A method for baking a metal shell lithium battery
Through the method of vacuum atmosphere heating and circulating inert gas filling, the problem of high nitrogen consumption in lithium battery baking is solved, the baking effect and efficiency are improved, the cost is reduced, and the process flow is simplified.
Patent Information
- Application Number
- CN202310433839.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-21
AI Technical Summary
In the existing lithium battery baking process, nitrogen consumption is high, the cost is high, and it is difficult to effectively improve the baking effect. Especially in large-capacity metal case lithium batteries, there are engineering difficulties in removing the moisture inside the cell through the small liquid injection port.
Use vacuum atmosphere to heat and circulate inert gas to reduce the charging pressure during circulation, increase the circulation frequency, accelerate water volatilization through micro-air pressure, reduce nitrogen consumption and baking time, and improve the baking effect.
It significantly reduces the consumption of inert gas, reduces equipment costs, improves the battery baking effect, simplifies the process, significantly reduces the baking time, and effectively reduces the moisture content of the battery cells.
Smart Images

Figure CN116613384B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of batteries, and in particular to a method for baking a metal shell lithium battery. Background Art
[0002] The demand for lithium-ion batteries in electric vehicles, energy storage, 3C and other fields has increased year by year, and lithium batteries have now entered a stage of rapid growth. There are strict requirements for moisture control in the production and manufacturing process of lithium batteries. Abnormal moisture content can easily lead to increased internal resistance, low capacity, and poor cycle performance of the battery, which directly affects the performance of the battery. Large-capacity metal-shell lithium batteries have a liquid injection process in the production process. Before the liquid is injected, the battery cell needs to be baked. The main purpose of baking is to remove the moisture contained in the internal pole pieces and diaphragms of the battery. That is, the baking process is the key process to control the internal moisture content of the lithium battery.
[0003] Large-capacity metal-cased lithium batteries are basically assembled before baking, with a liquid injection port left for liquid injection. The battery cell can only be baked to remove moisture inside the battery cell through the liquid injection port. The diameter of the liquid injection port is usually 3-8mm, and it is very difficult to remove moisture inside the battery cell through the liquid injection port.
[0004] Among them, a Chinese patent document discloses a rapid baking process for power battery cells [CN108923069A], which pre-bakes the bare cells and then performs secondary baking after the bare cells are assembled into batteries. The scheme requires design process route adjustment, large-scale equipment investment, and high cost;
[0005] In addition, Chinese patent literature discloses a method for vacuum drying lithium battery cells [CN 106643003A]. In this solution, nitrogen is filled during the baking process, but it needs to be filled to normal pressure. Frequent nitrogen filling will cause a large amount of nitrogen consumption.
[0006] The above solution solves the problem of difficulty in removing moisture from the battery cell in the prior art to a certain extent, but the solution still has many shortcomings, such as large nitrogen consumption and high cost, and it is difficult to effectively improve the baking effect. Summary of the invention
[0007] To achieve the above object, the present invention adopts the following technical scheme: a method for baking a metal shell lithium battery, the method comprising the following steps:
[0008] S1. Place the battery cell into the oven;
[0009] S2. Preheat the battery cell in an oven to heat the battery cell to the process temperature;
[0010] S3, vacuuming the oven;
[0011] S4, heating the oven in a vacuum atmosphere and filling it with inert gas;
[0012] S5, heating the oven with an inert gas atmosphere;
[0013] S6, looping through steps S3-S5;
[0014] S7, end the cycle and evacuate;
[0015] S8, cooling, end.
[0016] This method can greatly reduce the time of filling inert gas and effectively reduce the consumption of inert gas by reducing the pressure of the inert gas during circulation.
[0017] After reducing the pressure of the inert gas, multiple cycles can be easily achieved. At the same time, the difficulty of vacuuming during the cycle is reduced, and the load on the vacuum pump is significantly reduced;
[0018] By increasing the breathing frequency, the battery baking effect is significantly improved and the baking time can be greatly reduced, which not only reduces the equipment cost, but also reduces the consumption of inert gas, effectively improves the battery baking effect, and the method of use is simple and convenient.
[0019] In the above-mentioned method for baking a metal shell lithium battery, in step S4, the inert gas is nitrogen.
[0020] In the above-mentioned method for baking a metal shell lithium battery, in step S2, the temperature range for preheating the battery cell is 85-105°C.
[0021] In the above-mentioned method for baking a metal shell lithium battery, in step S3, when the oven is evacuated, the air pressure inside the battery cell is reduced, and the volatilization rate of water in the pole piece and the battery separator is accelerated.
[0022] In the above-mentioned method for baking a metal shell lithium battery, in step S3, the requirement for evacuating the oven is: making the vacuum pressure in the oven 50-100Pa.
[0023] In the above-mentioned method for baking a metal shell lithium battery, vacuum atmosphere heating is performed in a vacuum state on the inner side of the oven to ensure that moisture evaporates.
[0024] In the above-mentioned metal shell lithium battery baking method, in step S4, the cutoff condition for filling with nitrogen is that the air pressure in the oven is in the range of 0.5-10KPa. When the air pressure in the oven reaches 0.5-10KPa, the micro-air pressure can break the equilibrium state inside the battery.
[0025] In the above-mentioned method for baking a metal shell lithium battery, in step S5, the inert gas atmosphere heating is performed by filling nitrogen gas into the inner side of the oven circumference and then heating the oven so that the micro-pressure nitrogen gas enters the interior of the battery cell.
[0026] In the above-mentioned method for baking a metal shell lithium battery, the heating time in the inert gas atmosphere is 1-5 minutes.
[0027] In the above-mentioned metal shell lithium battery baking method, in step S6, the number of cycles is 10-26 times.
[0028] In the above-mentioned metal shell lithium battery baking method, in step S7, after the cycle is completed, vacuum is drawn to exhaust the inert gas in the oven and maintain the vacuum state in the oven.
[0029] Compared with the prior art, the advantages of the present invention are:
[0030] 1. By reducing the pressure of the inert gas during the cycle, the filling time can be greatly reduced and the inert gas consumption can be reduced. After reducing the inert gas pressure, multiple cycles can be easily achieved.
[0031] 2. Use low-pressure circulation and increase the circulation frequency to achieve good baking effect, reduce the vacuuming time, and reduce the load of vacuum equipment.
[0032] 3. By increasing the breathing frequency, the battery baking effect is significantly improved and the baking time can be greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a flow chart of the method of the present invention. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0035] like Figure 1 As shown, a method for baking a metal shell lithium battery comprises the following steps:
[0036] S1. Place the battery cell into the oven;
[0037] S2. Preheat the battery cell in an oven to heat the battery cell to the process temperature;
[0038] S3, vacuuming the oven;
[0039] S4, heating the oven in a vacuum atmosphere and filling it with inert gas;
[0040] S5, heating the oven with an inert gas atmosphere;
[0041] S6, looping through steps S3-S5;
[0042] S7, end the cycle and evacuate;
[0043] S8, cooling, end.
[0044] In step S4, the inert gas is nitrogen. The inert gas here can also be set to other inert gases, and the best effect is achieved when nitrogen is selected.
[0045] In step S2, the temperature range for preheating the battery cell is 85-105°C.
[0046] In step S3, when the oven is evacuated, the air pressure inside the battery cell decreases, and the volatilization rate of water in the electrode and the battery separator is accelerated.
[0047] In step S3, the requirement for evacuating the oven is to make the vacuum pressure in the oven 50-100Pa.
[0048] Vacuum atmosphere heating is heating in a vacuum state inside the oven to ensure that moisture evaporates.
[0049] In step S4, the cut-off condition for filling with nitrogen is that the air pressure in the oven is in the range of 0.5-10 KPa. When the air pressure in the oven reaches 0.5-10 KPa, the micro pressure can break the equilibrium state inside the battery.
[0050] In step S5, the inert gas atmosphere heating is performed by filling nitrogen gas into the inner side of the oven circumference and then heating the oven so that the slightly-pressure nitrogen gas enters the interior of the battery cell.
[0051] The heating time in the inert gas atmosphere is 1-5 minutes.
[0052] In step S6, the number of cycles is 10-26 times.
[0053] In step S7, after the cycle is completed, vacuum is drawn to exhaust the nitrogen in the oven and maintain the vacuum state in the oven.
[0054] Taking 300AH square aluminum shell lithium iron phosphate battery as an example, the following implementation examples are carried out:
[0055] Embodiment 1
[0056] Step a: placing the battery cell into an oven;
[0057] Step b: preheating, heating the internal temperature of the battery cell to the process temperature, the temperature is 100°C; time is 2 hours;
[0058] Step c: vacuum to 100 Pa;
[0059] Step d: heating in vacuum atmosphere for 195 min;
[0060] Step e: filling with nitrogen to 5kpa;
[0061] Step f: heating in an inert gas atmosphere for 5 minutes;
[0062] Step cycle: loop to step c, cycle 3 times;
[0063] Step g: end the cycle and evacuate the air;
[0064] Step h: Cooling, end.
[0065] Implementation Example 2:
[0066] Step a: placing the battery cell into an oven;
[0067] Step b: preheating, heating the internal temperature of the battery cell to the process temperature, the temperature is 100°C; time is 2h;
[0068] Step c: vacuum to 100 Pa;
[0069] Step d: Heating in vacuum atmosphere for 95 minutes
[0070] Step e: filling with nitrogen to 5kpa;
[0071] Step f: heating in an inert gas atmosphere for 5 minutes;
[0072] Step cycle: loop to step c, cycle 6 times;
[0073] Step g: End the cycle and evacuate
[0074] Step h: Cooling, end
[0075] Implementation Example 3:
[0076] Step a: placing the battery cell into an oven;
[0077] Step b: preheating, heating the internal temperature of the battery cell to the process temperature, the temperature is 100°C; time is 2h;
[0078] Step c: vacuum to 100 Pa;
[0079] Step d: heating in vacuum atmosphere for 61.7 min;
[0080] Step e: filling with nitrogen to 5kpa;
[0081] Step f: heating in an inert gas atmosphere for 5 minutes;
[0082] Step cycle: loop to step c, cycle 9 times;
[0083] Step g: end the cycle and evacuate the air;
[0084] Step h: Cooling, end.
[0085] Implementation Example 4:
[0086] Step a: placing the battery cell into an oven;
[0087] Step b: preheating, heating the internal temperature of the battery cell to the process temperature, the temperature is 100°C; time is 2h;
[0088] Step c: vacuum to 100 Pa;
[0089] Step d: heating in vacuum atmosphere for 45 min;
[0090] Step e: filling with nitrogen to 5kpa;
[0091] Step f: heating in an inert gas atmosphere for 5 minutes;
[0092] Step cycle: loop to step c, cycle 12 times;
[0093] Step g: end the cycle and evacuate the air;
[0094] Step h: Cooling, end.
[0095] The following table is prepared according to the above-mentioned embodiments 1 to 4:
[0096]
[0097]
[0098] The water content in the battery cells after baking in Examples 1 to 4 is shown in the following table:
[0099]
[0100] It can be seen from the above-mentioned embodiments 1 to 4 that, under the same baking time, increasing the number of baking cycles can significantly improve the baking effect, and the moisture content in the battery cell is significantly reduced.
[0101] In summary, the principle of this embodiment is: by reducing the pressure of nitrogen filling during the cycle, reducing the time of nitrogen filling, reducing the nitrogen consumption, and reducing the nitrogen pressure in the oven, multiple cycles of baking are performed, the difficulty of vacuuming is reduced during the cyclic baking process, the load of the vacuum pump is reduced, the number of vacuum preheating cycles is increased, and the baking effect on the battery cells is improved, thereby reducing the baking time and effectively reducing the water content of the battery cells.
[0102] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A method for baking a metal shell lithium battery, characterized in that: The method comprises the following steps: S1. Place the battery cell into the oven; S2. Preheat the battery cell in an oven to heat the battery cell to the process temperature; S3, evacuate the oven to make the vacuum pressure in the oven 50-100Pa; S4, heating the oven in a vacuum atmosphere and filling it with inert gas, wherein the cut-off condition for filling the inert gas is that the pressure in the oven is in the range of 0.5-10 KPa; S5, heating the oven with an inert gas atmosphere; S6, cyclically implement steps S3-S5; the number of cycles is 10-26 times; S7, end the cycle and evacuate; S8, cooling, end; total baking time 600min.
2. A metal shell lithium battery baking method according to claim 1, characterized in that: In step S4, the inert gas is nitrogen.
3. A metal shell lithium battery baking method according to claim 1, characterized in that: In step S2, the temperature range for preheating the battery cell is 85-105°C; in step S3, when the oven is evacuated, the air pressure inside the battery cell decreases, and the volatilization rate of water in the electrode and the battery separator is accelerated.
4. A method for baking a metal shell lithium battery according to claim 1, characterized in that: The vacuum atmosphere heating is performed in a vacuum state inside the oven to ensure that the water evaporates.
5. A method for baking a metal shell lithium battery according to claim 1, characterized in that: In step S5, the inert gas atmosphere heating is performed by filling nitrogen into the inner side of the oven circumference to allow the slightly-pressure nitrogen to enter the interior of the battery cell.
6. A method for baking a metal shell lithium battery according to claim 1, characterized in that: The duration of the inert gas atmosphere heating is 1-5 minutes.
7. A method for baking a metal shell lithium battery according to claim 1, characterized in that: In step S7, after the cycle is completed, vacuum is drawn to exhaust the nitrogen in the oven and maintain the vacuum state in the oven.