Filters and camera devices
By using a resin film containing Si, Ti, Zr, and Al in the filter and combining it with a phosphate-based or fluorophosphate-based glass substrate, the problem of insufficient adhesion is solved, achieving higher adhesion and mechanical strength, which meets the requirements of thinness and high oblique incidence in modern digital cameras.
Patent Information
- Application Number
- CN202310474382.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-29
- Filing Date
- 2019-06-04
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2039-06-04
AI Technical Summary
In the prior art, the adhesion between phosphate-based glass or fluorophosphate-based glass and the absorbent resin membrane is insufficient, especially in the presence of moisture, which can easily lead to problems and affect the performance of the filter.
A single-layer or multi-layer filter is formed by depositing a resin film containing one or more of Si, Ti, Zr and Al atoms on an absorbing glass substrate and improving the adhesion by using a specific coupling agent and a dehydration condensate of silanol.
It improves the adhesion between phosphate-based or fluorophosphate-based glass and the resin film, enhances the performance stability and mechanical strength of the filter, and meets higher requirements for oblique incidence optics.
Smart Images

Figure CN116594093B_ABST
Abstract
Description
[0001] This application is a divisional application of the application filed on June 4, 2019, with application number 201910480142.5 and entitled "Filter and Camera Device". Technical Field
[0002] This invention relates to filters and imaging devices. Background Technology
[0003] In imaging devices that use solid-state imaging devices such as CCD and CMOS image sensors, such as digital still cameras (DSC) and digital single-lens reflex cameras, in order to reproduce tones well and obtain clear images, a device called an infrared cut-off filter (IRCF) is used, which transmits visible light and blocks ultraviolet and near-infrared light (for example, see Patent Document 1 (Japanese Patent Application Publication No. 2014-148567)).
[0004] Figure 1 This is a schematic diagram illustrating the camera module that makes up the DSC. Figure 1 (a) is a schematic diagram illustrating the camera module of a small digital camera installed in a smartphone or similar device. Figure 1 (b) is a schematic diagram illustrating the camera module of a digital single-lens reflex camera.
[0005] exist Figure 1 In the camera module shown in (a), the ultraviolet and near-infrared light in the transmitted light from the lens L are selectively reflected by the infrared cut-off filter (IRCF) 1, and only the visible light region, which conforms to human visibility characteristics, is selectively introduced into the module and captured into the image sensor IC. Furthermore, in Figure 1 Similarly, in the camera module shown in (b), ultraviolet and near-infrared light in the transmitted light from the lens L are selectively reflected by the infrared cut-off filter (IRCF) 1, and alpha rays are removed by the cover glass CG while suppressing the intrusion of dust. Only the light in the visible light region that conforms to human visibility characteristics is selectively introduced into the module and taken into the image sensor IC.
[0006] Moreover, the mainstream approach for infrared cut-off filters (IRCFs) is to place a reflective film (UVIR film) on the upper surface side (light incident surface side) of the glass substrate and an anti-reflective film (aR film) on the lower surface side (light emitting surface side) of the glass substrate.
[0007] Figure 2 (a) is a schematic diagram illustrating the structure of a conventional infrared cutoff filter (IRCF) 1. Figure 2In the infrared cut-off filter (IRCF) 1 shown in (a), a reflective film (UVIR film) 2 is provided on the upper surface side (light incident surface side) of the glass substrate 3, and an anti-reflective film (aR film) 4 is provided on the lower surface side (light emitting surface side) of the glass substrate 3. The reflective film 2 selectively reflects ultraviolet and near-infrared light from the light incident from above, allowing only the visible light region that conforms to human visibility characteristics to pass through the glass substrate 3 and the anti-reflective film (aR film) 4, and to exit from the lower part of the anti-reflective film (aR film) 4.
[0008] However, for digital cameras, with the increasing demand for thinner designs, various components are also becoming smaller and thinner, and image sensors are being optically designed with a more oblique light incidence. On the other hand, for the aforementioned reflective infrared cut-off filter (IRCF), due to the high wavelength dependence of light, if the incident angle of light increases, a phase shift occurs, causing the cut-off frequency to deviate from the shorter wavelength side. The incident angle of the light incident on the infrared cut-off filter (IRCF) differs for light passing near the center of the lens and light passing through the periphery, thus making it easier for a decrease in color reproducibility to occur due to interference shift.
[0009] Therefore, as an infrared cut-off filter (IRCF), a hybrid infrared cut-off filter (IRCF) was studied, which not only has a reflective film (UVIR film), but also separately has an absorbing resin film, or uses a light-absorbing substrate (absorbing glass substrate) as a glass substrate, thereby reducing the burden on the reflective film (UVIR film), more effectively reducing ultraviolet and near-infrared light in the incident light, and can exert excellent oblique incidence characteristics.
[0010] Figure 2 (b) is a schematic diagram illustrating a structural example of the hybrid infrared cut-off filter (IRCF) 1 described above. Figure 2 (b) In the infrared cut-off filter (IRCF) 1 shown, a reflective film (UVIR film) 2 is provided on the upper surface side (light incident surface side) of the absorbing glass substrate 3' that absorbs at least one of ultraviolet light and near-infrared light, and an absorbing resin film 5 and an anti-reflective film (AR film) 4 are further provided sequentially on the lower surface side (light emitting surface side) of the absorbing glass substrate 3'. By using the above-mentioned reflective film (UVIR film) 2, absorbing glass substrate 3' and absorbing resin film 5 in combination, ultraviolet light and near-infrared light in the incident light are reduced more effectively, and a structure is formed that allows only the light in the visible light region to pass through and be emitted downward under high oblique incidence characteristics.
[0011] Existing technical documents
[0012] Patent documents
[0013] Patent Document 1: Japanese Patent Application Publication No. 2014-148567 Summary of the Invention
[0014] The problem that the invention aims to solve
[0015] However, during their research, the inventors discovered that phosphate-based glasses such as phosphate glass or fluorophosphate glass are typically used as the constituent material of the aforementioned absorbing glass substrate for absorbing ultraviolet or near-infrared light. On the other hand, organic materials containing various polymers are used as the constituent material of the aforementioned absorbing resin film, but the adhesion between the two is not necessarily sufficient, especially when moisture is present.
[0016] Under such circumstances, the object of the present invention is to provide a filter having a resin film having high adhesion to an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass, and to provide an imaging device having the above-mentioned filter.
[0017] Problem Solving Methods
[0018] In order to achieve the above objectives, the inventors conducted in-depth research and discovered that by using a resin film containing one or more bonding components selected from Si atoms, Ti atoms, Zr atoms and Al atoms to form an absorption glass substrate made of phosphate-based glass or fluorophosphate-based glass, the above technical problems can be solved, and the present invention was completed based on this discovery.
[0019] That is, the present invention provides the following content.
[0020] (1) A filter (hereinafter appropriately referred to as the filter 1 of the present invention) is formed by depositing a resin film on an absorbing glass substrate made of phosphate glass or fluorophosphate glass through a bonding layer, wherein the bonding layer contains Si atoms and one or more selected from Ti atoms, Zr atoms and Al atoms, and has a single-layer structure.
[0021] (2) In the above-mentioned filter (1), the total number of Ti atoms, Zr atoms and Al atoms in the above-mentioned bonding layer accounts for a proportion greater than 0 atomic% and less than 33.3 atomic% in the total number of Si atoms, Ti atoms, Zr atoms and Al atoms.
[0022] (3) The filter described in (1) or (2) above (hereinafter appropriately referred to as the filter 1-1 of the present invention) is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer contains a hydrolysis and dehydration condensate of one or more coupling agents selected from the compounds represented by general formula (I) and the compounds represented by general formula (II) below.
[0023] M(OSiR 1 R 2 R 3 ) n (I)
[0024] In formula (I), M is a Ti atom, Zr atom, or Al atom, and R 1 R 2 and R 3 The hydrocarbon group is a straight-chain or branched hydrocarbon group containing 1 to 10 carbon atoms, which may be the same or different. n is 4 when M is a Ti or Zr atom, and 3 when M is an Al atom. Multiple -OSiR groups are also present. 1 R 2 R 3 The bases can be the same or different.
[0025] (Ti k O k-1 (OSiR) 4 R 5 R 6 ) 2k+2 (II)
[0026] In equation (II), R 4 R 5 and R 6 The hydrocarbon group consisting of 1 to 10 carbon atoms (either linear or branched) containing oxygen or nitrogen atoms, and these carbon atoms may be the same or different; k is a real number of 2 or more and less than 15; and multiple -OSiR groups are allowed. 4 R 5 R 6 The bases can be the same or different.
[0027] (4) The filter described in any one of (1) to (3) above (hereinafter appropriately referred to as the filter 1-2 of the present invention) is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer comprises a hydrolysis and dehydration condensate of one or more coupling agents selected from the compounds represented by general formula (III) and the compounds represented by general formula (IV) below.
[0028] M{OSi(OR 7 (OR) 8 (OR) 9 )} n (III)
[0029] In formula (III), M is a Ti atom, a Zr atom, or an Al atom, and R 7 R 8 and R 9It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different; n is 4 when M is a Ti atom or a Zr atom, and 3 when M is an Al atom; multiple -OSi(OR) groups. 7 (OR) 8 (OR) 9 The bases can be the same or different.
[0030] (Ti k O k-1 ){OSi(OR 10 (OR) 11 (OR) 12 )} 2k+2 (IV)
[0031] In equation (IV), R 10 R 11 and R 12 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSi(OR) groups. 10 (OR) 11 (OR) 12 The bases can be the same or different.
[0032] (5) The filter described in (4) above, wherein the coupling agent represented by general formula (III) is a silicon compound represented by general formula (V) and a reactant selected from one or more metal alkoxides represented by general formula (VI), general formula (VII) and general formula (VIII).
[0033] Si(OR 7 (OR) 8 (OR) 9 )OH(V)
[0034] In equation (V), R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0035] Ti(OR 13 (OR) 14 (OR) 15 (OR) 16 (VI)
[0036] In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0037] Zr(OR 17 (OR) 18 (OR) 19 (OR) 20 (VII)
[0038] In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0039] Al(OR 21 (OR) 22 (OR) 23 (VIII)
[0040] In equation (VIII), R 21 R 22 and R 23 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
[0041] (6) The filter according to any one of (1) to (5) above, wherein the bonding layer further comprises a dehydrated condensate of silanol.
[0042] (7) The filter described in any one of (1) to (6) above is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer comprises a hydrolyzed and dehydrated condensate of a coupling agent composition, the coupling agent composition comprising 50 mol% or more and less than 100 mol% of a silicon compound represented by the following general formula (V), and more than 0 mol% and less than 50 mol% of one or more reactants selected from the following general formulas (VI), (VII) and (VIII).
[0043] Si(OR 7 (OR) 8 (OR) 9 )OH(V)
[0044] In equation (V), R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0045] Ti(OR 13 (OR) 14 (OR) 15 (OR) 16 (VI)
[0046] In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0047] Zr(OR 17 (OR) 18 (OR) 19 (OR) 20 (VII)
[0048] In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0049] Al(OR 21 (OR) 22 (OR) 23 (VIII)
[0050] In equation (VIII), R 21 R 22 and R 23 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
[0051] (8) The filter described in (7) above, wherein the coupling agent composition is a silicon compound represented by the above general formula (V) with a molar percentage greater than 80 mol% and less than 100 mol% and a reactant of one or more metal alkoxides selected from the above general formulas (VI) to (VIII) with a molar percentage greater than 0 mol% and less than 20 mol%.
[0052] (9) The filter described in (7) above, wherein the coupling agent composition is 85 to 94 mol% of a silicon compound represented by the above general formula (V) and 6 to 15 mol% of a reaction product of one or more metal alkoxides selected from the above general formulas (VI) to (VIII).
[0053] (10) A filter (hereinafter appropriately referred to as the filter 2 of the present invention) is formed by depositing a resin film on an absorbing glass substrate made of phosphate glass or fluorophosphate glass, said resin film comprising Si atoms and one or more selected from Ti atoms, Zr atoms and Al atoms.
[0054] (11) The filter described in (10) above, wherein in the resin film, the total number of Ti atoms, Zr atoms and Al atoms accounts for a proportion greater than 0 atomic% and less than 33.3 atomic% in the total number of Si atoms, Ti atoms, Zr atoms and Al atoms.
[0055] (12) The filter described in (10) or (11) above (hereinafter appropriately referred to as the filter 2-1 of the present invention) is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer comprises a hydrolysis and dehydration condensate of one or more coupling agents selected from the compounds represented by general formula (I) and the compounds represented by general formula (II) below.
[0056] M(OSiR 1 R 2 R 3 ) n (I)
[0057] In formula (I), M is a Ti atom, Zr atom, or Al atom, and R 1 R 2 and R 3 The hydrocarbon group is a straight-chain or branched hydrocarbon group containing 1 to 10 carbon atoms, which may be the same or different. n is 4 when M is a Ti or Zr atom, and 3 when M is an Al atom. Multiple -OSiR groups are also present. 1 R 2 R 3 The bases can be the same or different.
[0058] (Ti k O k-1 (OSiR) 4 R 5 R 6 ) 2k+2 (II)
[0059] In equation (II), R 4 R 5 and R 6 The hydrocarbon group consisting of 1 to 10 carbon atoms (either linear or branched) containing oxygen or nitrogen atoms, and these carbon atoms may be the same or different; k is a real number of 2 or more and less than 15; and multiple -OSiR groups are allowed. 4 R 5 R 6 The bases can be the same or different.
[0060] (13) The filter described in any one of (10) to (12) above (hereinafter appropriately referred to as the filter 2-2 of the present invention) is formed by providing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer comprises a hydrolysis and dehydration condensate of one or more coupling agents selected from the compounds represented by general formula (III) and the compounds represented by general formula (IV) below.
[0061] M{OSi(OR 7 (OR) 8 (OR) 9 )} n (III)
[0062] In formula (III), M is a Ti atom, a Zr atom, or an Al atom, and R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different; n is 4 when M is a Ti atom or a Zr atom, and 3 when M is an Al atom; multiple -OSi(OR) groups. 7 (OR) 8 (OR) 9 The bases can be the same or different.
[0063] (Ti k O k-1 ){OSi(OR 10 (OR) 11 (OR) 12 )} 2k+2 (IV)
[0064] In equation (IV), R 10 R 11 and R 12 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSi(OR) groups. 10 (OR) 11 (OR) 12 The bases can be the same or different.
[0065] (14) The filter described in (13) above, wherein the coupling agent represented by general formula (III) is a silicon compound represented by general formula (V) and a reactant selected from one or more metal alkoxides represented by general formula (VI), general formula (VII) and general formula (VIII).
[0066] Si(OR 7 (OR) 8 (OR) 9 )OH(V)
[0067] In equation (V), R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0068] Ti(OR 13 (OR) 14 (OR) 15 (OR) 16 (VI)
[0069] In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0070] Zr(OR 17 (OR) 18 (OR) 19 (OR) 20 (VII)
[0071] In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0072] Al(OR 21 (OR) 22 (OR) 23 (VIII)
[0073] In equation (VIII), R 21 R 22 and R 23 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
[0074] (15) The filter of any one of (10) to (14) above, wherein the resin film further comprises a dehydrated condensate of silanol.
[0075] (16) The filter described in any one of (10) to (15) above is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer comprises a hydrolyzed and dehydrated condensate of a coupling agent composition, the coupling agent composition comprising 50 mol% or more and less than 100 mol% of a silicon compound represented by the following general formula (V), and more than 0 mol% and less than 50 mol% of one or more reactants selected from the following general formulas (VI), (VII) and (VIII).
[0076] Si(OR 7 (OR) 8 (OR) 9 )OH(V)
[0077] In equation (V), R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0078] Ti(OR 13 (OR) 14 (OR) 15 (OR) 16 (VI)
[0079] In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0080] Zr(OR 17 (OR) 18 (OR) 19 (OR) 20 (VII)
[0081] In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0082] Al(OR 21 (OR) 22 (OR) 23 (VIII)
[0083] In equation (VIII), R 21 R 22 and R 23It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
[0084] (17) The filter described in (16) above, wherein the coupling agent composition is a reaction product of a silicon compound represented by the above general formula (V) with a molar percentage greater than 80 mol% and less than 100 mol% and one or more metal alkoxides represented by the above general formulas (VI) to (VIII) with a molar percentage greater than 0 mol% and less than 20 mol%.
[0085] (18) The filter described in (16) above, wherein the coupling agent composition is 85 to 94 mol% of a silicon compound represented by the above general formula (V) and 6 to 15 mol% of one or more metal alkoxides represented by the above general formulas (VI) to (VIII).
[0086] as well as
[0087] (19) A camera device having a solid-state camera device, a camera lens, and a filter as described in any one of (1) to (18) above.
[0088] The effects of the invention
[0089] According to the present invention, a filter having a resin film with high adhesion provided on an absorbing glass substrate made of phosphate-based glass or fluorophosphate glass can be provided, and an imaging device having the above-mentioned filter can be provided. Attached Figure Description
[0090] Figure 1 This is a schematic diagram illustrating the camera module. Figure 1 (a) is a schematic diagram illustrating the camera module of a small digital camera. Figure 1 (b) is a schematic diagram illustrating the camera module of a digital single-lens reflex camera.
[0091] Figure 2 This is a schematic diagram illustrating the structure of the infrared cut-off filter (IRCF) 1. Figure 2 (a) is a schematic diagram illustrating the reflective type of IRCF that reflects ultraviolet and near-infrared light through a reflective film (UVIR film). Figure 2 (b) is a schematic diagram of a hybrid IRCF that, in addition to a reflective film (UVIR film), also has an absorbing glass substrate that absorbs ultraviolet or near-infrared light and an absorbing resin film that absorbs ultraviolet or near-infrared light.
[0092] Figure 3 This is a cross-sectional image (image contrast) of an example of the filter of the present invention using a scanning transmission electron microscope-energy dispersive X-ray spectrometer (STEM-EDX).
[0093] Figure 4 This is a diagram showing STEM-EDX lines (EDX (K-ray) detection intensity lines of each element constituting the filter in the depth direction) in an example of the filter of the present invention.
[0094] Symbol Explanation
[0095] 1. Filter (Infrared Cut-off Filter (IRCF))
[0096] 2. Reflective film (UVIR film)
[0097] 3 Glass substrate
[0098] 3' Absorbing glass substrate
[0099] 4. Anti-reflective film (AR film)
[0100] 5 Absorbent Resin Membrane
[0101] L lens
[0102] CG Cover Glass
[0103] IC Image Sensor Detailed Implementation
[0104] The filter 1 of the present invention is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer. The bonding layer contains Si atoms and one or more selected from Ti atoms, Zr atoms and Al atoms, and has a single-layer structure. Specific examples of this invention include the filter 1-1 or the filter 1-2 of the present invention described below.
[0105] Furthermore, the filter 2 of the present invention is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass. The resin film contains Si atoms and one or more selected from Ti atoms, Zr atoms and Al atoms. As a specific example, the filter 2-1 or the filter 2-2 of the present invention described later can be cited.
[0106] The filter 1 of the present invention is formed by depositing a resin film on an absorbing glass substrate through a bonding layer having a single-layer structure containing Si atoms and one or more selected from Ti atoms, Zr atoms and Al atoms. The filter 2 of the present invention is formed by depositing a resin film containing Si atoms and one or more selected from Ti atoms, Zr atoms and Al atoms on an absorbing glass substrate. The two are the same in all aspects except for this difference.
[0107] Therefore, unless otherwise specified, the description of the filters of the present invention described below is the same as that in filter 1 and filter 2 of the present invention.
[0108] [Glass substrate]
[0109] The filter of the present invention has an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass as the glass substrate.
[0110] In the filter of the present invention, the thickness of the absorbing glass substrate is preferably 0.01 to 1.50 mm, more preferably 0.01 to 0.70 mm, and even more preferably 0.01 to 0.30 mm.
[0111] By keeping the thickness of the absorbing glass substrate within the above-mentioned range, the filter can be easily made thinner.
[0112] In the filter of the present invention, the absorbing glass substrate is made of phosphate-based glass or fluorophosphate-based glass.
[0113] The phosphate-based glass in this invention refers to glass containing P, O, and other arbitrary components as essential elements, with CuO being particularly preferred. Phosphate-based glass, by containing CuO, can more effectively absorb near-infrared light. Other arbitrary components that can be included in phosphate-based glass include, for example, Ca, Mg, Sr, Ba, Li, Na, K, and Cs.
[0114] The fluorophosphate glass of this invention refers to glass containing P, O, F, and other arbitrary components as essential elements, with CuO being particularly preferred. By containing CuO, fluorophosphate glass can more effectively absorb near-infrared light. Other arbitrary components that can be included in fluorophosphate glass include, for example, Ca, Mg, Sr, Ba, Li, Na, K, and Cs.
[0115] As the above-mentioned phosphate-based glass, it preferably contains:
[0116] P2O5 is greater than 0% by mass and less than 70% by mass.
[0117] Al2O3 0-40% by mass
[0118] BaO 0-40% by mass
[0119] CuO 0–40% by mass
[0120] The above-mentioned phosphate-based glass more preferably contains:
[0121] P2O5 20-60% by mass
[0122] Al2O3 0-10% by mass
[0123] BaO 0-10% by mass
[0124] CuO 0–10% by mass
[0125] As for the above-mentioned phosphate-based glass, it is further preferred to contain:
[0126] P2O5 20-60% by mass
[0127] Al2O3 1-10% by mass
[0128] BaO 1-10% by mass
[0129] CuO 1-10% by mass
[0130] As the above-mentioned fluorophosphate-based glass, it preferably contains:
[0131] P2O5 is greater than 0% by mass and less than 70% by mass.
[0132] Al2O3 0-40% by mass
[0133] BaO 0-40% by mass
[0134] CuO 0–40% by mass, and further containing more than 0% by mass and less than 40% by mass of fluoride.
[0135] More preferably, the glass containing the above-mentioned fluorophosphate glass includes:
[0136] P2O5 20-60% by mass
[0137] Al2O3 0-10% by mass
[0138] BaO 0-10% by mass
[0139] CuO 0–10% by mass, and further containing 1–30% by mass of fluoride.
[0140] As for the above-mentioned fluorophosphate-based glass, it is further preferred to contain:
[0141] P2O5 20-60% by mass
[0142] Al2O3 1-10% by mass
[0143] BaO 1-10% by mass
[0144] CuO 1-10% by mass, and further contains 2-30% by mass of fluoride.
[0145] As examples of the aforementioned fluorides, one or more can be selected from MgF2, CaF2, SrF2, etc.
[0146] The filter 1 of the present invention is characterized in that it is formed by depositing a resin film on the glass substrate through a bonding layer, the bonding layer containing Si atoms and one or more selected from Ti atoms, Zr atoms and Al atoms, and having a single-layer structure.
[0147] In the filter 1 of the present invention, as a bonding layer, a bonding layer containing a hydrolysis and dehydration condensate of the coupling agent described later can be cited as an example.
[0148] In the filter 1 of the present invention, the bonding layer contains Si atoms and one or more selected from Ti atoms, Zr atoms and Al atoms, and has a single-layer structure.
[0149] In this application, a single-layer structure refers to a layered structure specifically composed of forming materials having the same composition, as determined by the measurement image (image contrast) or elemental analysis results obtained under the following conditions and using a scanning transmission electron microscope-energy dispersive X-ray spectrometer (STEM-EDX).
[0150] <Measurement Conditions>
[0151] Scanning transmission electron microscope: ARM200F, manufactured by Nippon Electron Ltd.
[0152] Energy-dispersive X-ray spectrometer: JED-2300T manufactured by Nippon Electron Ltd.
[0153] Sample preparation: Focused ion beam processing (FIB)
[0154] Accelerating voltage: 200kV
[0155] Elemental analysis: EDX mapping (resolution: 256×256)
[0156] Figure 3 This is a STEM-EDX image (image contrast) obtained under the above measurement conditions in one example of the filter of the present invention. According to the image, the filter is formed by depositing a resin film R on an absorbing glass substrate G with a bonding layer B in between. The bonding layer B is composed of a single-layer structure.
[0157] In the filter 1 of the present invention, the thickness of the bonding layer is preferably less than 1000 nm, more preferably 10 to 500 nm, and even more preferably 30 to 300 nm.
[0158] By keeping the thickness of the bonding layer below 1000 nm, it is easy to suppress unevenness during the formation of the bonding layer (during firing), thereby making the film surface of the bonding layer easy to homogenize.
[0159] In addition, when the thickness of the bonding layer is 10nm or more, the bonding layer can easily achieve sufficient bonding strength, which can easily improve the mechanical strength of the filter.
[0160] It should be noted that, in this application document, the thickness of the bonding layer refers to the arithmetic mean of the thickness of the bonding layer at 50 locations measured in the measurement image (image contrast) of the filter cross-section obtained when using the above-mentioned STEM-EDX measurement.
[0161] In the filter 1 of the present invention, the bonding layer contains Si atoms and one or more selected from Ti atoms, Zr atoms, and Al atoms. Preferably, Ti atoms are selected from Ti atoms, Zr atoms, and Al atoms and included in the bonding layer along with Si atoms.
[0162] Figure 4 The example shown is the STEM-EDX line (the intensity line of each element constituting the filter in the depth direction of the EDX (K-ray) detection line) of the filter 1 of the present invention, measured under the above conditions. Figure 4 In the example shown, a resin film containing C atoms and O atoms as main components (described later) is provided in the region from 0 to 980 nm from the surface; a bonding layer containing Si atoms, Ti atoms and O atoms as main components is provided in the region from 980 to 1150 nm from the surface; and an absorbing glass substrate containing P atoms, F atoms and O atoms as main components is provided in the region from the surface greater than 1150 nm. The constituent elements of each region can be confirmed by the STEM-EDX line. In addition, the thickness of the bonding layer and the like can be confirmed.
[0163] exist Figure 4 As shown in the example, the bonding layer of filter 1 contains Si atoms and Ti atoms.
[0164] In the bonding layer constituting the filter 1 of the present invention, the proportion α (atomic %) of the total number of Ti atoms, Zr atoms and Al atoms in the total number of Si atoms, Ti atoms, Zr atoms and Al atoms (total number of atoms) is preferably greater than 0 atomic % and less than 33.3 atomic %; more preferably 9 to 33.3 atomic %; and even more preferably 12 to 33.3 atomic %.
[0165] In this application, the percentage α (atomic %) of the total number of Ti, Zr and Al atoms constituting the bonding layer in the total number of Si, Ti, Zr and Al atoms (total number of atoms) refers to a value calculated by the following method.
[0166] (1) The STEM-EDX measurement of the filter was performed under the above measurement conditions, and the results were as follows: Figure 4The STEM-EDX lines shown are the intensity lines of EDX (K-ray) rays in the depth direction for each element that makes up the filter.
[0167] (2) Calculate the cumulative EDX intensity X of Si atoms in the region constituting the bonding layer. Si Cumulative intensity X of EDX rays of Ti atoms Ti Cumulative intensity X of EDX rays from Zr atoms Zr and the cumulative intensity X of EDX rays of Al atoms Al .
[0168] (3) Multiply the cumulative intensity of each EDX ray obtained in (2) by the k-factor (a correction coefficient that depends on the accelerating voltage, detection efficiency, and varies according to the atom number). For convenience, the k-factor of Si atoms will be set to K below. Si Set the k-factor of the Ti atom to K. Ti Set the k-factor of the Zr atom to K. Zr Set the k-factor of the Al atom to K. Al The resulting value can be considered as corresponding to the weight ratio of each constituent element. Therefore, for example, the weight ratio A of Ti atoms constituting the bonding layer... Ti (by weight%) can be calculated using the following formula.
[0169] [Mathematical Expression 1]
[0170]
[0171] (4) Further, the value obtained by multiplying the cumulative EDX intensity X of each atom by the k factor and dividing it by the atomic weight M can be set as a ratio corresponding to the number of atoms of each constituent element. Therefore, when the atomic weight of Si is set as M... Si Let the atomic weight of Ti atoms be M. Ti Let the atomic weight of Zr atoms be M. Zr Let the atomic weight of Al atoms be M. Al In cases such as the ratio α of the number of Ti atoms constituting the bonding layer Ti (atomic percentage) can be calculated using the following formula.
[0172] [Mathematical Expression 2]
[0173]
[0174] In addition, the proportion α (atomic percent) of the total number of Ti atoms, Zr atoms and Al atoms constituting the bonding layer can be calculated by the following formula.
[0175] [Mathematical Expression 3]
[0176]
[0177] For example, in Figure 4 In the example shown, the bonding layer contains Si atoms and Ti atoms, but not Zr atoms and Al atoms. Therefore, the proportion α (atomic %) of the total number of Ti atoms, Zr atoms and Al atoms constituting the bonding layer can be calculated by the following formula.
[0178] [Mathematical Expression 4]
[0179]
[0180] It should be noted that in this application document, K is designated as K. Si =1.000, K Ti =1.033, K Zr =5.696, K Al =1.050.
[0181] As embodiments of the filter 1 of the present invention, filter 1-1 and filter 1-2 of the present invention can be listed.
[0182] The filter 1-1 of the present invention is formed by depositing a resin film on the above-mentioned absorbing glass substrate through a bonding layer, wherein the bonding layer comprises a hydrolysis and dehydration condensate of one or more coupling agents selected from the compounds represented by general formula (I) and the compounds represented by general formula (II).
[0183] M(OSiR 1 R 2 R 3 ) n (I)
[0184] In formula (I), M is a Ti atom, Zr atom, or Al atom, and R 1 R 2 and R 3 The hydrocarbon group is a straight-chain or branched hydrocarbon group containing 1 to 10 carbon atoms, which may be the same or different. n is 4 when M is a Ti or Zr atom, and 3 when M is an Al atom. Multiple -OSiR groups are also present. 1 R 2 R 3 The bases can be the same or different.
[0185] (Ti k O k-1 (OSiR) 4 R 5 R 6 ) 2k+2 (II)
[0186] In equation (II), R 4R 5 and R 6 The hydrocarbon group consisting of 1 to 10 carbon atoms (either linear or branched) containing oxygen or nitrogen atoms, and these carbon atoms may be the same or different; k is a real number of 2 or more and less than 15; and multiple -OSiR groups are allowed. 4 R 5 R 6 The bases can be the same or different.
[0187] Furthermore, the filters 1-2 of the present invention are formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer comprises a hydrolysis and dehydration condensate of one or more coupling agents selected from the compounds represented by general formula (III) and the compounds represented by general formula (IV) below.
[0188] M{OSi(OR 7 (OR) 8 (OR) 9 )} n (III)
[0189] In formula (III), M is a Ti atom, a Zr atom, or an Al atom, and R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different; n is 4 when M is a Ti atom or a Zr atom, and 3 when M is an Al atom; multiple -OSi(OR) groups. 7 (OR) 8 (OR) 9 The bases can be the same or different.
[0190] (Ti k O k-1 ){OSi(OR 10 (OR) 11 (OR) 12 )} 2k+2 (IV)
[0191] In equation (IV), R 10 R 11 and R 12 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSi(OR) groups. 10 (OR) 11 (OR) 12 The bases can be the same or different.
[0192] The compound represented by general formula (III) that is a component of the above-mentioned bonding layer is a further definition of the compound represented by general formula (I). In addition, the compound represented by general formula (IV) that is a component of the above-mentioned bonding layer is a further definition of the compound represented by general formula (II).
[0193] Therefore, in the following description of the bonding layer of the filter 1 of the present invention, the compounds represented by general formula (I) and general formula (III), as well as the compounds represented by general formula (II) and general formula (IV) that are constituent components of the bonding layer, will be described in turn, and the method of forming the bonding layer will be described.
[0194] In the filter 1 of the present invention, M constituting the compound represented by the following general formula (I) is a Ti atom, a Zr atom, or an Al atom, preferably a Ti atom.
[0195] M(OSiR 1 R 2 R 3 ) n (I).
[0196] In the compounds represented by the above general formula (I), R 1 R 2 and R 3 The hydrocarbon group is a straight-chain or branched hydrocarbon group with 1 to 10 carbon atoms containing oxygen or nitrogen atoms, preferably a straight-chain or branched hydrocarbon group with 1 to 4 carbon atoms containing oxygen or nitrogen atoms, and more preferably a straight-chain or branched hydrocarbon group with 1 to 3 carbon atoms containing oxygen or nitrogen atoms.
[0197] As R 1 R 2 and R 3 Specifically, examples include straight-chain, branched-chain, or cyclic hydrocarbon groups selected from methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl, as well as -C3H6(COO)CHCH2, -CH2(COO)CHCH2, -C2H4(COO)CHCH2, -C4H8(COO)CHCH2, and -C5H 10 (COO)CHCH2、-C6H 12 (COO)CHCH2、-C7H 14 (COO)CHCH2、-C8H 16 (COO)CHCH2、-C9H 18 (COO)CHCH2、-C 10 H 20 Groups such as (COO)CHCH2 and other straight-chain, branched, or cyclic hydrocarbon groups.
[0198] In the filter 1 of the present invention, by making R 1 R 2 and R 3 When the number of carbon atoms is within the above range, it is easy to maintain a suitable reaction rate between silicon compounds and metal alkoxides, thus making it easier to prepare more homogeneous coupling agents.
[0199] Furthermore, in compounds represented by general formula (I), R is bonded to silicon atoms. 1 R 2 and R 3 The functional groups indicated can affect the adhesion between the resin film and the bonding layer. Therefore, an appropriate R is selected based on the resin film disposed on the bonding layer. 1 R 2 and R 3 The base can be used to adjust the adhesion between the resin film and the bonding layer.
[0200] The above R 1 R 2 and R 3 They can be the same or different.
[0201] Additionally, n is 4 when M is a Ti or Zr atom, and 3 when M is an Al atom, with multiple -OSiR 1 R 2 R 3 The bases can be the same or different.
[0202] In the filter 1 of the present invention, compounds represented by general formula (I) can be listed below as compounds represented by general formula (III).
[0203] M{OSi(OR 7 (OR) 8 (OR) 9 )} n (III)
[0204] In formula (III), M is a Ti atom, a Zr atom, or an Al atom, and R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different; n is 4 when M is a Ti atom or a Zr atom, and 3 when M is an Al atom; multiple -OSi(OR) groups. 7 (OR) 8 (OR) 9 The bases can be the same or different.
[0205] In the compounds represented by the above general formula (III), M is a Ti atom, a Zr atom, or an Al atom, preferably a Ti atom.
[0206] In the compounds represented by the above general formula (III), R 7 R 8 and R 9 It is a straight-chain or branched hydrocarbon group with 1 to 10 carbon atoms, preferably a straight-chain or branched hydrocarbon group with 1 to 4 carbon atoms, and more preferably a straight-chain or branched hydrocarbon group with 1 to 3 carbon atoms.
[0207] As R 7 R 8 and R 9 Specifically, groups selected from straight-chain or branched-chain, cyclic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl can be listed.
[0208] R 7 R 8 and R 9 They can be the same or different.
[0209] In the filter 1 of the present invention, by making R 7 R 8 and R 9 When the number of carbon atoms is within the above range, it is easy to maintain a suitable reaction rate between silicon compounds and metal alkoxides, thus making it easier to prepare more homogeneous coupling agents.
[0210] The above R 7 R 8 and R 9 They can be the same or different.
[0211] Additionally, n is 4 when M is a Ti or Zr atom, and 3 when M is an Al atom, with multiple -OSi(OR) 7 (OR) 8 (OR) 9 The bases can be the same or different.
[0212] The coupling agent represented by general formula (III) above preferably contains a silicon compound represented by general formula (V) below, and one or more reactants selected from general formulas (VI), (VII) below and (VIII) below.
[0213] Si(OR 7 (OR) 8 (OR) 9 )OH(V)
[0214] In equation (V), R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0215] Ti(OR 13 (OR) 14 (OR) 15 (OR) 16 (VI)
[0216] In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0217] Zr(OR 17 (OR) 18 (OR) 19 (OR) 20 (VII)
[0218] In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0219] Al(OR 21 (OR) 22 (OR) 23 (VIII)
[0220] In equation (VIII), R 21 R 22 and R 23 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
[0221] In the silicon compounds represented by the above general formula (V), the above R 7 R 8 and R 9 The number of carbon atoms, and specific examples are as described above, R 7 R 8 and R 9 They can be the same or different.
[0222] The silicon compounds represented by the above general formula (V) can be readily generated by partially hydrolyzing the corresponding silanol salt, as described below.
[0223] Si(OR 7 (OR) 8 (OR) 9 (OR) a ) + H2O → Si(OR) 7 (OR)8 (OR) 9 )OH+R a OH
[0224] Among them, R 7 R 8 R 9 and R a It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
[0225] The above hydrocarbon group R 7 R 8 and R 9 The preferred method is as described above, R a The preferred method is also related to the hydrocarbon group R 7 R 8 and R 9 The preferred method is the same.
[0226] Silane alkoxides, under conditions of complete hydrolysis, react as described below to generate silanol Si(OH)4.
[0227] Si(OR 7 (OR) 8 (OR) 9 (OR) a ) + 4H2O → Si(OH)4 + R 7 OH+R 8 OH+R 9 OH+
[0228] R a OH
[0229] On the other hand, by controlling the amount of water used to hydrolyze the silanol salt, a silicon compound represented by the general formula (V) can be obtained as described above.
[0230] The above general formula (VI)Ti(OR) 13 (OR) 14 (OR) 15 (OR) 16 Titanium alkoxides represented by ) and the above general formula (VII)Zr(OR) 17 (OR) 18 (OR) 19 (OR) 20 Zirconium alkoxides represented by (VIII)Al(OR) 21 (OR) 22 (OR) 23 In the aluminum alkoxide represented by ), R 13 ~R 23 (R 13 R 14 R15 R 16 R 17 R 18 R 19 R 20 R 21 R 22 and R 23 The hydrocarbon group is a straight-chain or branched hydrocarbon group with 1 to 10 carbon atoms, preferably a straight-chain or branched hydrocarbon group with 2 to 9 carbon atoms, and more preferably a straight-chain or branched hydrocarbon group with 3 to 8 carbon atoms.
[0231] As R 13 R 14 R 15 R 16 R 17 R 18 R 19 R 20 R 21 R 22 Or R 23 Specifically, groups can be selected from straight-chain or branched-chain, cyclic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl.
[0232] R 13 R 14 R 15 R 16 R 17 R 18 R 19 R 20 R 21 R 22 and R 23 They can be the same or different.
[0233] In the filter 1 of the present invention, by making R 13 R 14 R 15 R 16 R 17 R 18 R 19 R 20 R 21 R 22 Or R 23 Having 2 or more carbon atoms can effectively improve the stability of metal alkoxides to moisture. By making the number of carbon atoms less than 9, the increase in viscosity of metal alkoxides can be suppressed, thus effectively improving their processability.
[0234] Using the above general formula Si(OR) 7 (OR) 8 (OR) 9Silicon compounds represented by )OH and titanium alkoxides represented by the above general formula (VI) Ti(OR) 13 (OR) 14 (OR) 15 (OR) 16 Taking this as an example, we believe that the reactions of the two proceed as described below.
[0235] 4Si(OR 7 (OR) 8 (OR) 9 )OH+Ti(OR 13 (OR) 14 (OR) 15 (OR) 16 )
[0236] →Ti{OSi(OR 7 (OR) 8 (OR) 9 )}4+R 13 OH+R 14 OH+R 15 OH+R 16 OH
[0237] Within the reaction system, by means of the general formula Ti(OR) 13 (OR) 14 (OR) 15 (OR) 16 ) represents 1 mole of titanium alkoxide, and contains the general formula Si(OR) 7 (OR) 8 (OR) 9 The reaction is carried out in the presence of more than 4 moles of silicon compound represented by OH, and it is assumed that all titanium alkoxides present in the system react according to the above formula.
[0238] As the filter 1 of the present invention, an example is a filter formed by placing a resin film, described later, on an absorbing glass substrate through a bonding layer containing a hydrolyzed and dehydrated condensate of a coupling agent, wherein the coupling agent comprises a compound represented by the following general formula (III).
[0239] M{OSi(OR 7 (OR) 8 (OR) 9 )} n (III)
[0240] In formula (III), M is a Ti atom, a Zr atom, or an Al atom, and R 7 R 8 and R 9It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different; n is 4 when M is a Ti atom or a Zr atom, and 3 when M is an Al atom; multiple -OSi(OR) groups. 7 (OR) 8 (OR) 9 The bases can be the same or different.
[0241] If the coupling agent containing the compound represented by the above general formula (III) is Ti{OSi(OR) 7 (OR) 8 (OR) 9 Taking case 4 as an example, the above coupling agent undergoes hydrolysis by adding water into the system, as shown in the following reaction formula.
[0242] Ti{OSi(OR 7 (OR) 8 (OR) 9 )}4+12H2O→Ti{OSi(OH)3}4+4R 7 OH+4R 8 OH+
[0243] 4R 9 OH
[0244] The above hydrolysis reaction can be carried out, for example, at a temperature of 10–40°C, using a catalyst such as HCl, in the presence of an appropriate amount of water.
[0245] Next, a coating solution containing a hydrolysate of a coupling agent composed of a compound represented by the above general formula (III) is coated onto an absorbent glass substrate to form a coating film.
[0246] The concentration of the coupling agent composed of the compound represented by general formula (III) in the above coating solution is preferably 0.1 to 10.0% by mass. Furthermore, the coating amount of the above coating solution on the absorbent glass substrate is preferably 0.01 to 0.10 ml / cm². 2 .
[0247] As a method for applying the above-mentioned coating liquid containing the hydrolysate of the coupling agent, one or more coating methods selected from dip coating, casting coating, spray coating, spin coating, etc., may be listed.
[0248] Based on this, the coating liquid for forming resin film, as described later, is coated onto the above-mentioned coated film to form an absorbent resin coated film. Then, appropriate heating is performed to obtain the dehydrated condensate [-Ti(OSiO3)3-] as a coupling agent. n (where n is a positive integer) represents the reactants.
[0249] It is believed that the above-mentioned dehydration condensate and coupling agent are strongly bonded together, with the coupling agent and the absorbing glass or resin film. Therefore, according to the present invention, a filter 1 having a resin film with high adhesion provided on an absorbing glass substrate made of phosphate glass or fluorophosphate glass can be readily provided.
[0250] For the filter 1 of the present invention, the bonding layer may further contain silanol hydrolysis and dehydration condensate.
[0251] That is, by appropriately heating silanol Si(OH)4, a dehydration condensate (Si-O-Si)2 is generated as shown in the following reaction formula.
[0252] Si(OH) 4→ (Si-O-Si)2+2H2O
[0253] According to the research of the inventors, if only the above-mentioned dehydration condensate of silanol is used, the adhesion to the absorbent glass substrate and resin film is easily insufficient, especially when moisture is present. However, by using it in combination with the dehydration condensate obtained by dehydrating and condensing the hydrolysate of the coupling agent containing the above-mentioned general formula (I) or general formula (III), the above-mentioned adhesion can be improved by mutual complementation.
[0254] After adding the above-mentioned silanol to a coating solution containing a hydrolysate of a coupling agent composed of a compound represented by general formula (I) or general formula (III), the coating solution is coated onto an absorbent glass substrate to form a coating film. Then, the above-mentioned heat treatment is appropriately applied, thereby allowing the silanol to react with the dehydration condensate [-Ti(OSiO3)3-] of the coupling agent hydrolysate. n (where n is a positive integer) together form a dehydration condensate of silanol.
[0255] Preferably, the filter 1 of the present invention is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass, with a bonding layer containing a hydrolyzed and dehydrated condensate of a coupling agent composition. The coupling agent composition contains 50 mol% or more and less than 100 mol% of a silicon compound represented by the following general formula (V), and more than 0 mol% and less than 50 mol% of one or more reactants selected from the following general formulas (VI), (VII), and (VIII).
[0256] Si(OR 7 (OR) 8 (OR) 9 )OH(V)
[0257] In equation (V), R 7 R 8 and R 9It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0258] Ti(OR 13 (OR) 14 (OR) 15 (OR) 16 (VI)
[0259] In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0260] Zr(OR 17 (OR) 18 (OR) 19 (OR) 20 (VII)
[0261] In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different.
[0262] Al(OR 21 (OR) 22 (OR) 23 (VIII)
[0263] In equation (VIII), R 21 R 22 and R 23 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
[0264] By reducing the metal alkoxide content to below 50 mol%, the coatability of the resulting coupling agent can be effectively improved.
[0265] In the filter 1 of the present invention, the coupling agent composition is preferably a reaction composition of more than 50 mol% and less than 100 mol% of a silicon compound represented by the above general formula (V) and more than 0 mol% and less than 50 mol% of a metal alkoxide selected from the above general formulas (VI), (VII) and (VIII), more preferably a reaction composition of more than 80 mol% and less than 100 mol% of a silicon compound represented by the above general formula (V) and more than 0 mol% and less than 20 mol% of a metal alkoxide selected from the above general formulas (VI), (VII) and (VIII), and even more preferably a reaction composition of 85 to 94 mol% of a silicon compound represented by the above general formula (V) and 6 to 15 mol% of a metal alkoxide selected from the above general formulas (VI), (VII) and (VIII).
[0266] By making the reaction ratio of the silicon compound represented by the above general formula (V) with one or more metal alkoxides selected from the above general formulas (VI), (VII) and (VIII) within the above range, a homogeneous, smooth, and non-peelable film can be easily formed.
[0267] The details of the above-mentioned absorbing glass substrate, silicon compound represented by general formula (V), metal alkoxide represented by general formula (VI), general formula (VII) and general formula (VIII) are as described above.
[0268] In the filter 1 of the present invention, a uniform coating solution containing the above-mentioned coupling agent composition can be easily prepared by reacting a silicon compound represented by general formula (V) with a metal alkoxide represented by general formula (VI), general formula (VII) and general formula (VIII) in the above-mentioned proportions, and uniform film formation can be easily achieved.
[0269] As described above, if we use the general formula (V)Si(OR) 7 (OR) 8 (OR) 9 Silicon compounds represented by )OH and titanium alkoxides represented by the above general formula (VI) Ti(OR) 13 (OR) 14 (OR) 15 (OR) 16 For example, the reactions of the two are as follows.
[0270] 4Si(OR 7 (OR) 8 (OR) 9 )OH+Ti(OR 13 (OR) 14 (OR) 15 (OR)16 )
[0271] →Ti{OSi(OR 7 (OR) 8 (OR) 9 )}4+R 13 OH+R 14 OH+R 15 OH+R 16 OH
[0272] When the reaction is carried out in excess of silicon compound with more than 4 moles of silicon compound relative to 1 mole of the aforementioned titanium alkoxide, it can be assumed that all of the aforementioned titanium alkoxide in the system reacts according to the above formula. Conversely, if the amount of silicon compound is less than 4 moles relative to 1 mole of the aforementioned titanium alkoxide, then alkoxy groups (OR) remain in the generated titanium compound. 13 base, OR 14 base, OR 15 base, OR 16 If a large amount of such alkoxy-containing titanium compounds are present, the titanium compounds will precipitate in the coating solution, making it difficult to form a uniform film. Therefore, it is preferable to use a coupling composition prepared by reacting a silicon compound in an excess of the theoretical amount.
[0273] As described above, by making Ti{OSi(OR) generated in the above reaction 7 (OR) 8 (OR) 9 Hydrolysis is carried out appropriately in the presence of a catalyst containing inorganic acids such as HCl, and the hydrolysis reaction proceeds according to the following reaction formula.
[0274] Ti{OSi(OR 7 (OR) 8 (OR) 9 )}4+12H2O→Ti{OSi(OH)3}4+4R 7 OH+4R 8 OH+
[0275] 4R 9 OH
[0276] Additionally, if an excess of the silicon compound represented by general formula (V) is present in the system at this time, hydrolysis will occur according to the following reaction formula to generate silanol Si(OH)4.
[0277] Si(OR 7 (OR) 8 (OR) 9 OH + 3H₂O → Si(OH)₄ + R 7 OH+R 8 OH+R9 OH
[0278] As described above, by appropriately heating the hydrolysate Ti{OSi(OH)3}4, a dehydration condensate of the hydrolysate, [-Ti(OSiO3)3-], can be obtained. n (where n is a positive integer) represents the reactants.
[0279] In addition, as described above, the silanol Si(OH)4 generated by the above hydrolysis is also suitable for heat treatment, thereby causing a dehydration condensation reaction as shown in the following reaction formula to generate a dehydration condensate (Si-O-Si)2.
[0280] Si(OH)4→(Si-O-Si)2+2H2O
[0281] When only the above-mentioned silanol dehydration condensate is used, the adhesion to the absorbent glass substrate and resin film is easily insufficient, especially when moisture is present. However, by using it in combination with the above-mentioned coupling agent hydrolysate Ti{OSi(OH)3}4 dehydration condensate, they can complement each other and improve the adhesion to the absorbent glass substrate and the like.
[0282] In addition to the silicon compound represented by the above general formula (V) and the reaction product with the metal alkoxide represented by the above general formula (VI), general formula (VII) or general formula (VIII), the above coupling agent composition may further contain any components such as a reaction catalyst, pH adjuster, leveling agent, and defoamer.
[0283] In the filter 1 of the present invention, the compound represented by the following general formula (II) is different from the compound represented by the above general formula (I), and has a polymer structure (-Ti-O-Ti-) containing more than 2 Ti atoms in the molecule.
[0284] (Ti k O k-1 (OSiR) 4 R 5 R 6 ) 2k+2 (II)
[0285] In equation (II), R 4 R 5 and R 6 The hydrocarbon group consisting of 1 to 10 carbon atoms (either linear or branched) containing oxygen or nitrogen atoms, and these carbon atoms may be the same or different; k is a real number of 2 or more and less than 15; and multiple -OSiR groups are allowed. 4 R 5 R 6 The bases can be the same or different.
[0286] In compounds represented by general formula (II), R4 R 5 and R 6 The hydrocarbon group is a straight-chain or branched hydrocarbon group with 1 to 10 carbon atoms containing oxygen or nitrogen atoms, preferably a straight-chain or branched hydrocarbon group with 1 to 4 carbon atoms containing oxygen or nitrogen atoms, and more preferably a straight-chain or branched hydrocarbon group with 1 to 3 carbon atoms containing oxygen or nitrogen atoms.
[0287] As R 4 R 5 and R 6 Specifically, examples include straight-chain, branched-chain, or cyclic hydrocarbon groups selected from methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl, as well as -C3H6(COO)CHCH2, -CH2(COO)CHCH2, -C2H4(COO)CHCH2, -C4H8(COO)CHCH2, and -C5H 10 (COO)CHCH2、-C6H 12 (COO)CHCH2、-C7H 14 (COO)CHCH2、-C8H 16 (COO)CHCH2、-C9H 18 (COO)CHCH2、-C 10 H 20 Groups such as (COO)CHCH2 and other straight-chain, branched, or cyclic hydrocarbon groups.
[0288] In compounds represented by general formula (II), by making R 4 R 5 and R 6 When the number of carbon atoms is within the above range, it is easy to maintain a suitable reaction rate between silicon compounds and metal alkoxides, thus making it easier to prepare more homogeneous coupling agents.
[0289] Furthermore, in compounds represented by general formula (II), R is bonded to silicon atoms. 4 R 5 and R 6 The functional groups indicated can affect the adhesion between the resin film and the bonding layer. Therefore, an appropriate R can be selected based on the resin film disposed on the bonding layer. 4 R 5 and R 6 The base is used to adjust the adhesion between the resin film and the bonding layer.
[0290] In compounds represented by general formula (II), k is a real number of 2 or more and 15 or less, more preferably a real number of 4 or more and 10 or less, and particularly preferably 4, 7 or 10.
[0291] In the compound represented by general formula (II), by making k within the above range, a resin film with high adhesion can be easily formed on an absorbent glass substrate made of phosphate-based glass or fluorophosphate glass.
[0292] In compounds represented by general formula (II), R 4 R 5 and R 6 They can be the same or different.
[0293] In addition, multiple -OSiR 4 R 5 R 6 The bases can be the same or different.
[0294] In the filter 1 of the present invention, compounds represented by general formula (II) can be listed below as compounds represented by general formula (IV).
[0295] (Ti k O k-1 ){OSi(OR 10 (OR) 11 (OR) 12 )} 2k+2 (IV)
[0296] In equation (IV), R 10 R 11 and R 12 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSi(OR) groups. 10 (OR) 11 (OR) 12 The bases can be the same or different.
[0297] R constitutes the compound represented by general formula (IV) 10 R 11 and R 12 It is a straight-chain or branched hydrocarbon group with 1 to 10 carbon atoms, preferably a straight-chain or branched hydrocarbon group with 1 to 4 carbon atoms, and more preferably a straight-chain or branched hydrocarbon group with 1 to 3 carbon atoms.
[0298] As R 10 R 11 and R 12 Specifically, groups selected from straight-chain or branched-chain, cyclic hydrocarbon groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl can be listed.
[0299] R 10 R 11 and R 12 They can be the same or different.
[0300] In compounds represented by general formula (IV), by making R 10 R 11 and R 12 When the number of carbon atoms is within the above range, it is easy to maintain a suitable reaction rate between silicon compounds and metal alkoxides, thus making it easier to prepare more homogeneous coupling agents.
[0301] In compounds represented by general formula (IV), k is a real number of 2 or more and 15 or less, more preferably a real number of 4 or more and 10 or less, and particularly preferably 4, 7 or 10.
[0302] In addition, multiple -OSi(OR) 10 (OR) 11 (OR) 12 The bases can be the same or different.
[0303] In the compound represented by general formula (IV), by making k within the above range, a resin film with high adhesion can be easily formed on an absorbent glass substrate made of phosphate-based glass or fluorophosphate glass.
[0304] In compounds represented by general formula (IV), when k is 2, they can be represented by the following structural formula.
[0305] [Chemical Formula 1]
[0306]
[0307] Among them, multiple R 10 R 11 and R 12 They can be the same or different. Additionally, multiple -OSi (OR) 10 (OR) 11 (OR) 12 The bases can be the same or different.
[0308] In compounds represented by general formula (IV), when k is 3, they can be represented by the following structural formula.
[0309] [Chemical Formula 2]
[0310]
[0311] Among them, multiple R 10 R 11 and R 12 They can be the same or different. Additionally, multiple -OSi (OR) 10 (OR) 11 (OR) 12 The bases can be the same or different.
[0312] The coupling agent represented by the above general formula (IV) preferably comprises a silicon compound represented by the following general formula (IX) and a reactant of tetrahydroxytitanium represented by the following formula Ti(OH)4.
[0313] Si(OR 10 (OR) 11 (OR) 12 )OH(IX)
[0314] In equation (IX), R 10 R 11 and R 12 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
[0315] In the silicon compounds represented by the above general formula (IX), the above R 10 R 11 and R 12 The number of carbon atoms, and specific examples are as described above, R 10 R 11 and R 12 They can be the same or different.
[0316] The above general formula (IX)Si(OR) is considered to be 10 (OR) 11 (OR) 12 The reaction of silicon compounds represented by )OH with tetrahydroxytitanium represented by the above formula Ti(OH)4 is carried out, for example, as described below.
[0317] 6Si(OR 10 (OR) 11 (OR) 12 )OH+2Ti(OH)4
[0318] →Ti2O{OSi(OR 10 (OR) 11 (OR) 12 )}6+4H2O
[0319] The general formula Ti2O{OSi(OR) obtained from the above reaction is Ti2O{OSi(OR)} 10 (OR) 11 (OR) 12 The compound represented by )}6 is equivalent to the compound represented by the above general formula (IV) where k is 2.
[0320] It can be assumed that the presence of more than 6 moles of the general formula Si(OR) relative to tetrahydroxytitanium (Ti(OH)4)2 moles in the reaction system 10 (OR) 11 (OR) 12The reaction is carried out in the presence of an excess of silicon compound represented by )OH, and all tetrahydroxytitanium present in the system reacts according to the above formula.
[0321] As the filter 1 of the present invention, it is preferably a filter formed by placing the resin film described below on an absorbing glass substrate through a bonding layer containing a hydrolyzed, dehydrating condensate of one or more coupling agents selected from the following general formula (IV).
[0322] (Ti k O k-1 ){OSi(OR 10 (OR) 11 (OR) 12 )} 2k+2 (IV)
[0323] In equation (IV), R 10 R 11 and R 12 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSi(OR) groups. 10 (OR) 11 (OR) 12 The bases can be the same or different.
[0324] If the coupling agent composed of the compound represented by the above general formula (IV) is Ti2O{OSi(OR) 10 (OR) 11 (OR) 12 Taking the case of 6 (where k is 2 in the compound represented by the above general formula (IV)) as an example, the above coupling agent undergoes a hydrolysis reaction by adding water into the system as shown in the following reaction formula.
[0325] Ti2O{OSi(OR 10 (OR) 11 (OR) 12 )}6+18H2O→
[0326] Ti2O{OSi(OH)3}6+6R 10 OH+6R 11 OH+6R 12 OH
[0327] The above hydrolysis reaction can be carried out, for example, at a temperature of 10–40°C, using a catalyst such as HCl, in the presence of an appropriate amount of water.
[0328] Next, a coating solution containing a hydrolysate of a coupling agent composed of a compound represented by the above general formula (IV) is coated onto an absorbent glass substrate to form a coating film.
[0329] The concentration of the coupling agent composed of the compound represented by general formula (IV) in the above coating solution is preferably 0.5% to 20% by mass. Furthermore, the coating amount of the above coating solution on the absorbent glass substrate is preferably 0.005 to 0.5 ml / cm². 2 .
[0330] As a method for applying the above-mentioned coating liquid containing the hydrolysate of the coupling agent, one or more coating methods selected from dip coating, casting coating, spray coating, spin coating, etc., may be listed.
[0331] Based on this, the coating liquid for forming resin film, as described later, is coated onto the above-mentioned coated film to form an absorbent resin coated film. Then, appropriate heating is performed to obtain [-(TiO3)2(SiO3)5-] as a dehydration condensate of the hydrolysate. m (where m is a positive integer.) represents the reactants.
[0332] It is believed that the above-mentioned dehydration condensate and coupling agent are strongly bonded together, with the coupling agent and the absorbing glass or resin film. Therefore, according to the present invention, a filter 1 having a resin film with high adhesion provided on an absorbing glass substrate made of phosphate glass or fluorophosphate glass can be readily provided.
[0333] In the filter 1 of the present invention, as described above, the bonding layer may further contain a hydrolyzed and dehydrated condensate of silanol.
[0334] That is, by appropriately heating silanol Si(OH)4, a dehydration condensate (Si-O-Si)2 is generated as shown in the following reaction formula.
[0335] Si(OH)4→(Si-O-Si)2+2H2O
[0336] According to the research of the inventors, when only the above-mentioned dehydration condensate of silanol is used, the adhesion to the absorbent glass substrate and resin film is easily insufficient, especially when moisture is present. However, by using it in combination with a dehydration condensate obtained by dehydrating and condensing a coupling agent containing a compound represented by the above-mentioned general formula (II) or general formula (IV), the above-mentioned adhesion can be improved by mutual complementation.
[0337] By adding the above-mentioned silanol to a coating solution containing a hydrolysate of a coupling agent composed of a compound represented by the above-mentioned general formula (II) or general formula (IV), and coating the coating solution onto an absorbent glass substrate to form a coating film, and then appropriately applying the above-mentioned heat treatment, a dehydration condensate of silanol can be generated together with the dehydration condensate of the hydrolysate of the coupling agent.
[0338] Next, the filter 2 of the present invention will be described.
[0339] The filter 2 of the present invention is formed by depositing a resin film containing Si atoms and one or more selected from Ti atoms, Zr atoms and Al atoms on an absorbing glass substrate made of phosphate glass or fluorophosphate glass. Specific examples include the filter 2-1 or the filter 2-2 of the present invention.
[0340] The filter 2-1 of the present invention is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass, with a bonding layer containing a hydrolysis and dehydration condensate of a compound selected from the compounds represented by general formula (I) and general formula (II) below.
[0341] M(OSiR 1 R 2 R 3 ) n (I)
[0342] In formula (I), M is a Ti atom, Zr atom, or Al atom, and R 1 R 2 and R 3 The hydrocarbon group is a straight-chain or branched hydrocarbon group containing 1 to 10 carbon atoms, which may be the same or different. n is 4 when M is a Ti or Zr atom, and 3 when M is an Al atom. Multiple -OSiR groups are also present. 1 R 2 R 3 The bases can be the same or different.
[0343] (Ti k O k-1 (OSiR) 4 R 5 R 6 ) 2k+2 (II)
[0344] In equation (II), R 4 R 5 and R 6 The hydrocarbon group consisting of 1 to 10 carbon atoms (either linear or branched) containing oxygen or nitrogen atoms, and these carbon atoms may be the same or different; k is a real number of 2 or more and less than 15; and multiple -OSiR groups are allowed. 4 R 5 R 6 The bases can be the same or different.
[0345] Furthermore, the filter 2-2 of the present invention is formed by providing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass, with a bonding layer containing a hydrolysis and dehydration condensate of a coupling agent selected from the compounds represented by general formula (III) and general formula (IV) below.
[0346] M{OSi(OR 7 (OR) 8 (OR) 9 )} n (III)
[0347] In formula (III), M is a Ti atom, a Zr atom, or an Al atom, and R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different; n is 4 when M is a Ti atom or a Zr atom, and 3 when M is an Al atom; multiple -OSi(OR) groups. 7 (OR) 8 (OR) 9 The bases can be the same or different.
[0348] (Ti k O k-1 ){OSi(OR 10 (OR) 11 (OR) 12 )} 2k+2 (IV)
[0349] In equation (IV), R 10 R 11 and R 12 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSi(OR) groups. 10 (OR) 11 (OR) 12 The bases can be the same or different.
[0350] Regarding the filter 2 of the present invention, in relation to the filter 1 of the present invention described above, the difference lies in the inclusion of a binding layer component (e.g., a coupling agent or a hydrolyzed, dehydrated condensate of a coupling agent composition) within the resin film, as described later. All other aspects are the same. Therefore, the detailed description of the same matter is as described above.
[0351] Furthermore, in the resin film constituting the filter 2 of the present invention, the proportion α (atomic %) of the total number of Ti atoms, Zr atoms and Al atoms in the total number of Si atoms, Ti atoms, Zr atoms and Al atoms (total number of atoms) is preferably greater than 0 atomic % and less than 33.3 atomic %; more preferably 9 to 33.3 atomic %; and even more preferably 12 to 33.3 atomic %.
[0352] It should be noted that, in this application document, the ratio α (atomic %) of the total number of Ti atoms, Zr atoms and Al atoms constituting the resin film also refers to the value calculated by STEM-EDX measurement of the filter under the same measurement conditions as the ratio α (atomic %) of the total number of Ti atoms, Zr atoms and Al atoms constituting the bonding layer.
[0353] As a method for manufacturing the filter 2 of the present invention, examples include coating an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass with a resin film-forming liquid containing the hydrolysate of the coupling agent composition described above (described later) to form a coated film, and then performing a suitable heat treatment and dehydration condensation reaction. Through this manufacturing method, the coupling agent is strongly bonded to itself, or the hydrolysate and dehydration condensate of the coupling agent and the absorbing glass substrate are strongly bonded together, thus forming a desired filter.
[0354] [Resin film]
[0355] In the filter of the present invention, examples of resin films include, for example, absorbing resin films that absorb ultraviolet or near-infrared light, anti-reflective films, reflective magnifying films, protective films for preventing glass from losing its luster, reinforcing films for improving the strength of glass, and water-repellent films.
[0356] As an absorbing resin film for absorbing ultraviolet or near-infrared light, examples include resin films containing near-infrared absorbing pigments and transparent resins, with resin films in which near-infrared absorbing pigments are uniformly dissolved or dispersed in transparent resins being preferred.
[0357] The near-infrared absorbing pigment constituting the absorbing resin film can be any known pigment, preferably selected from anthocyanin pigments, polymethyl pigments, and squaric acid. One or more of the following: squarylium-based pigments, porphyrin-based pigments, metal dithiol complex-based pigments, phthalocyanine-based pigments, diimine-based pigments, and inorganic oxide particles; more preferably, squaryl acid. One or more of the following: salt-based pigments, anthocyanin-based pigments, and phthalocyanine-based pigments.
[0358] The resin constituting the resin film can be any known transparent resin, and may be selected from one or more of acrylic resins, epoxy resins, olefin-thiol resins, polycarbonate resins, polyether resins, polyarylate resins, polysulfone resins, polyethersulfone resins, poly(p-phenylene) resins, polyarylene ether phosphine oxide resins, polyimide resins, polyamide-imide resins, polyolefin resins, cyclic olefin resins, and polyester resins.
[0359] From the viewpoints of transparency, solubility of near-infrared absorbing pigments in transparent resins, and heat resistance, transparent resins with high glass transition temperature (Tg) are preferred. Specifically, resins selected from one or more of polyester resins, polycarbonate resins, polyethersulfone resins, polyarylate resins, polyimide resins, and epoxy resins are preferred, and resins selected from one or more of polyester resins and polyimide resins are more preferred.
[0360] The polyester resin is preferably selected from one or more of polyethylene terephthalate resin and polyethylene naphthalate resin.
[0361] In addition to the aforementioned near-infrared absorbing pigments and transparent resins, the resin film may further contain any components such as color-correcting pigments, leveling agents, antistatic agents, heat stabilizers, light stabilizers, antioxidants, dispersants, flame retardants, lubricants, and plasticizers, without compromising the effectiveness of the present invention.
[0362] As described above, when the filter of the present invention is the filter 1 of the present invention, for example, a hydrolysis forming film is formed on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass by hydrolyzing a containing liquid containing the above-mentioned coupling agent composition, and a resin film forming liquid that absorbs at least one of ultraviolet light and near-infrared light is coated thereon to form a coated film.
[0363] In addition, when the filter of the present invention is the filter 2 of the present invention, for example, a resin film forming liquid containing the above-mentioned coupling agent composition is coated onto an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass to form a coating film.
[0364] The resin film can be formed, for example, by dissolving or dispersing pigments, transparent resins, and coupling agents and any coordinating components used in the case of forming the infrared cut-off filter of the second aspect of the present invention in a solvent to prepare a resin film forming liquid, applying and drying it, and further curing it as needed.
[0365] The aforementioned resin film forming solution may contain known surfactants such as cationic, anionic, and nonionic surfactants.
[0366] The resin film forming liquid can be applied using one or more coating methods selected from dip coating, casting coating, spray coating, spin coating, etc.
[0367] A resin film can be formed by applying the above-mentioned resin film forming liquid onto a substrate and then drying it.
[0368] Examples of filters used in this invention include infrared cut-off filters (IRCF).
[0369] When the filter of the present invention is an infrared cutoff filter (IRCF), for example, such as Figure 2 (b) As exemplified, an infrared cut-off filter (IRCF) 1 may be provided on the lower surface side (light emitting side) of the absorbing glass substrate 3' that absorbs ultraviolet or near-infrared light, which further has an absorbing resin film 5 that absorbs ultraviolet or near-infrared light.
[0370] exist Figure 2 In the manner shown in (b), a reflective film (UVIR film) 2 is provided on the upper surface side (light incident surface side) of the absorbing glass substrate 3' that absorbs ultraviolet or near-infrared light, and an anti-reflective film (AR film) 4 is further provided on the lower surface side of the absorbing resin film 5 that absorbs ultraviolet or near-infrared light.
[0371] In the above examples, any reflective film (UVIR film) can be used to transmit visible light and block light in the ultraviolet and near-infrared regions. Examples of such reflective films (UVIR films) include reflective films formed by dielectric multilayer films.
[0372] The dielectric multilayer film is composed of alternating layers of low-refractive-index dielectric film (low-refractive-index film) and high-refractive-index dielectric film (high-refractive-index film). As the constituent material of the high-refractive-index film, one or more of the following can be selected: Ta2O5, TiO2, Nb2O5, etc., with TiO2 being preferred.
[0373] In addition, materials selected from SiO2 and SiO2 can be used as constituent materials for low refractive index films. x N y One or more of the following, with SiO2 being preferred.
[0374] As an anti-reflective film (AR film), dielectric multilayer films can also be listed.
[0375] According to the present invention, an infrared cut-off filter can be provided in which a resin film with high adhesion is provided on an absorbing glass substrate made of phosphate glass or fluorophosphate glass.
[0376] Next, the camera device of the present invention will be described.
[0377] The imaging device of the present invention is characterized by having a solid-state imaging device, an imaging lens, and the filter of the present invention.
[0378] As solid-state imaging devices, examples include CCD (Charge-Coupled Device) sensors and CMOS (Complementary Metal Oxide Semiconductor) sensors.
[0379] Examples of the configuration of the camera device of the present invention can be listed below. Figure 1 The example camera module is shown in the image.
[0380] Figure 1 (a) is a schematic diagram illustrating the camera module of a small digital camera used in smartphones and the like. Figure 1 (a) The camera module shown has 1 (or more than 1 integer n) lenses L (or lenses L1...Ln), the filter 1 of the present invention, and the image sensor IC.
[0381] in addition, Figure 1 (b) is a schematic diagram illustrating the camera module of a digital single-lens reflex camera. Figure 1 (b) shows a camera module having a lens L, a filter 1 of the present invention, a cover glass CG, and an image sensor IC.
[0382] According to the present invention, an imaging device having a filter is provided, wherein the filter is provided with a resin film having high adhesion to an absorbing glass substrate made of phosphate-based glass or fluorophosphate glass.
[0383] Example
[0384] The present invention will be further illustrated below by way of examples and comparative examples, but the present invention is not limited to the following examples.
[0385] (Examples 1-7, Comparative Example 1)
[0386] 1. Preparation of coating solution containing coupling agent
[0387] (1) Weigh 0.3 mL of 0.5 N (mol / L) HCl aqueous solution and 2.2 mL of 2-methoxyethanol in a container and mix them in a sealed container.
[0388] (2) Tetraethyl orthosilicate (Si(OC2H5)4) was added to the above container and mixed for 30 minutes under a sealed environment, causing the reaction represented by the following reaction formula to occur.
[0389] Si(OC2H5)4+H2O→HO-Si(OC2H5)3+C2H5OH
[0390] Through the above reaction, water is completely consumed and hydroxyl groups are generated. Therefore, even if an alkoxide of Ti with a fast hydrolysis rate is added, hydroxide will not precipitate, and the solution can be expected to become homogeneous.
[0391] (3) Titanium butoxide (IV) (Ti(OC4H9)4) was further added to the above container according to the proportions shown in Table 1, and mixed for 30 minutes under sealed conditions to prepare a coating solution containing coupling agent. Table 1 shows the addition proportions of HO-Si(OC2H5)3 and Ti(OC4H9)4 when the total amount of HO-Si(OC2H5)3 and Ti(OC4H9)4 was set to 100 mol%.
[0392] It should be noted that the reaction represented by the following reaction formula is assumed to have occurred inside the container at this time.
[0393] 4OH-Si(OC2H5)3+Ti(OC4H9)4→Ti(O-Si(OC2H5)3)4+4C4H9OH
[0394] 2. Formation of the coating film
[0395] In a container containing the above-mentioned coating solution containing coupling agent, 1.2 mL of 0.5 N HCl aqueous solution, 4.7 mL of water, and 8.1 mL of 2-methoxyethanol were weighed and mixed for 30 minutes under a sealed environment to prepare the coating film forming solution.
[0396] At this point, it is assumed that the reaction represented by the following reaction formula occurred inside the container.
[0397] Ti{(O-Si(OC2H5)3}4+12H2O→Ti{(O-Si(OH)3}4+12C2H5OH
[0398] HO-Si(OC2H5)3+3H2O→Si(OH)4+3C2H5OH
[0399] The resulting coating film forming solution was prepared using a spin coater to a concentration of 0.03 mL / cm². 2 The coating is applied to an absorbent glass substrate (HOYA Corporation CD700, 0.59 mm thick) made of fluorophosphate glass.
[0400] An absorbent glass substrate coated with the above-mentioned coating film forming liquid was placed on a hot plate heated to 250°C and heated for 30 minutes to dehydrate and condense, thereby producing an absorbent glass substrate (hereinafter referred to as "evaluation substrate 1") with a cured film (bonding layer) on its surface.
[0401] In the above embodiments and comparative examples, multiple evaluation substrates 1 were prepared as follows: (1) an untreated evaluation substrate, (2) an evaluation substrate treated by boiling, (3) an evaluation substrate treated by a high-accelerated life test apparatus (PCT treatment), or (4) an evaluation substrate subjected to high temperature and high humidity treatment.
[0402] The contents of the above-mentioned boiling treatment, high-accelerated life test device treatment (PCT treatment) and high temperature and high humidity treatment are described as follows.
[0403] (Boiling treatment)
[0404] The evaluation substrate was immersed in a boiling hot water bath and boiled for another 60 minutes. The evaluation substrate was then removed and dried by blowing nitrogen gas.
[0405] (Highly Accelerated Life Testing Equipment Treatment (PCT Treatment))
[0406] The evaluation substrate was placed in a highly accelerated life test apparatus (ESPEC Corporation EHS-411M) and subjected to pressure treatment at 0.13 MPa for 72 hours at a temperature of 135°C and a humidity of 85% before being removed.
[0407] (High temperature and high humidity treatment)
[0408] The evaluation substrate was placed in a high temperature and high humidity test chamber (ESPEC Corporation PL-2KPH) and treated for 1000 hours at 85°C and 85% humidity before being removed.
[0409] For the above-mentioned (1) untreated evaluation substrate, (2) boiled evaluation substrate, (3) highly accelerated life test (PCT) treated evaluation substrate and (4) high temperature and high humidity treated evaluation substrate, an adhesion cross-section test was performed on the side with the above-mentioned cured film in accordance with JIS5600-5-6.
[0410] The test results at this time were classified based on the following evaluation criteria 0 to 5, and the results are shown in Table 1.
[0411] 0: The cut edges are completely smooth, and no eye of any grid cell has been peeled off;
[0412] 1: At the intersection of the cuts, the laminates have small peeling, less than 5% peeling per unit area;
[0413] 2: The coating peels off along the cut edge and / or at the intersection, with a peel of more than 5% and less than 15% per unit area;
[0414] 3: Large peeling of the coating along the cut edge in local or entire areas, and / or peeling of various parts of the eye in local or entire areas, with peeling of more than 15% and 35% per unit area.
[0415] 4: Large peeling of the coating occurs locally or throughout the entire surface along the cut edge, and / or peeling occurs locally or throughout the entire surface at several locations, less than 35% peeling per unit area;
[0416] 5: More than 35% of the area is stripped.
[0417] (Example 8)
[0418] Zirconium(IV)-butanol (Zr(OC4H9)4) was used instead of titanium(IV)-butanol (Ti(OC4H9)4) in Example 6. Otherwise, the same coupling agent coating solution was prepared as in Example 6, and an evaluation substrate with the coating film was made. The cross-section test was also performed, and the results are shown in Table 2.
[0419] (Example 9)
[0420] Aluminum n-butanol (Al(OC4H9)3) was used instead of titanium n-butoxide (IV) (Ti(OC4H9)4) in Example 3. Otherwise, the same coupling agent coating solution was prepared as in Example 3, and an evaluation substrate with the coating film was made. The cross-section test was also performed, and the results are shown in Table 3.
[0421] (Examples 10-12)
[0422] 1. Preparation of coating solution containing coupling agent
[0423] (1) Weigh 0.3 mL of 0.5 N (mol / L) HCl aqueous solution and 2.2 mL of 2-methoxyethanol in a container and mix them in a sealed container.
[0424] (2) Tetraethyl orthosilicate (Si(OC2H5)4) was added to the above container and mixed for 30 minutes under a sealed environment, causing the reaction represented by the following reaction formula to occur.
[0425] Si(OC2H5)4+H2O→HO-Si(OC2H5)3+C2H5OH
[0426] Through the above reaction, all water is consumed and hydroxyl groups are generated. Therefore, even if an alkoxide of Ti with a fast hydrolysis rate is added, hydroxide will not precipitate, and the solution is expected to become homogeneous.
[0427] (3) By further adding tetra-n-butoxy titanium polymer (Ti4O3(OC4H9)) to the above-mentioned container in the proportions shown in Table 4. 10The mixture was then stirred in a sealed container for 30 minutes to prepare a coating solution containing the coupling agent. It should be noted that the reaction represented by the following equation is assumed to have occurred within the container at this time.
[0428] 10OH-Si(OC2H5)3+Ti4O3(OC4H9) 10 →Ti4O3(O-Si(OC2H5)3) 10 +10C4H9OH
[0429] Using Ti7O6(OC4H9) 16 (Example 11) and Ti 10 O9(OC4H9) 22 (Example 12) to replace Ti4O3(OC4H9) 10 (Example 10) A coating solution was prepared similarly. Table 4 shows the proportions of silicon and titanium compounds in each coating solution. It should be noted that the proportions shown in Table 4 refer to the ratio of HO-Si(OC2H5)3 to Ti (general formula). k O k-1 (OC4H9) 2k+2 The total amount of each titanium compound is set to 100 mol% when the proportions of HO-Si(OC2H5)3 and the titanium compounds are shown.
[0430] 2. Formation of the coating film
[0431] In a container containing the above-mentioned coating solution containing coupling agent, 1.2 mL of 0.5 N HCl aqueous solution, 4.7 mL of water, and 8.1 mL of 2-methoxyethanol were weighed and mixed for 30 minutes under a sealed environment to prepare the coating film forming solution.
[0432] For example, when using Ti4O3(OC4H9) 10 Under certain conditions, the following reaction, represented by the following reaction formula, occurred inside the container.
[0433] Ti4O3{O-Si(OC2H5)3} 10 +30H2O→Ti4O3{(O-Si(OH)3} 10 +30C2H5OH
[0434] HO-Si(OC2H5)3+3H2O→Si(OH)4+3C2H5OH
[0435] The obtained coating film forming solution was applied using a spin coater at a concentration of 0.03 mL / cm². 2 The coating is applied to an absorbent glass substrate (HOYA Corporation CD700, 0.59 mm thick) made of fluorophosphate glass.
[0436] An absorbent glass substrate coated with the above-mentioned coating film forming liquid was placed on a hot plate heated to 250°C and heated for 30 minutes to dehydrate and condense, thereby producing an absorbent glass substrate (evaluation substrate 1) with a cured film (bonding layer) on its surface.
[0437] 3. Formation of the resin film
[0438] On the absorbent glass substrate with a cured film (bonding layer) on the surface obtained by the above process, a resin film is further formed in the following order.
[0439] (1) Weigh 0.2g of polyvinyl butyral resin and 1.8g of cycloheptanone in a container and mix them in a sealed container.
[0440] (2) 0.09 g of toluene diisocyanate was added to the above container and mixed in a sealed environment to prepare a resin film forming solution.
[0441] (3) Using a spin coater, the obtained resin film forming solution was prepared at a concentration of 0.03 mL / cm³. 2 The coating is applied to an absorbent glass substrate having a cured film (bonding layer) on its surface, obtained through the above process.
[0442] (4) The absorbent glass substrate coated with the above-mentioned resin film forming liquid was placed on a hot plate heated to 160°C and heated for 20 minutes to solidify it, thereby producing a glass substrate with a resin film on its surface (evaluation substrate 2).
[0443] In the above Examples 10 to 12, for the evaluation substrate 1, which only has a cured film (bonding layer) formed, and the evaluation substrate 2, which has a resin film further formed on the bonding layer, as described below, (1) an untreated evaluation substrate and (2) an evaluation substrate that has undergone boiling treatment in the same manner as in Examples 1 to 9.
[0444] For the untreated evaluation substrate (1) and the evaluation substrate treated by boiling, an adhesion cross-section test was performed on the side of the evaluation substrate 1 with the cured film (bonding layer) or the side of the evaluation substrate 2 with the resin film, in accordance with the provisions of JIS5600-5-6. The evaluation was performed based on evaluation criteria 0 to 5 in the same manner as in Examples 1 to 9, and the results are shown in Table 4.
[0445] In addition, STEM-EDX measurements were performed on the evaluation substrate 2 obtained in Example 11 to obtain STEM-EDX lines (EDX ray detection intensity lines of each element constituting the filter in the depth direction). The proportion α (atomic %) of Ti atoms in the total number of Si atoms and Ti atoms constituting the bonding layer portion and the proportion β (atomic %) of Si atoms in the total number of Si atoms and Ti atoms were calculated according to the following formula.
[0446] [Mathematical Expression 5]
[0447]
[0448] [Mathematical Expression 6]
[0449]
[0450] (It should be noted that X) Si This refers to the cumulative intensity of EDX rays and X-rays of Si atoms in the region constituting the bonding layer. Ti This refers to the cumulative intensity of EDX rays and K in the region constituting the bonding layer of Ti atoms. Si This refers to the k-factor (correction coefficient) of Si atoms, K Ti This refers to the k-factor (correction coefficient) of Ti atoms, M Si This refers to the atomic weight of Si atoms, M Ti This refers to the atomic weight of Ti atoms.
[0451] The results are shown in Table 5.
[0452] [Table 1]
[0453]
[0454] [Table 2]
[0455]
[0456] [Table 3]
[0457]
[0458] [Table 4]
[0459]
[0460] [Table 5]
[0461]
[0462] As shown in Tables 1 to 3, in Examples 1 to 9, the cured film formed on the absorbing glass substrate contains the general formula M{OSi(OR) 7 (OR)8 (OR) 9 )} n The solidified film (bonding layer) of the hydrolysis and dehydration condensate of the specific coupling agent indicates that it has high adhesion to the absorbing glass substrate.
[0463] Furthermore, as shown in Tables 4 and 5, in Examples 10 to 12, the cured film (bonding layer) or resin film formed on the absorbing glass substrate contains the general formula (Ti). k O k-1 ){OSi(OR 10 (OR) 11 (OR) 12 )} 2k+2 The cured film (bonding layer) of the hydrolysis and dehydration condensate of the specific coupling agent, or the resin film formed on the cured film (bonding layer), exhibits high adhesion to the absorbent glass substrate. It is evident that, particularly in Examples 10-12, even with a low proportion (mol%) of the titanium compound constituting the cured film, the adhesion is superior compared to Examples 1-3, where the proportion (mol%) of the titanium compound is the same. Therefore, it is clear that using a polymer as the titanium compound allows for superior adhesion at a lower content compared to using a monomer.
[0464] On the other hand, as shown in Table 1, in Comparative Example 1, the cured film (bonding layer) formed on the absorbent glass substrate does not contain hydrolysis and dehydration condensates of the specific coupling agent. Therefore, especially in the presence of moisture, the adhesion to the absorbent glass substrate is poor.
[0465] Industrial applicability
[0466] According to the present invention, an infrared cut-off filter having a resin film having high adhesion to an absorbing glass substrate made of phosphate-based glass or fluorophosphate glass can be provided, and an imaging device having the above-mentioned infrared cut-off filter can be provided.
Claims
1. A filter comprising a resin film disposed on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer comprises MO-Si bonds, wherein, M is selected from one or more of Ti atoms, Zr atoms, and Al atoms, and the bonding layer has a single-layer structure. In the bonding layer, the total number of Ti atoms, Zr atoms, and Al atoms accounts for a proportion greater than 0 atomic% and less than 33.3 atomic% of the total number of Si atoms, Ti atoms, Zr atoms, and Al atoms.
2. The filter according to claim 1 is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer comprises a hydrolysis and dehydration condensate of one or more coupling agents selected from compounds represented by general formula (I) and compounds represented by general formula (II). M(OSiR 1 R 2 R 3 ) n (AND) In formula (I), M is a Ti atom, Zr atom, or Al atom, and R 1 R 2 and R 3 It is a straight-chain or branched hydrocarbon group containing 1 to 10 carbon atoms, which may be the same or different. n is 4 when M is a Ti atom or a Zr atom, and 3 when M is an Al atom. Multiple -OSiR 1 R 2 R 3 The bases can be the same or different. (Ti k ABOUT k-1 )(OSiR 4 R 5 R 6 ) 2k+2 (II) In equation (II), R 4 R 5 and R 6 It is a linear or branched hydrocarbon group containing 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSiR groups are allowed. 4 R 5 R 6 The bases can be the same or different.
3. The filter according to claim 1 is formed by depositing a resin film on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, wherein the bonding layer comprises a hydrolysis and dehydration condensate of one or more coupling agents selected from compounds represented by general formula (III) and compounds represented by general formula (IV). M{OSi(OR 7 )(OR 8 )(OR 9 )} n (III) In formula (III), M is a Ti atom, a Zr atom, or an Al atom, and R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups can be the same or different. n is 4 when M is a Ti or Zr atom, and 3 when M is an Al atom. Multiple -OSi (OR) 7 (OR) 8 (OR) 9 The bases can be the same or different. (Ti k O k-1 ){OSi(OR 10 )(OR 11 )(OR 12 )} 2k+2 (IV) In equation (IV), R 10 R 11 and R 12 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSi (OR) groups. 10 (OR) 11 (OR) 12 The bases can be the same or different.
4. The filter according to claim 3, wherein, The coupling agent represented by general formula (III) is a silicon compound represented by general formula (V) and a reactant selected from one or more metal alkoxides represented by general formulas (VI), (VII), and (VIII). Si(OR 7 )(OR 8 )(OR 9 )OH (V) In equation (V), R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Ti(OR 13 )(OR 14 )(OR 15 )(OR 16 ) (VI) In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Zr(OR 17 )(OR 18 )(OR 19 )(OR 20 ) (VII) In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Al(OR 21 )(OR 22 )(OR 23 ) (VIII) In equation (VIII), R 21 R 22 and R 23 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
5. The filter according to claim 1, wherein, The bonding layer also contains a dehydrated condensate of silanol.
6. The filter according to claim 1, wherein a resin film is disposed on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass through a bonding layer, the bonding layer comprising a hydrolyzed and dehydrated condensate of a coupling agent composition, the coupling agent composition containing 50 mol% or more and less than 100 mol% of a silicon compound represented by the following general formula (V), and more than 0 mol% and less than 50 mol% of one or more reactants selected from the following general formulas (VI), (VII), and (VIII). Si(OR 7 )(OR 8 )(OR 9 )OH (V) In equation (V), R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Ti(OR 13 )(OR 14 )(OR 15 )(OR 16 ) (VI) In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Zr(OR 17 )(OR 18 )(OR 19 )(OR 20 ) (VII) In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Al(OR 21 )(OR 22 )(OR 23 ) (VIII) In equation (VIII), R 21 R 22 and R 23 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
7. The filter according to claim 6, wherein, The coupling agent composition is a silicon compound represented by the general formula (V) of greater than 80 mol% and less than 100 mol% and a reactant of one or more metal alkoxides selected from the general formulas (VI) to (VIII) of greater than 0 mol% and less than 20 mol%.
8. The filter according to claim 6, wherein, The coupling agent composition is 85-94 mol% of a silicon compound represented by the general formula (V) and 6-15 mol% of a reaction product of one or more metal alkoxides selected from the general formulas (VI) to (VIII).
9. A filter comprising a resin film disposed on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass, wherein the resin film contains MO-Si bonds, wherein... M is selected from one or more of Ti atoms, Zr atoms, and Al atoms. In the resin film, the total number of Ti atoms, Zr atoms, and Al atoms accounts for a proportion greater than 0 atomic% and less than 33.3 atomic% in the total number of Si atoms, Ti atoms, Zr atoms, and Al atoms.
10. The filter according to claim 9, wherein a resin film is disposed on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass, the resin film comprising a hydrolysis and dehydration condensate of one or more coupling agents selected from compounds represented by general formula (I) and compounds represented by general formula (II). M(OSiR 1 R 2 R 3 ) n (AND) In formula (I), M is a Ti atom, Zr atom, or Al atom, and R 1 R 2 and R 3 It is a straight-chain or branched hydrocarbon group containing 1 to 10 carbon atoms, which may be the same or different. n is 4 when M is a Ti atom or a Zr atom, and 3 when M is an Al atom. Multiple -OSiR 1 R 2 R 3 The bases can be the same or different. (Ti k ABOUT k-1 )(OSiR 4 R 5 R 6 ) 2k+2 (II) In equation (II), R 4 R 5 and R 6 It is a linear or branched hydrocarbon group containing 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSiR groups are allowed. 4 R 5 R 6 The bases can be the same or different.
11. The filter according to claim 9, wherein a resin film is disposed on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass, the resin film comprising a hydrolysis and dehydration condensate of one or more coupling agents selected from compounds represented by general formula (III) and compounds represented by general formula (IV). M{OSi(OR 7 )(OR 8 )(OR 9 )} n (III) In formula (III), M is a Ti atom, a Zr atom, or an Al atom, and R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups can be the same or different. n is 4 when M is a Ti or Zr atom, and 3 when M is an Al atom. Multiple -OSi (OR) 7 (OR) 8 (OR) 9 The bases can be the same or different. (Ti k O k-1 ){OSi(OR 10 )(OR 11 )(OR 12 )} 2k+2 (IV) In equation (IV), R 10 R 11 and R 12 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, which may be the same or different; k is a real number greater than 2 and less than 15; and multiple -OSi (OR) groups. 10 (OR) 11 (OR) 12 The bases can be the same or different.
12. The filter according to claim 11, wherein, The coupling agent represented by general formula (III) is a silicon compound represented by general formula (V) and a reactant selected from one or more metal alkoxides represented by general formulas (VI), (VII), and (VIII). Si(OR 7 )(OR 8 )(OR 9 )OH (V) In equation (V), R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Ti(OR 13 )(OR 14 )(OR 15 )(OR 16 ) (VI) In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Zr(OR 17 )(OR 18 )(OR 19 )(OR 20 ) (VII) In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Al(OR 21 )(OR 22 )(OR 23 ) (VIII) In equation (VIII), R 21 R 22 and R 23 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
13. The filter according to claim 9, wherein, The resin film also contains a dehydrated condensate of silanol.
14. The filter according to claim 9, wherein a resin film is disposed on an absorbing glass substrate made of phosphate-based glass or fluorophosphate-based glass, the resin film comprising a hydrolyzed and dehydrated condensate of a coupling agent composition, the coupling agent composition comprising 50 mol% or more and less than 100 mol% of a silicon compound represented by the following general formula (V), and more than 0 mol% and less than 50 mol% of one or more reactants selected from the following general formulas (VI), (VII), and (VIII). Si(OR 7 )(OR 8 )(OR 9 )OH (V) In equation (V), R 7 R 8 and R 9 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Ti(OR 13 )(OR 14 )(OR 15 )(OR 16 ) (VI) In equation (VI), R 13 R 14 R 15 and R 16 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Zr(OR 17 )(OR 18 )(OR 19 )(OR 20 ) (VII) In equation (VII), R 17 R 18 R 19 and R 20 It consists of straight-chain or branched hydrocarbon groups having 1 to 10 carbon atoms, and these groups may be the same or different. Al(OR 21 )(OR 22 )(OR 23 ) (VIII) In equation (VIII), R 21 R 22 and R 23 It consists of straight-chain or branched hydrocarbon groups with 1 to 10 carbon atoms, and these groups may be the same or different.
15. The filter according to claim 14, wherein, The coupling agent composition is a reaction product of a silicon compound represented by general formula (V) of greater than 80 mol% and less than 100 mol% and one or more metal alkoxides represented by general formulas (VI) to (VIII) of greater than 0 mol% and less than 20 mol%.
16. The filter according to claim 14, wherein, The coupling agent composition is 85-94 mol% of a silicon compound represented by general formula (V) and 6-15 mol% of one or more metal alkoxides represented by general formulas (VI) to (VIII).
17. A camera device comprising a solid-state camera, a camera lens, and a filter according to any one of claims 1 to 16.
Citation Information
Patent Citations
Resin composition and near-infrared ray cut filter
JP2014148567A
Near-infrared cut filter and solid-state imaging device
CN104755969A
Organic-inorganic hybrids surface adhesion promoter
US20020123592A1