A composite fiber fastener, a manufacturing method, and a preparation mold
By cross-winding composite fiber cloth into fasteners and using a mold pressing block assembly for pressure curing, the problems of low strength and complex processing of existing fasteners outside the fiber direction are solved, realizing the manufacturing of high-strength, low-cost fasteners.
Patent Information
- Application Number
- CN202310581329.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-05-22
AI Technical Summary
Existing fasteners have low strength outside the direction of the fiber material, require high processing precision, are complex to operate, and are costly.
Composite fiber tape is wound along its fiber direction and cross-wound with composite fiber cloth. It is then pressed and cured using a mold pressing block assembly to form a mesh fastener structure, which simplifies the manufacturing process and reduces costs.
It improves the strength of fasteners in all directions, reduces the requirements for machining accuracy and operational complexity, and significantly reduces manufacturing costs.
Smart Images

Figure CN116604837B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite fiber material products technology, specifically to a composite fiber fastener, a manufacturing method, and a preparation mold. Background Technology
[0002] The traditional processing flow for fasteners (generally bolts, nuts, etc.) typically involves: wire rod forming, annealing, pickling, cold drawing, cold forging, thread machining, heat treatment, and surface treatment. Currently, commonly used fasteners are typically made of stainless steel, carbon steel, or copper. Manufacturing these fasteners requires significant energy, generates a large amount of waste, involves complex processes, and results in low strength. Furthermore, these fasteners are not heat-resistant, have poor corrosion resistance, and poor wear resistance.
[0003] Currently, a high-strength fastener made of reinforcing fibers and resin materials (generally carbon fiber composites) has appeared on the market. Existing technology discloses a patent application with application number CN201980007909.0, entitled "Manufacturing Method of Fiber Reinforced Resin Bolt and Invention Patent of Fiber Reinforced Resin Bolt". It forms a reinforcing fiber resin tape layer by winding the reinforcing fibers (i.e., carbon fibers) in the direction of the tape, and then pressurizes and heats the above-mentioned reinforcing fiber resin tape layer to cure it, and finally forms a high-strength bolt.
[0004] However, this existing technology has the following problems:
[0005] 1. Because the fastener is wound along the direction of the fiber material, the strength of the fastener is low in other directions besides the direction of the fiber material.
[0006] 2. Fasteners require high machining precision and are complex to manufacture, resulting in high costs. Summary of the Invention
[0007] In order to overcome the shortcomings and deficiencies of the existing technology, the present invention aims to provide a composite fiber fastener, a manufacturing method and a preparation mold, which can improve the strength of fasteners in other directions besides the fiber direction, while the manufacturing process is simple and the cost is lower.
[0008] This invention is achieved through the following technical solution:
[0009] Application Example 1
[0010] The present invention relates to a method for manufacturing composite fiber fasteners, which comprises the following steps:
[0011] Winding process:
[0012] The composite fiber tape is wound along its fiber direction to form a concentric composite fiber inner part around the winding axis.
[0013] A composite fiber cloth with a fiber direction intersecting the fiber direction of the composite fiber cloth is wound again on the composite fiber inner part, so that the composite fiber cloth forms a concentric composite fiber roll around the winding axis of the composite fiber inner part.
[0014] Curing process:
[0015] The composite fiber roll is placed in the cavity of the mold. By applying pressure to one end of the winding shaft of the composite fiber roll in the radial direction and one or both ends perpendicular to the winding shaft in the axial direction, the composite fiber roll is cured to form a fastener wound into a mesh shape around the winding shaft.
[0016] Before the winding process, the insert with external threads is placed on the composite fiber tape, so that the direction of the external threads of the insert is consistent with the direction of the fibers of the composite fiber tape. Then, the winding process is carried out along the central axis of the insert, so that the central axis of the insert coincides with the winding axis of the composite fiber inner part. After the curing process, the insert is removed.
[0017] The mold cavity is connected to an overflow well on one side, so that during the curing process, some of the composite fiber roll can overflow into the overflow well to form an overflow portion; the manufacturing method also includes a post-processing step: removing the fastener from the cavity; and cutting off and separating the fastener from the overflow portion.
[0018] In the winding process, the composite fiber fabric is cut from one of the following: unidirectional plain weave fabric, twill weave fabric, and bidirectional woven fabric.
[0019] Before the curing process, the composite fiber roll is preheated to 60°C to 90°C.
[0020] In the curing process, the composite fiber roll is heated to 130-160℃ and then pressurized.
[0021] Application Example 2
[0022] The present invention relates to a composite fiber fastener, which is manufactured by the manufacturing method described in Application Example 1 above.
[0023] Application Example 3
[0024] The present invention relates to a preparation mold for manufacturing composite fiber fasteners, comprising a front mold, a rear mold, a first slide, a pressure block assembly, and an ejection assembly. The pressure block assembly is installed in the front mold, and the ejection assembly is installed in the rear mold. When the front mold and the rear mold are engaged, the shape of the cavity forms the outer diameter shape of the composite fiber fastener.
[0025] The first row position is used to press one end of the winding shaft of the composite fiber roll in the axial direction, the pressure block assembly is used to press one end of the winding shaft perpendicular to the axial direction of the composite fiber roll, and the ejection assembly is used to eject the composite fiber roll from the rear mold.
[0026] Application Example 4
[0027] The present invention relates to a preparation mold for manufacturing composite fiber fasteners, comprising a front mold, a rear mold, a first slide, a second slide, a pressure block assembly, and an ejection assembly. The pressure block assembly is installed in the front mold, and the ejection assembly is installed in the rear mold. When the front mold and the rear mold are engaged, the shape of the cavity forms the outer diameter shape of the composite fiber fastener.
[0028] The pressure block assembly is used to apply pressure to one end of the winding shaft of the composite fiber roll, the first and second positions are respectively used to apply pressure to both ends perpendicular to the winding shaft of the composite fiber roll, and the ejection assembly is used to eject the composite fiber roll from the rear mold.
[0029] Application Example 5
[0030] According to the preparation mold described in Application 3 and Application Example 4, the rear mold is provided with an overflow well communicating with the cavity.
[0031] Application Example 6
[0032] According to the preparation mold described in Application 3 and Application Example 4, an elastic element for resetting the pressure block assembly is provided between the front mold and the pressure block assembly.
[0033] The beneficial effects of this invention are:
[0034] 1. Higher strength in directions other than the fiber material direction: The manufacturing method of this invention involves winding a composite fiber strip along its fiber direction, followed by winding a composite fiber cloth. Based on the characteristics of the composite fibers and the application scenario of the fastener, the intersection angle between the fiber direction of the composite fiber cloth and the fiber direction of the composite fiber strip can be customized to form a mesh-like internal structure of the fastener, thereby increasing the overall strength of the fastener, overcoming limitations in application scenarios, and improving performance.
[0035] 2. The fasteners have lower processing precision requirements and are simpler to manufacture, resulting in lower costs: The mold of this invention uses a pressure block assembly in the front mold to press the fasteners together. Compared with the prior art where the front and rear molds are locked by bolts and nuts, the processing precision requirements are lower. Moreover, while applying force to the pressure block assembly, it can simultaneously lock the front and rear molds, eliminating the need to remove the bolts and nuts after curing as in the prior art. This makes the operation simpler and the cost lower. Attached Figure Description
[0036] The present invention will be further described with reference to the accompanying drawings, but the embodiments in the drawings do not constitute any limitation on the present invention. For those skilled in the art, other drawings can be obtained based on the following drawings without creative effort.
[0037] Figure 1 This is a schematic diagram of the mold opening process in Example 1.
[0038] Figure 2 This is a schematic diagram of the lower mold in Example 1.
[0039] Figure 3 This is a force diagram of the mold before the curing process in Example 1.
[0040] Figure 4 This is a diagram showing the force applied to the mold during the curing process in Example 1.
[0041] Figure 5 This is a schematic diagram of the fastener being ejected from the mold in Example 1.
[0042] Figure 6 This is a schematic diagram of the structure after the fastener is ejected in Example 1.
[0043] Figure 7 This is a schematic diagram of the mold opening process in Example 2.
[0044] Figure 8 This is a schematic diagram of the composite fiber roll being placed into the mold in Example 2.
[0045] Figure 9 This is a force diagram of the mold before the curing process in Example 2.
[0046] Figure 10 This is a diagram showing the force applied to the mold during the curing process in Example 2.
[0047] Figure 11 This is a schematic diagram of the fastener being ejected from the mold in Example 2.
[0048] Figure 12 This is a schematic diagram of the structure after the fastener is ejected in Example 2.
[0049] Figure 13 This is a schematic diagram of the insert after it has been removed from the nut in the embodiment.
[0050] Figure Labels
[0051] Front mold -- 100, pressure block assembly -- 101, elastic element -- 102,
[0052] Rear mold -- 200, Ejector assembly -- 201
[0053] First row position -- 301, Second row position -- 302, Overflow well -- 303, Insertion hole -- 304
[0054] Bolt--401, Nut--402, Insert--403. Detailed Implementation
[0055] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0056] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0057] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0058] The traditional processing flow for fasteners (generally bolts, nuts, etc.) typically involves: wire rod forming, annealing, pickling, cold drawing, cold forging, thread machining, heat treatment, and surface treatment. Currently, commonly used fasteners are typically made of stainless steel, carbon steel, or copper. Manufacturing these fasteners requires significant energy, generates a large amount of waste, involves complex processes, and results in low strength. Furthermore, these fasteners are not heat-resistant, have poor corrosion resistance, and poor wear resistance.
[0059] Currently, a high-strength fastener made of reinforcing fibers and resin materials (generally carbon fiber composites) has appeared on the market. Existing technology discloses a patent application with application number CN201980007909.0, entitled "Manufacturing Method of Fiber Reinforced Resin Bolt and Invention Patent of Fiber Reinforced Resin Bolt". It forms a reinforcing fiber resin tape layer by winding the reinforcing fibers (i.e., carbon fibers) in the direction of the tape, and then pressurizes and heats the above-mentioned reinforcing fiber resin tape layer to cure it, and finally forms a high-strength bolt.
[0060] However, this existing technology has the following problems:
[0061] 1. Because the fastener is wound along the direction of the fiber material, the strength of the fastener is low in other directions besides the direction of the fiber material.
[0062] 2. Fasteners require high machining precision and are complex to manufacture, resulting in high costs.
[0063] Example 1
[0064] To address the aforementioned issues, this embodiment discloses a method for manufacturing composite fiber fasteners. The composite fiber fasteners are formed using the following steps. In this embodiment, the fastener is a bolt 401.
[0065] The first step is the winding process, which consists of the following steps:
[0066] The composite fiber tape is wound along its fiber direction to form a concentric composite fiber inner part around the winding axis.
[0067] A composite fiber cloth with a fiber direction intersecting the fiber direction of the composite fiber inner component is wound again onto the composite fiber inner component, so that it forms a concentric composite fiber roll around the winding axis of the composite fiber inner component.
[0068] The composite fiber tape uses carbon fiber reinforced epoxy resin composite material, carbon fiber reinforced polyacrylonitrile-based composite material, and other carbon fiber composite materials; while the composite fiber cloth is cut from one of the following: unidirectional plain weave cloth, twill weave cloth, and bidirectional woven cloth, and its specifications include 1K, 3K, 12K and other specifications.
[0069] It should be noted that the wrapping direction of the carbon fiber cloth in this embodiment is determined according to the usage requirements. That is, if the manufactured bolts need to have a larger stress range in the direction perpendicular to the winding axis of the composite fiber tape, then the fiber direction of the composite fiber cloth should be perpendicular to the fiber direction of the wound composite fiber tape to achieve better strength.
[0070] Next, start the heating component of the mold to preheat the mold. Generally, the composite fiber roll is preheated to 60°C to 90°C before use.
[0071] Next, as Figure 2 As shown, the composite fiber roll is placed in a mold for a curing process; the curing process consists of the following steps:
[0072] The composite fiber roll is placed in the cavity of the mold. By applying pressure to one end of the winding shaft of the composite fiber roll along the axial direction and the other end perpendicular to the winding shaft, the composite fiber roll is cured to form a fastener that is wound into a mesh around the winding shaft.
[0073] Specifically, in this embodiment, the pressure block assembly 101 applies pressure to one end of the winding shaft perpendicular to the axial direction of the composite fiber roll, and the first row position 301 applies pressure to one end of the winding shaft of the composite fiber roll.
[0074] Specifically, the composite fiber roll, which is formed into a ring, is placed into the cylindrical part of the mold that is close to the threaded part, so that the winding axis of the composite fiber roll is substantially aligned with the axial direction of the threaded part of the mold.
[0075] molds, such as Figure 1 As shown, it is divided into two parts: a front mold 100 and a rear mold 200, and also includes a first slide 301, a pressure block assembly 101, and an ejector assembly 201; when the front mold 100 and the rear mold 200 are engaged, the shape of the cavity forms the outer diameter shape of the composite fiber fastener. After the composite fiber fastener is placed in the lower mold, it is used as follows... Figure 3 The mold is pressurized in the manner shown, causing the mold to... Figure 4 As shown, the first insert 301 and the pressure block assembly 101 are inserted into the cavity of the mold. After the upper mold and the lower mold are engaged, an insertion hole 304 is formed on one side of the cavity. The first insert 301 includes an insertion portion having an outer diameter slightly smaller than the diameter of the insertion hole 304 and a cylindrical head provided at one end of the insertion portion.
[0076] Moreover, such as Figure 1 As shown, the outermost end of the insertion portion of the first slide 301 is a molded version of the screw hole at the top of the nut of the bolt 401. That is, the cavity has the shape of a threaded portion and a nut portion. The front mold 100, the pressure block assembly 101 and the first slide 301 are pressurized simultaneously. The front mold 100 and the pressure block assembly 101 can be installed at the output end of the hydraulic press. At the same time, during the pressurization process, the temperature of the heater is adjusted so that the temperature of the cavity inside the mold reaches a curing temperature of 130°C to 160°C, so that it cures and forms a fastener.
[0077] After the curing process is completed, the heater is turned off, the upper mold and the first slide 301 are released, and the ejector assembly 201 is ejected. Figure 5The fastener is ejected to complete the manufacturing process; wherein, an elastic element 102 is provided between the ejection component 201 and the front mold 100 to facilitate the reset of the ejection component 201.
[0078] Furthermore, an overflow well 303 is connected to one side of the cavity of the rear mold 200, allowing some of the composite fiber roll to overflow into the overflow well 303 during the curing process. The function of the overflow well 303 is to allow composite fibers, air, and other substances to overflow from the overflow well 303 due to the increase in temperature and pressure when the composite fiber roll is cured in the cavity. In the prior art, the amount of composite fiber used needs to be configured very precisely, and in such cases, it is also necessary to replenish the material in the cavity. Therefore, the setting of the overflow well 303 means that the amount of composite fiber used in this embodiment does not need to be configured very precisely. It is only necessary to cut off the overflow portion of the fastener after the curing process, which can greatly reduce the manufacturing difficulty and cost of the fastener.
[0079] Additionally, refer to Figure 5 and Figure 6 The overflow portion serves as the force-bearing position when the ejector component 201 ejects, thereby preventing the ejection action from being directly applied to the fastener and causing dents on the fastener surface.
[0080] In addition, the mold in this embodiment can also be as follows: Figure 1 The diagram shows an additional set of cavities and a second row 302 for simultaneously manufacturing another set of bolts 401. Specific machining diagrams can be found in the provided image. Figure 2 and Figure 3 Furthermore, its manufacturing steps and principles are the same as those of the aforementioned bolt 401, and will not be repeated here.
[0081] Reference Figure 6 The fasteners manufactured through this embodiment, based on the characteristics of the composite fibers and the application scenarios of the fasteners, allow for customization of the intersection angle between the fiber directions of the composite fiber cloth and the composite fiber strip, forming a mesh-like internal structure within the fastener. This increases the overall strength of the fasteners of this invention, overcomes limitations in application scenarios, and improves performance. Compared to existing technologies, its tensile strength in all directions can be increased by approximately 2.7 to 3.1 times in tensile breaking strength.
[0082] In addition, the mold in this embodiment uses a pressure block assembly 101 on the front mold 100 to press the fasteners together by applying pressure to both the front mold 100 and the pressure block assembly 101. This also locks the front mold 100 and the rear mold 200 together. Compared with the prior art where the front and rear molds 200 are locked by bolts 401 and nuts 402, the processing accuracy requirements are lower. Furthermore, while applying force to the pressure block assembly 101, it can simultaneously lock the front and rear molds 200 together, eliminating the need to remove the bolts 401 and nuts 402 after curing, as is done in the prior art. This makes the operation simpler and the cost lower.
[0083] In the above embodiment, the inner surface shape of the mold is shown as an example of the outer shape of the bolt 401, but it is not limited to this shape. For example, it can be other shapes without a nut.
[0084] Example 2
[0085] like Figures 7 to 12 As shown, in this embodiment, the composite fiber fastener is formed by the following process, and the fastener in this embodiment is nut 402;
[0086] First, a winding process is performed. The steps of the winding process are generally the same as those in Example 1, but there is one difference: before the winding process, the insert 403 with external threads is placed on the composite fiber tape, so that the direction of the external threads of the insert 403 is consistent with the direction of the fibers of the composite fiber tape. Then, the winding process is performed along the central axis of the insert 403, so that the central axis of the insert 403 coincides with the winding axis of the composite fiber inner part.
[0087] Meanwhile, the structure of the mold is slightly different from that of Example 1: for details, please refer to... Figure 6 Since the structure of nut 402 is different from that of bolt 401, the placement direction of the composite fiber roll in this embodiment is also different from that in embodiment 1. Specifically, the pressure block assembly 101 is used to press one end of the winding shaft of the composite fiber roll, and the first row position 301 and the second row position 302 are respectively used to press the two ends perpendicular to the winding shaft of the composite fiber roll.
[0088] Among them, the outermost ends of the insertion parts of the first row position 301 and the second row position 302 are exactly half of a regular hexagon. After they are inserted into the insertion holes 304 on both sides of the cavity, they form a regular hexagonal structure of nut 402.
[0089] In addition, after the curing process, the insert 403 needs to be unscrewed from the nut 402 to form the final product.
[0090] It should be noted that, apart from the features described in this embodiment, all other features are the same as in Embodiment 1, and will not be repeated here.
[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A method for manufacturing composite fiber fasteners, characterized in that, The following processes are used to form composite fiber fasteners; Winding process: The composite fiber tape is wound along its fiber direction to form a concentric composite fiber inner part around the winding axis. A composite fiber cloth with a fiber direction intersecting the fiber direction of the composite fiber cloth is wound again on the composite fiber inner part, so that the composite fiber cloth forms a concentric composite fiber roll around the winding axis of the composite fiber inner part. When the composite fiber fastener is a bolt, the curing process is as follows: The composite fiber roll is placed in a closed cavity formed by the snap-fitting of a front mold and a rear mold. After the front mold and the rear mold are snapped together, an insertion hole for inserting a slide is formed on one side of the cavity. The insertion part of the first row is inserted into the cavity through the insertion hole, and the first row and the pressure block assembly installed on the front mold apply pressure to one end of the winding shaft of the composite fiber roll and one end perpendicular to the winding shaft of the composite fiber roll, so that the composite fiber roll is cured in the cavity to form a fastener wound into a mesh around the winding shaft, thereby obtaining the bolt. When the composite fiber fastener is a nut, the curing process is as follows: The composite fiber roll is placed in a closed cavity formed by the snap-fitting of a front mold and a rear mold. After the front mold and the rear mold are snapped together, insertion holes for inserting the roll are formed on both sides of the cavity. The insertion portions of the first and second rows are inserted into the cavity through the insertion holes on both sides, and the first and second rows and the pressure block assembly installed on the front mold apply pressure to one end of the winding shaft of the composite fiber roll and both ends perpendicular to the winding shaft of the composite fiber roll, so that the composite fiber roll is cured in the cavity to form a fastener wound into a mesh around the winding shaft, thereby obtaining the nut.
2. The method for manufacturing a composite fiber fastener according to claim 1, characterized in that, Before the winding process, the insert with external threads is placed on the composite fiber tape, so that the direction of the external threads of the insert is consistent with the direction of the fibers of the composite fiber tape. Then, the winding process is carried out along the central axis of the insert, so that the central axis of the insert coincides with the winding axis of the composite fiber inner part. After the curing process, the insert is removed.
3. The method for manufacturing a composite fiber fastener according to claim 1, characterized in that, The mold cavity is connected to an overflow well on one side, so that during the curing process, some of the composite fiber roll can overflow into the overflow well to form an overflow portion; The manufacturing method further includes a post-processing step: Remove the fastener from the cavity; Cut off and separate the fastener from the overflow portion.
4. The method for manufacturing a composite fiber fastener according to claim 1, characterized in that, In the winding process, the composite fiber fabric is cut from one of the following: unidirectional plain weave, twill weave, and bidirectional woven fabric.
5. The method for manufacturing a composite fiber fastener according to claim 1, characterized in that, Before the curing process, the composite fiber roll is preheated to 60°C to 90°C; In the curing process, the composite fiber roll is heated to 130-160℃ and then pressurized.
6. A composite fiber fastener, characterized in that, Made by the manufacturing method according to any one of claims 1-5.
7. A preparation mold for manufacturing composite fiber fasteners, characterized in that, It includes a front mold, a rear mold, a first slide, a pressure block assembly, and an ejection assembly. The pressure block assembly is installed in the front mold, and the ejection assembly is installed in the rear mold. When the front mold and the rear mold are engaged, the shape of the cavity forms the outer diameter shape of the composite fiber fastener. After the front mold and the rear mold are engaged, an insertion hole is formed on one side of the cavity; the first slide includes an insertion part, which is inserted into the cavity through the insertion hole and is used to press one end of the winding shaft of the composite fiber roll in the axial direction; the pressure block assembly is used to press one end of the winding shaft perpendicular to the axial direction of the composite fiber roll; the ejection assembly is used to eject the composite fiber roll from the rear mold.
8. A preparation mold for manufacturing composite fiber fasteners, characterized in that, It includes a front mold, a rear mold, a first slide, a second slide, a pressure block assembly, and an ejection assembly. The pressure block assembly is installed in the front mold, and the ejection assembly is installed in the rear mold. When the front mold and the rear mold are engaged, the shape of the cavity forms the outer diameter shape of the composite fiber fastener. After the front mold and the rear mold are engaged, insertion holes are formed on both sides of the cavity; the first slide and the second slide both include an insertion part, which is inserted into the cavity through the insertion holes on both sides; the pressure block assembly is used to press one end of the winding shaft of the composite fiber roll, the first slide and the second slide are used to press both ends perpendicular to the winding shaft of the composite fiber roll, and the ejection assembly is used to eject the composite fiber roll from the rear mold.
9. The preparation mold according to claim 7 or 8, characterized in that, The rear mold is provided with an overflow well that communicates with the cavity.
10. The preparation mold according to claim 7 or 8, characterized in that, An elastic element for resetting the pressure block assembly is provided between the front mold and the pressure block assembly.
Citation Information
Patent Citations
Fiber-reinforced resin bolt manufacturing method and fiber-reinforced resin bolt
CN111587326A
Carbon fiber composite compression molding die
CN210634146U
Composite fiber fastener and preparation mold
CN219583557U
Manufacturing method of screw fastening component
JP2017003091A
Fiber reinforced plastic bolt and method for producing the same
US20120063866A1