Secondary battery first charge and discharge method

By using the negative electrode sheet with an active metal supplementary layer in the secondary battery to perform a discharge process that consumes residual metal after the first charge, the problem of low efficiency of the secondary battery during the first charge and discharge is solved, and the cell performance and cycle life are improved. A low-cost, significant improvement in battery performance is achieved.

CN116598620BActive Publication Date: 2024-10-01JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310528474.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-10-01
Estimated Expiration
2043-05-11

AI Technical Summary

Technical Problem

When existing secondary batteries are first charged and discharged, active metals are rapidly consumed, resulting in low efficiency, irreversible cycle processes, and rapid capacity attenuation. In addition, existing methods for improving lithium replenishment efficiency are costly and have limited effects.

Method used

Using a negative electrode sheet with an active metal supplementary layer, the residual metal is consumed by the first step of discharge after the first charge, followed by at least two steps of discharge. The discharge current of the first step is smaller than the subsequent discharge current, and the discharge amount is in the range of 3-10%. This process is used to improve the utilization of active metals and cell performance.

Benefits of technology

It effectively reduces the residual metal content, increases the utilization rate of the negative active metal, improves the performance of the secondary battery, is simple to operate, has low cost, and significantly improves the energy density and cycle life of the battery core.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116598620B_ABST
    Figure CN116598620B_ABST
Patent Text Reader

Abstract

The disclosed embodiment provides a method for charging and discharging a secondary battery for the first time, by charging the secondary battery for the first time, discharging the secondary battery for the first time in the first step to consume the residual metal in the active metal replenishment layer, and discharging the second battery after the first step of discharge in at least two steps. The disclosed embodiment designs the first discharge process with an active metal replenishment layer, and utilizes the first step of discharge to consume the residual metal in the active metal layer, so that the residual metal of the battery after the first charge participates in the discharge consumption, further reducing the content of residual metal, indirectly improving the utilization rate of the negative electrode active metal, and improving the performance of the secondary battery. Based on the relevant technology, this method does not improve the raw materials. By designing the first discharge process, it improves the active metal replenishment efficiency, improves the performance of the battery cell, is simple to operate, low cost, and has significant effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of secondary batteries, and in particular to a method for charging and discharging a secondary battery for the first time. Background Art

[0002] A secondary battery (rechargeable battery), also known as a rechargeable battery or storage battery, refers to a battery that can be recharged to activate the active material after being discharged and continue to be used.

[0003] Currently, secondary batteries include a battery core composed of a positive electrode sheet, a negative electrode sheet and a separator located between the positive electrode sheet and the negative electrode sheet. The battery core is placed in an electrolyte, and the secondary battery works by moving metal ions between the positive electrode and the negative electrode.

[0004] Therefore, how to improve the battery performance of metal secondary batteries is a topic that the industry generally considers. Summary of the invention

[0005] In view of the above shortcomings of the related art, an object of the present disclosure is to provide a method for charging and discharging a secondary battery for the first time, so as to solve the technical problem of low performance of the secondary battery in the related art.

[0006] The first aspect of the present disclosure provides a method for charging and discharging a secondary battery for the first time. The secondary battery includes a negative electrode sheet having an active metal supplement layer. The method for charging and discharging the secondary battery includes:

[0007] Charging the secondary battery for the first time;

[0008] performing a first step of discharging the first-charged secondary battery to consume residual metal in the active metal replenishment layer;

[0009] The second battery after the first step of discharge is discharged in at least two steps.

[0010] Optionally, the current of the first step current is less than a preset value.

[0011] Optionally, the current of the first step discharge is smaller than the current of at least two steps of discharge after the first step discharge.

[0012] Optionally, the first discharge step uses a current of 0.01-0.2C for constant current discharge.

[0013] Optionally, the current range of at least two steps of discharge after the first step of discharge is 0.01-20C.

[0014] Optionally, the discharge amount of the first step of discharging ranges from 3-10%.

[0015] Optionally, the secondary battery after the first step of discharge is discharged in at least two steps, including:

[0016] Performing a second step of discharging the secondary battery after the first step of discharging;

[0017] The second battery after the second step discharge is charged and the third step discharge is performed after the charging.

[0018] Optionally, the secondary battery is a lithium-ion battery, and the active metal supplement layer is a lithium supplement layer.

[0019] Optionally, the lithium supplement layer is at least one of lithium foil and lithium powder.

[0020] Optionally, the lithium foil is at least one of rolled intermittent zebra-pattern lithium supplementation, stripe-pattern lithium supplementation, and full-film lithium supplementation.

[0021] As described above, the first charge and discharge method of a secondary battery is provided in the embodiment of the present disclosure, by charging the secondary battery for the first time, performing the first discharge on the first charged secondary battery to consume the residual metal in the active metal replenishment layer, and performing at least two discharges on the second battery after the first discharge. The embodiment of the present disclosure designs the first discharge process with an active metal replenishment layer, and utilizes the first discharge to consume the residual metal in the active metal layer, so that the residual metal of the battery after the first charge participates in the discharge consumption, further reducing the content of residual metal, indirectly improving the utilization rate of the negative electrode active metal, and improving the performance of the secondary battery. Based on the relevant technology, this method does not improve the raw materials. By designing the first discharge process, it improves the active metal replenishment efficiency, improves the performance of the battery cell, is simple to operate, low cost, and has significant effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram showing a discharge curve of a secondary battery of the related art after the first charge and discharge.

[0023] Figure 2 A flow chart showing a method for charging and discharging a secondary battery for the first time according to an embodiment of the present disclosure.

[0024] Figure 3 A comparison chart showing the discharge curves after the second charge and the first charge and discharge method.

[0025] Figure 4 exhibit Figure 3 A partial enlarged view of the discharge curve in the initial stage after the second charge is shown. DETAILED DESCRIPTION

[0026] The following describes the embodiments of the present disclosure through specific examples, and those skilled in the art can easily understand other advantages and effects of the present disclosure from the information disclosed in the present disclosure. The present disclosure can also be implemented or applied through other different specific embodiments, and the details in the present disclosure can also be modified or changed in various ways according to different viewpoints and application systems without departing from the spirit of the present disclosure. It should be noted that the embodiments and features in the embodiments in the present disclosure can be combined with each other without conflict.

[0027] The following is a detailed description of the embodiments of the present disclosure with reference to the accompanying drawings so that those skilled in the art can easily implement the present disclosure. The present disclosure can be embodied in many different forms and is not limited to the embodiments described herein.

[0028] In the representations of the present disclosure, the reference terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" and the like mean that the specific features, structures, materials, or characteristics represented in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure. Moreover, the specific features, structures, materials, or characteristics represented may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples represented in the present disclosure and the features of different embodiments or examples, unless they are mutually contradictory.

[0029] Although not defined differently, all terms, including technical and scientific terms used herein, have the same meaning as those generally understood by those skilled in the art to which the present disclosure belongs. Terms defined in commonly used dictionaries are additionally interpreted as having meanings consistent with relevant technical literature and the message of the present disclosure, and shall not be overly interpreted as ideal or very formal meanings unless defined.

[0030] In the related art, research on the working principle of secondary batteries found that during the first charge and discharge, the electrolyte undergoes a reduction reaction on the surface of the negative electrode to produce a large amount of organic or inorganic products, which are deposited on the surface of the negative electrode to form a dense passivation film, namely the solid electrolyte interface (SEI) film.

[0031] During the first charge and discharge process, there is a rapid consumption of active metals, such as SEI film formation and repair, deactivation of negative electrode active sites, and irreversible deposition of active metals, which leads to low first efficiency, reversible cycle process, and rapid capacity decay.

[0032] Therefore, in the relevant technology, the energy density and cycle life of the battery cell can be significantly improved by slowing down or supplementing the consumption of active metals in the SEI film formation process to achieve the first efficiency improvement.

[0033] Taking lithium-ion batteries as an example, the relevant technologies for lithium replenishment include pre-lithiation, among which negative electrode lithium replenishment is a common pre-lithiation technology. The so-called negative electrode lithium replenishment refers to setting a lithium replenishment layer on the negative electrode sheet, using an external lithium source to replenish the film consumption of the SEI film, and greatly improving the initial efficiency of the battery cell.

[0034] When the secondary battery after lithium supplementation at the negative electrode was tested for the first time for charge and discharge, it was found that Figure 1 As shown in the figure, after the first charge, there is an additional discharge platform in the early stage of the discharge process of the lithium supplement group. This platform is the voltage platform of the negative electrode lithium metal to the positive electrode LFP (Lithium iron phosphate, also known as lithium iron phosphate, lithium iron phosphate) during the discharge process. The generation of this platform indicates that there is still residual lithium in the negative electrode after pre-lithiation. This part of lithium will react with the electrolyte in the later stage and affect the performance of the battery. At the same time, the existence of this platform indicates that after the pre-lithiation is completed, the remaining lithium in the early stage of charge and discharge is not completely passivated and can still participate in the charge and discharge reaction. As the charge and discharge cycle proceeds, this part of lithium is gradually passivated to form dead lithium, thereby deteriorating the battery performance.

[0035] At present, in the relevant technologies, the main methods to improve the efficiency of lithium replenishment are: coated modified lithium powder, core-shell structure lithium powder, high expansion negative electrode materials, lithium zebra intermittent stripes lithium replenishment, micron-scale microporous lithium membrane, etc. Among them, in the core-shell structure lithium powder, the core is a conductive material, and the shell is lithium metal. After pre-lithiation, the pole piece structure is stabilized to improve the transmission of electrons and ions. For high expansion negative electrode materials, the expansion of the material in the later stage of lithium replenishment is utilized. Under the action of the expanded lithium, the dead lithium structure breaks and can continue the pre-lithiation reaction to provide active lithium. Compared with the full lithium membrane covering the pole piece, the intermittent zebra stripes lithium replenishment reduces the area affected by dead lithium on the pole piece. The micron-scale microporous lithium membrane uses the micropores of the lithium membrane to improve the pre-lithiation efficiency and improve the impact of dead lithium in pre-lithiation.

[0036] However, for lithium powder modification, the cost of lithium powder itself is extremely high, and further modification will increase the cost again and the improvement effect is limited. High-expansion negative electrode materials limit the system and have a narrow application range. In addition, the overall performance of batteries using high-expansion negative electrode materials is poor and the life is short. As for the intermittent stripe lithium replenishment of lithium belts, with the same lithium replenishment amount design, the use of intermittent lithium replenishment means that after the lithium replenishment layer is depleted, there will be more dead lithium in the lithium replenishment layer after pre-lithiation and it will be more protruding, which is easy to form lithium dendrites and affect the safety performance of the battery cell. For micron-scale microporous lithium membranes, the material manufacturing cost increases, the lithium membrane has poor timeliness, and the micron-scale lithium membrane has high requirements for timeliness. It will fail after a long time of storage and cannot be coated on the negative electrode sheet.

[0037] In view of the problems existing in the related art, the embodiments of the present disclosure analyze the above problems in the field of lithium batteries and propose an improvement solution that can be applied to more secondary batteries to improve the performance of secondary batteries.

[0038] Figure 2 The first charge and discharge method of a secondary battery proposed in an embodiment of the present disclosure is presented, wherein the secondary battery includes a negative electrode sheet having an active metal supplement layer, and the charge and discharge method of the secondary battery includes:

[0039] Step 210: charging the secondary battery for the first time;

[0040] Step 220: performing a first discharge on the first-charged secondary battery to consume residual metal in the active metal replenishment layer;

[0041] Step 230: performing at least two-step discharge on the second battery after the first-step discharge.

[0042] The disclosed embodiment designs the first discharge process with an active metal supplement layer, and uses the first discharge to consume the residual metal of the active metal layer, so that the residual metal of the battery after the first charge participates in the discharge consumption, further reducing the content of residual metal, indirectly improving the utilization rate of the negative electrode active metal, and improving the performance of the secondary battery. Based on the relevant technology, this method does not improve the raw materials. By designing the first discharge process, it improves the active metal supplement efficiency and the performance of the battery cell, and is simple to operate, low cost, and effective.

[0043] Taking lithium-ion batteries as an example, by designing the first discharge process of the negative electrode lithium-replenishing battery cell, the residual lithium content is further reduced after the pre-lithiation is completed, which indirectly improves the utilization rate of the negative electrode lithium replenishment, reduces the amount of dead lithium, and further improves the performance of the lithium-replenishing battery cell.

[0044] Figure 3 Shows the comparison of discharge curves after the second charge after the first charge and discharge method. Figure 4 exhibit Figure 3 The figure is a partial enlarged diagram of the discharge curve in the initial stage after the second charge, wherein the solid line is an embodiment of the charge and discharge method using the embodiment of the present disclosure, and the dotted line is a comparative example.

[0045] Among them, the comparison examples are as follows:

[0046] The negative electrode sheet is replenished with lithium through the calendering lithium replenishment process, and then wound with the positive electrode sheet and separator to make a bare battery cell, and assembled into a punched aluminum-plastic film, after top sealing and liquid injection, it is left to stand after sealing, fully charged after formation, discharged at 0.5C constant current to 2.0V, and finally charged to 3.65V with 0.5C constant current and constant voltage, with a cut-off current of 0.05C and a constant current discharge of 0.5C to 2.0V.

[0047] The examples are as follows:

[0048] The negative electrode sheet is replenished with lithium through the calendering lithium replenishment process, and then it is wound with the positive electrode sheet and the separator to make a bare battery cell, and assembled into a punched aluminum-plastic film. After top sealing and liquid injection, it is left to stand after sealing, fully charged after formation, and a step-by-step discharge process is adopted: the first step is 0.1C discharge for 30 minutes, that is, 5% SOC, the second step is 0.5C constant current discharge to 2.0V, and finally 0.5C constant current and constant voltage charge to 3.65V, the cut-off current is 0.05C, and 0.5C constant current discharge to 2.0V.

[0049] Performance test through the second charge and discharge:

[0050] For the above soft-pack battery, the potential of the discharge curve changes during the second charge and discharge: 0.5C constant current and constant voltage charging to 3.65V, cut-off current 0.05C, 0.5C constant current discharge to 2.0V.

[0051] Combination Figure 2 and Figure 3 As shown, after the lithium-replenished battery cell is fully charged for the first time, the potential of the secondary battery using the step discharge process of the embodiment of the present disclosure decreases at the initial stage of discharge. The potential at this point is mainly affected by the residual lithium content after pre-lithiation. The lower the residual lithium content, the lower the potential. This shows that the embodiment of the present disclosure helps to improve the efficiency of lithium replenishment, reduce dead lithium, and improve the performance of the battery cell. It is also simple to operate, low cost, and has significant effects.

[0052] In the embodiment of the present disclosure, the secondary battery may also be a magnesium ion battery, a sodium ion battery, an aluminum ion battery, etc., which are not listed here one by one. For different types of secondary batteries, the active metal selects the corresponding type of active metal.

[0053] In the disclosed embodiment, the secondary battery is charged to full charge for the first time. The current of the first discharge step is small, which can make the residual metal of the negative electrode of the secondary battery stay at the positive electrode discharge potential for a longer time, which is conducive to the participation of the residual metal in the discharge consumption. Taking lithium-ion batteries as an example, the current of the first discharge step is small, which makes the residual lithium of the secondary battery stay at the positive electrode discharge potential for a longer time after the negative electrode is pre-lithiated, which is conducive to the participation of the residual lithium in the discharge consumption after the pre-lithiation.

[0054] In the embodiment of the present disclosure, the current of the first discharge step may be less than a preset value, and the preset value may be set according to specific circumstances such as the type and parameters of the secondary battery, and is not limited here.

[0055] In the embodiment of the present disclosure, the current of the first discharge is smaller than the current of at least two discharges after the first discharge. The first discharge consumes the residual metal in the active metal supplementary layer, so the discharge current is smaller than the subsequent conventional discharge current.

[0056] In the embodiment disclosed herein, the first step of discharge uses a constant current discharge of 0.01-0.2C. This parameter can more thoroughly consume the residual metal in the active metal supplement layer. In other corresponding embodiments, if the parameter range is exceeded, the effect may be compromised, but it may also be exceeded without affecting the feasibility of the solution.

[0057] In the embodiment of the present disclosure, the current range of at least two steps of discharge after the first step of discharge is 0.01-20 C. The at least two steps of discharge after the second step of discharge are discharged to the termination voltage. Within the above parameter range, the secondary battery can be discharged more fully.

[0058] In the embodiment of the present disclosure, the discharge capacity range of the first step of discharge is 3-10% SOC. In the corresponding test, within this discharge capacity range, the residual metal can be fully consumed.

[0059] In one embodiment of the present disclosure, the secondary battery after the first step of discharge is discharged in at least two steps, including:

[0060] Performing a second step of discharging the secondary battery after the first step of discharging;

[0061] The second battery after the second step discharge is charged and the third step discharge is performed after the charging.

[0062] In the embodiment of the present disclosure, the secondary battery is a lithium-ion battery, and the active metal supplement layer is a lithium supplement layer.

[0063] In one embodiment, the lithium supplement layer is at least one of lithium foil or lithium powder.

[0064] In one embodiment, the lithium foil is at least one of rolled intermittent zebra-pattern lithium supplementation, stripe-pattern lithium supplementation, and full-film lithium supplementation.

[0065] In one embodiment, the lithium powder supplementation of the negative electrode lithium supplementation battery cell is at least one of lithium powder particles and slurry supplementation containing lithium powder.

[0066] In the disclosed embodiment, the secondary battery further includes a negative electrode sheet, a positive electrode sheet, a separator, and an electrolyte. The separator is located between the positive and negative electrode sheets. The battery cell is manufactured by a stacking or winding process, and the secondary battery is obtained by assembly, injection, and packaging.

[0067] In one embodiment, the negative electrode sheet includes a current collector and a negative electrode active material, the current collector is copper foil, and the negative electrode active material includes a negative electrode active material, a conductive agent, and a binder, and the proportions are 90% to 98%, 1% to 5%, and 1% to 5%, respectively. The negative electrode active material is at least one of artificial graphite, natural graphite, silicon oxygen negative electrode, silicon carbon negative electrode, mesophase carbon microspheres, hard carbon, and soft carbon. The conductive agent is at least one of conductive carbon black, acetylene black, Ketjen black, carbon nanofiber tubes, carbon nanotubes, single-walled carbon nanotubes, and graphene. The binder is at least one of fluorine-containing resin, polypropylene resin, polyacrylic acid and modified polyacrylic acid, polyaniline, polyimide, and rubber binders.

[0068] The positive electrode sheet includes a current collector and a positive electrode active material. The current collector is aluminum foil. The positive electrode active material includes a positive electrode active material, a conductive agent, and a binder, accounting for 90% to 98%, 1% to 5%, and 1% to 5% respectively. The positive electrode active material is at least one of lithium iron phosphate, lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium manganese oxide, cobalt-free layered positive electrode material, and lithium-rich manganese-based material. The conductive agent is at least one of conductive carbon black, acetylene black, Ketjen black, carbon nanofiber tubes, carbon nanotubes, single-walled carbon nanotubes, and graphene. The binder is at least one of fluorine-containing resin, polypropylene resin, fiber-type binder, or polyimide-type binder.

[0069] The isolation membrane is a porous sheet or layered membrane made of polyethylene, polypropylene, or non-woven fabric, and its surface can be coated with ceramic material or glue.

[0070] The electrolyte includes a non-aqueous organic solvent and a lithium salt, wherein the non-aqueous organic solvent is at least one of carbonate, carboxylate, ether and ketone solvents. The lithium salt is one or more of LiBF4, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, LiPO2F2, Li2PO3F and LiAsF6.

[0071] Taking lithium-ion batteries as an example, the preparation method thereof includes:

[0072] 1) Preparation of positive electrode sheet: LiFePO4, SP and PVDF are uniformly dispersed in NMP according to the mass ratio of 96.5%:1.5%:2% to form positive electrode slurry, which is then rolled after coating and drying, die-cut and baked for standby use.

[0073] 2) Preparation of negative electrode sheet: Preparation of graphite electrode sheet: artificial graphite, SP (super pll, i.e. conductive carbon black), (Ceramic Matrix Composite, i.e. ceramic matrix composite material), SBR (Polymerized Styrene Butadiene Rubber, i.e. styrene butadiene rubber) are uniformly dispersed in deionized water at a ratio of 95.4%:1.8%:1%:1.8% to form a negative electrode slurry, which is then coated and dried, rolled, die-cut, and baked for standby use; the obtained negative electrode sheet is replenished with lithium using a lithium belt calendering lithium replenishment process to obtain a lithium-replenished electrode sheet.

[0074] 3) Preparation of isolation membrane: A porous polymer membrane with a polyethylene substrate is used, and its surface is coated with ceramic and PVDF glue, and its specific thicknesses are 9um, 3um, and 2um respectively.

[0075] 4) Preparation of lithium-ion batteries: The prepared positive electrode sheet, negative electrode sheet after lithium supplementation, and separator are wound into bare cells according to the production process, and assembled into a punched aluminum-plastic film. After top sealing, liquid injection, standing after sealing, formation / cancellation of formation, aging, secondary sealing, capacity division and other processes, a soft-pack battery with a voltage range of 2.5 to 3.65V is obtained.

[0076] The above embodiments are merely illustrative of the principles and effects of the present disclosure, and are not intended to limit the present disclosure. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present disclosure. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present disclosure shall still be covered by the claims of the present disclosure.

Claims

1. A method for charging and discharging a secondary battery for the first time, characterized in that: The secondary battery comprises a negative electrode sheet having an active metal supplement layer, and the secondary battery charging and discharging method comprises: Charging the secondary battery for the first time; performing a first step of discharging the first-charged secondary battery to consume the residual metal in the active metal supplement layer; Discharging the second battery after the first step discharge in at least two steps; The current of the first step discharge is smaller than the current of at least two steps of discharge after the first step discharge, the first step discharge uses a current of 0.01-0.2C for constant current discharge, and the current range of at least two steps of discharge after the first step discharge is 0.01-20C; The step of discharging the secondary battery after the first step of discharge in at least two steps comprises: Performing a second step of discharging the secondary battery after the first step of discharging; The second battery after the second step discharge is charged and the third step discharge is performed after the charging.

2. The method for charging and discharging a secondary battery for the first time according to claim 1, characterized in that: The current of the first step of discharging is less than a preset value.

3. The method for charging and discharging a secondary battery for the first time according to claim 1, characterized in that: The discharge capacity of the first step of discharging is in the range of 3-10%.

4. The method for charging and discharging a secondary battery for the first time according to claim 1, characterized in that: The secondary battery is a lithium ion battery, and the active metal supplement layer is a lithium supplement layer.

5. The method for charging and discharging a secondary battery for the first time according to claim 4, characterized in that: The lithium supplement layer is at least one of lithium foil and lithium powder.

6. The method for charging and discharging a secondary battery for the first time according to claim 5, characterized in that: The lithium foil is at least one of rolled intermittent zebra-pattern lithium-replenishing, stripe-pattern lithium-replenishing, and full-film lithium-replenishing.

Citation Information

Patent Citations

  • Lithium-ion capacitor composite cathode plate, preparation method thereof and lithium-ion capacitor

    CN105513828A

  • Safety lithium-supplementing composite negative pole piece and preparation method thereof

    CN108878775A

  • Lithium supplement material and preparation method thereof, lithium ion battery and lithium supplement method thereof

    CN114566645A

  • Active lithium excitation method and application of lithium battery with supplemented lithium pole piece

    CN114744301A