0043] (2) Dip the fired body in glaze for 10 seconds, ensuring that the glaze thickness reaches 2 mm, and then dry it at room temperature overnight.

[0044] (3) The firing system of the blue-veined gold-spotted glaze is: 25℃-300℃, heating rate 5℃ / min; 300℃-900℃, heating rate 3℃ / min; 900℃-1280℃, heating rate 1.5℃ / min, heating to 1280℃ and keeping warm for 30 minutes, and cooling down to room temperature with the furnace after firing. The firing of the blue-veined gold-spotted glaze must be carried out in a reducing atmosphere, specifically using an oxidizing flame at 25℃-900℃, and the high-temperature firing of the glaze uses a reducing flame. When the temperature in the furnace is 900℃, the plug must be pulled out and 400g of charcoal must be added to ensure the firing of the reducing flame.

[0045] Comparative Example 1

[0046] The raw material formula of the blue-veined gold-spotted glaze in this comparative example is: 8g iron oxide, 3g cobalt black, 35g feldspar, 27g kaolin, and 21g quartz.

[0047] The preparation process of the blue-veined gold-spotted glaze specifically comprises the following steps:

[0048] (1) Mix the raw materials with 200g of ball stones of different particle sizes, add 70mL of water and wet-mill for 40min, keep the speed at 300r / min, and ensure the material ratio during wet-milling is ball stone: raw material: water = 200g: 94g: 70mL. When the glaze concentration reaches 60%, sieve with 80-mesh and 150-mesh sieves to obtain a glaze with uniform and fine texture of blue-veined gold-spotted glaze.

[0049] (2) Dip the fired body in glaze for 10 seconds. After the glaze thickness reaches 2 mm, dry it at room temperature overnight.

[0050] (3) The firing system of the blue-veined gold-spotted glaze is: 25℃-300℃, heating rate 5℃ / min; 300℃-900℃, heating rate 3℃ / min; 900℃-1280℃, heating rate 1.5℃ / min, heating to 1280℃ and keeping warm for 30min. After the firing is completed, the temperature is cooled down to room temperature with the furnace. The firing of the blue-veined gold-spotted glaze must be carried out in a reducing atmosphere, specifically using an oxidizing flame at 25℃-900℃. The high-temperature firing of the glaze uses a reducing flame. When the temperature in the furnace is 900℃, the plug must be pulled out and 500g of charcoal must be added to ensure the firing of the reducing flame.

[0051] Sodium tripolyphosphate and sodium carboxymethyl cellulose are added to the glaze slurry of the aqueous solvent as inorganic surfactants and emulsifiers to make the viscosity controllable and the slurry suspension stable. In this comparative example, no viscosity regulator is added. After the slurry is left to stand, the water and raw materials are separated into distinct layers. After sufficient stirring, the thickness distribution after glazing is uneven. The fired blue glaze surface and yellow crystallization are messy, and the bubbles in the glaze are obvious, which cannot be used normally.

[0052] Comparative Example 2

[0053] The raw material formula of the blue-veined gold-spotted glaze of this comparative example is as follows: 35g of feldspar, 27g of kaolin, 21g of quartz, 10g of iron oxide, 3g of cobalt black, 0.5g of sodium tripolyphosphate, and 0.8g of sodium carboxymethyl cellulose.

[0054] The preparation process of the blue-veined gold-spotted glaze specifically comprises the following steps:

[0055] (1) The raw materials are mixed with 200 g of ball stones of different particle sizes, and 70 mL of water is added for wet ball milling for 35 min, with the rotation speed maintained at 300 r / min. During wet ball milling, the material ratio is ensured to be ball stone: raw material: water = 200 g: 97.3 g: 70 mL. The glaze concentration reaches 60%, and sieves are sieved with 80 mesh and 150 mesh to obtain a glaze with uniform and fine texture of blue-veined gold-spotted glaze.

[0056] (2) Dip the fired body in glaze for 10 seconds. After the glaze thickness reaches 2 mm, dry it at room temperature overnight.

[0057] (3) The firing system of the blue-veined gold-spotted glaze is: 25℃-300℃, heating rate 5℃ / min; 300℃-900℃, heating rate 3℃ / min; 900℃-1280℃, heating rate 1.5℃ / min, heating to 1280℃ and keeping warm for 30min, after firing, cooling down to room temperature with the furnace. The firing of the blue-veined gold-spotted glaze must be carried out in a reducing atmosphere, specifically using an oxidizing flame at 25℃-900℃, and the high-temperature firing of the glaze uses a reducing flame. When the temperature in the furnace is 900℃, the plug must be pulled out and 400g of charcoal must be added to ensure the firing of the reducing flame.

[0058] Adjusting the raw material ratio requires adjusting the reducing atmosphere in the kiln, which can be controlled by adding a reasonable amount of charcoal. When the iron oxide concentration is high, the amount of charcoal added must be changed accordingly. In this experiment, the iron oxide content was relatively high, but the amount of charcoal added did not change. The amount of crystallization on the fired glaze was large, making the glaze appear brown-yellow all over, and losing the effect of the blue-veined gold-spotted glaze.

[0059] Comparative Example 3

[0060] The raw material formula of the blue-veined gold-spotted glaze of this comparative example is as follows: 8g of iron oxide, 3g of cobalt black, 35g of feldspar, 27g of kaolin, 21g of quartz, 0.5g of sodium tripolyphosphate, and 0.8g of sodium carboxymethyl cellulose.

[0061] The preparation process of the blue-veined gold-spotted glaze specifically comprises the following steps:

[0062] (1) The raw materials are mixed with 200 g of ball stones of different particle sizes, and 70 mL of water is added for wet ball milling for 40 min, with the rotation speed maintained at 300 r / min. During wet ball milling, the material ratio is ensured to be ball stone: raw material: water = 200 g: 95.3 g: 70 mL. The glaze concentration reaches 60%, and sieves are sieved with 80 mesh and 150 mesh to obtain a glaze with uniform and fine texture of blue-veined gold-spotted glaze.

[0063] (2) Dip the fired body in glaze for 10 seconds. After the glaze thickness reaches 2 mm, dry it at room temperature overnight.

[0064] (3) The firing system of the blue-veined gold-spotted glaze is: 25℃-300℃, heating rate 5℃ / min; 300℃-900℃, heating rate 3℃ / min; 900℃-1280℃, heating rate 1.5℃ / min, heating to 1280℃ and keeping warm for 30min, and cooling down to room temperature with the furnace after firing. The firing of the blue-veined gold-spotted glaze is carried out in an oxidizing atmosphere. After the glazed body is dried, it is directly fired in the kiln. An oxidizing flame is used at 25℃-1280℃, and no reducing materials such as charcoal are added to change the atmosphere.

[0065] The color of iron oxide in ceramic glaze is rich in color due to the changeable kiln atmosphere. In this experiment, red iron oxide is used as the raw material. The continuous combustion of oxygen in the kiln makes the crystallization glaze with high iron content appear brown, and cobalt oxide appears cyan. The two colors are similar, which makes the glaze lose its special color and cannot be used. This shows that the firing process mentioned in the present invention must be carried out in a reducing atmosphere. The high-temperature complete combustion of charcoal causes the iron oxide to continue to melt and decompose the iron element, which reacts with other raw materials to form smooth and shiny ferromagnesian diopside crystals, making the glaze appear dazzling golden yellow.

Claims

1. A method for preparing a blue-veined gold-spotted glaze, characterized in that: The following steps are involved: (1) preparing a glaze; wherein the glaze comprises, by weight, 20-40 parts of feldspar, 10-21 parts of quartz, 10-30 parts of kaolin, 1-4 parts of cobalt black, 6-10 parts of iron oxide, 0.2-0.8 parts of sodium tripolyphosphate, and 0.5-1.5 parts of sodium carboxymethyl cellulose; (2) dipping the bisque-fired body into the glaze and then drying it; (3) firing the green body dried in step (2) at 25°C-900°C using an oxidizing flame and at 900°C-1280°C using a reducing flame to obtain a blue-veined gold-spotted glaze; In step (3), the firing is carried out at 900°C-1280°C using a reducing flame. Specifically, when the temperature rises to 900°C, 300 parts to 600 parts of charcoal are added into the firing furnace for firing.

2. The method for preparing the blue-veined gold-spotted glaze according to claim 1, characterized in that: Step (1) specifically comprises: mixing feldspar, quartz, kaolin, cobalt black, iron oxide, sodium tripolyphosphate and sodium carboxymethyl cellulose with ball stone, adding water, wet ball milling, and then sieving to obtain a glaze.

3. The method for preparing the blue-veined gold-spotted glaze according to claim 2, characterized in that: The ball milling time is 30-40min.

4. The method for preparing the blue-veined gold-spotted glaze according to claim 2, characterized in that: The sieving is specifically performed using 80-mesh and 150-mesh sieves.

5. The method for preparing the blue-veined gold-spotted glaze according to claim 1, characterized in that: Step (2) specifically comprises: dipping the bisque-fired body into the glaze so that the glaze thickness is 1-3 mm, and then drying.

6. The method for preparing the blue-veined gold-spotted glaze according to claim 1, characterized in that: In step (3), the firing system is as follows: heating from room temperature to 300°C at a heating rate of 5°C / min, then heating to 900°C at a heating rate of 3°C / min, then heating to 1280°C at a heating rate of 1.5°C / min, and keeping at 1280°C for 30 minutes.

7. The blue-veined gold-spotted glaze obtained by the preparation method according to any one of claims 1 to 6.