A high-throughput preparation system and method for multi-component glass materials based on fused deposition

By combining fused deposition modeling (FDM) technology with machine learning models, the problem of inaccurate calculation of softening point temperature in the preparation of multi-component glass materials has been solved, enabling efficient and precise glass material forming and improving the efficiency of component screening and the speed of research and development.

CN116621433BActive Publication Date: 2026-11-10NANJING FIBERGLASS RES & DESIGN INST CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310563940.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2026-11-10
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

Existing technologies are inefficient in screening glass material components, traditional preparation methods are time-consuming and costly, and fused deposition modeling technology lacks a precise method for calculating the softening point temperature in the preparation of multi-component glass materials, resulting in poor molding quality.

Method used

A high-throughput preparation system for multi-component glass materials based on fused deposition modeling technology is adopted. A calculation and prediction model of glass composition and softening point temperature is established by combining machine learning technology. The efficient preparation of glass samples is achieved through the integration of the batching unit, melting unit and printing unit.

Benefits of technology

This technology enables high-throughput preparation of multi-component glass materials, precise control of nozzle printing temperature, improved molding quality, shortened preparation time, and enhanced glass material screening efficiency and R&D speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116621433B_ABST
    Figure CN116621433B_ABST
Patent Text Reader

Abstract

This invention discloses a high-throughput preparation system and method for multi-component glass materials based on fused deposition modeling (FDM). Under program control, different raw material powders are pneumatically delivered and mixed uniformly according to a designed glass component ratio. Then, based on FDM technology, the batch is heated to a molten glass state and extruded through a nozzle via a pipeline. A calculation and prediction model of the softening point temperature of multi-component glass effectively guides the setting of key printing parameters, such as nozzle printing temperature, thereby printing the desired bulk glass material sample. This method, based on FDM technology, integrates glass batching, glass melting, printing, and computer control unit processes for high-throughput glass sample preparation. It has advantages such as short melting preparation time, fast printing speed, and high printing quality. With a single setup and multiple runs, it can quickly, simply, and efficiently prepare 25 different component discrete bulk glass material samples in a high-throughput manner.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of glass preparation technology, and specifically to a high-throughput preparation system and method for multi-component glass materials based on fused deposition modeling technology. Background Technology

[0002] As one of the three key technologies of "materials genome technology," high-throughput materials preparation technology is becoming an important tool for new materials research and development. High-throughput materials experimental technology mainly includes two parts: high-throughput preparation and high-throughput characterization. Its core idea is to replace the original sequential iterative method with parallel or efficient serial experiments, using quantitative changes to lead to qualitative changes in the efficiency of materials research. High-throughput materials experiments can not only provide experimental verification for the results of materials simulation calculations, allowing for the optimization and correction of computational models, but also quickly provide valuable research results, accelerating the screening and optimization of materials. The high-throughput materials preparation process is generally divided into two steps: "combination" and "phase formation." First, multiple elements are systematically mixed to obtain the desired material composition combination, and then crystalline or amorphous phase materials are formed through diffusion or thermodynamic processes. After years of development, high-throughput materials preparation technology has been widely accepted in the materials science and technology industry and is widely used in the research and industrialization of materials such as metals, ceramics, inorganic compounds, and polymers. Currently, various high-throughput preparation technologies covering thin films, bulk materials, and powder materials have been gradually developed.

[0003] The composition of glass materials significantly impacts their performance, making composition selection crucial for optimizing glass properties. Traditionally, the development and selection of glass material compositions largely employs a trial-and-error approach: composition design, glass preparation, performance testing, and composition optimization. This iterative process continuously improves the physicochemical properties of the glass. Clearly, the traditional trial-and-error method involves a massive workload, long performance adjustment cycles, and high costs in glass composition selection experiments. In the laboratory, the primary constraint on the efficiency of glass composition optimization lies in the glass preparation process, typically employing a melt-quench process. This process involves manually weighing and mixing various raw materials, melting and clarifying them at high temperatures, and finally cooling and shaping them. This traditional method consumes large quantities of raw materials, is time-consuming, and produces very few glass samples at a time, significantly reducing the efficiency of determining the optimal glass composition. Therefore, to accelerate the research and optimization of new glass materials, it is urgent to find a suitable and efficient experimental method. High-throughput preparation technology will provide an important pathway for efficient research and development of glass materials. Currently, the application of high-throughput preparation technology in the field of glass materials is rarely reported; developing high-throughput preparation methods for glass materials will have significant theoretical and practical implications.

[0004] As a rapid prototyping technology, 3D printing is a technique that uses digital model files as a basis and employs powdered metals or plastics and other bondable materials to construct objects layer by layer. Fused Deposition Modeling (FDM) is a 3D technology suitable for manufacturing complex-shaped parts, and in recent years researchers have applied it to the rapid prototyping of glass materials. Compared to traditional melt-cooling methods, FDM integrates the previously separate melting, cooling, and forming processes of traditional glass manufacturing into a single process, significantly improving the efficiency of glass sample preparation and facilitating high-throughput glass production. However, selecting appropriate printing parameters is crucial for this technology, especially the nozzle printing temperature setting, which is key to successful printing. If the nozzle printing temperature is set too low, the glass rod will not soften sufficiently, making it difficult to form; if the printing temperature is set too high, the glass will be too soft, in a molten state, with large deformation and flow, also making it difficult to form. Generally speaking, the nozzle printing temperature must be higher than the softening point temperature of the glass being prepared, and therefore can be set according to the glass's softening point temperature. Currently, researchers in this field are using fused deposition modeling (FDM) to prepare binary or ternary glass materials, such as soda-lime glass and chalcogenide glass. However, there are no reports on the preparation of more multi-component glasses, and empirical formulas are generally used to roughly determine the softening point temperature. The main drawback of using empirical formulas is their insufficient extrapolation ability; when applied to calculating the softening point temperature of more multi-component glasses, the accuracy is low or even impossible. Therefore, for high-throughput fabrication of multi-component glass materials using FDM, there is an urgent need to find a more precise method for calculating the softening point temperature. This method should allow for accurate prediction of the softening point temperature of the multi-component glass before the experiment, which would scientifically and effectively guide the setting of the nozzle printing temperature, helping to improve the forming quality of the glass samples and obtain the desired printed glass samples. Summary of the Invention

[0005] In view of the above background, the purpose of this invention is to provide a high-throughput preparation method for multi-component glass materials based on fused deposition modeling. This method first involves pneumatically feeding and uniformly mixing different powder raw materials according to a pre-designed glass component ratio under program control. Then, based on fused deposition modeling technology, the batch material is heated to a molten glass state and extruded through a pipe to a nozzle, thereby printing out the desired bulk glass material sample.

[0006] The above-mentioned objectives of the present invention are achieved by the technical features of the independent claims, and the dependent claims develop the technical features of the independent claims in an alternative or advantageous manner.

[0007] To achieve the above objectives, the following technical solutions can be used.

[0008] A high-throughput preparation system for multi-component glass materials based on fused deposition modeling technology includes: a batching unit for batching materials, a melting unit for heating and melting the batching materials, a printing unit for printing bulk glass materials, and a control unit for controlling the batching, melting, and printing processes.

[0009] Preferably, the batching unit includes a powder feeder, with multiple raw material powder cylinders mounted above the powder feeder. Each raw material powder cylinder is equipped with a powder feeding pipeline, which is connected to a powder mixer. Below the powder mixer is a batching feed pipeline, which is connected to a screw feeder.

[0010] Preferably, the melting unit includes a furnace body, a crucible in the middle of the furnace body, an opening at the top of the crucible for feeding material into the crucible by a screw feeder, and heating elements on both sides of the furnace body.

[0011] Preferably, the printing unit includes a printing nozzle, a heating element on the printing nozzle, the printing nozzle being connected to a glass melt pipeline, the other end of the glass melt pipeline being connected to a crucible, a printing platform being provided below the printing nozzle, and a heating element being provided at the bottom of the printing platform.

[0012] Preferably, the control unit includes a computer software console, which controls the glass component ratio and weight, pneumatic powder flow rate, powder mixing time, and screw feed flow rate in the batching unit; controls the crucible heating regime in the melting unit; and controls the printing parameters and glass processing dimensions in the printing unit. In setting the printing nozzle parameters, the key feature is the ability to perform calculations to generate the corresponding glass softening point temperature for each glass component.

[0013] A high-throughput preparation method for multi-component glass materials based on fused deposition modeling technology includes:

[0014] Step 1: Set or generate various operating parameters in the control unit, including glass composition ratio and glass preparation weight, pneumatic powder feeding flow rate, powder mixing time, screw feeding flow rate, crucible heating regime, printing parameters and glass processing dimensions;

[0015] Step 2: Start-up. The crucible in the melting unit, as well as the printing nozzle and printing platform in the printing unit, begin heating according to the set operating parameters. The control console in the control unit displays the heating temperature in real time. Once the set heating temperature is reached, temperature control and heat preservation begin.

[0016] Step 3: After the crucible has been kept at the target temperature for a period of time, the powder feeder in the batching unit starts to run. The raw material powder is quantitatively fed into the powder mixer through the powder feeding pipeline according to the set pneumatic powder feeding flow rate. When the amount of raw material powder fed into each raw material powder cylinder reaches the calculated amount, the powder feeder stops running.

[0017] Step 4: The powder mixer mixes the fed raw material powder evenly according to the set powder mixing time. After the powder mixing time is reached, the powder mixer stops running.

[0018] Step 5: The uniformly mixed powder in the powder mixer flows into the screw feeder along the feeding pipeline. The screw feeder feeds the material into the crucible in a spiral manner according to the set screw feeding flow rate. After feeding is completed, the crucible is temperature controlled and kept warm. The material in the crucible reacts completely into molten glass.

[0019] Step 6: After the crucible reaches the temperature control and holding time, the molten glass liquid in the crucible is transported to the printing nozzle through the pipeline. After being continuously heated and softened by the heating elements set around the printing nozzle, the temperature of the molten glass liquid at the printing nozzle reaches the set printing temperature of the printing nozzle.

[0020] Step 7: After the printing nozzle of the printing unit prints one layer of slices on the printing platform according to the preset printing parameters and glass processing dimensions, the printing platform moves down one layer and repeats the above process until the desired printed block glass sample is printed.

[0021] Step 8: Repeat steps 1 to 7 to complete multiple printed bulk glass samples with different glass composition ratios.

[0022] Step 9: After a batch of printed bulk glass samples has been prepared, remove them and anneal them.

[0023] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0024] 1. Faced with fused deposition modeling of a series of glass components with different components, the computer software system has established a calculation and prediction model for the composition and softening point temperature of up to 10 component oxide glasses based on machine learning technology. It can accurately calculate and predict the softening point temperature of the prepared glass, effectively guide the setting of key printing parameters such as nozzle printing temperature, and help to obtain bulk glass material samples with good forming quality.

[0025] 2. Equipped with a multi-pipeline powder feeder and a powder mixer, it has functions such as formula setting, raw material dosage calculation and powder path linkage selection. It uses less raw materials, has high powder feeding accuracy and good material uniformity, ensuring the accurate proportion of glass components. It can realize the automatic and accurate conveying of glass powder raw materials with up to 10 different components and particle sizes.

[0026] 3. This method is based on fused deposition modeling technology for high-throughput preparation of glass samples. It integrates glass batching, glass melting and printing unit processes, and has the advantages of short melting preparation time, fast printing speed and wide glass processing size. After one setup and multiple runs, it can quickly, simply and efficiently prepare 25 different component discrete block glass material samples.

[0027] 4. Due to the use of a layer-by-layer deposition molding printing method, the cooling rate is high, which can obtain a wider range of glass composition. The prepared glass material samples are of excellent quality and have advantages such as high surface flatness, uniform composition, low crystallization tendency, and not easily cracking.

[0028] 5. It breaks through the traditional glass melting method of "one furnace, one style". Combined with subsequent characterization, it helps to quickly establish the correlation between glass "composition and performance", greatly improves the efficiency of glass component optimization and screening, realizes the rapid research and development of new glass materials, and has great practical value.

[0029] It should be understood that all combinations of the foregoing concepts and the additional concepts described in more detail below may be considered part of the inventive subject matter of this application, provided that such concepts do not contradict each other. Furthermore, all combinations of the claimed subject matter are considered part of the inventive subject matter of this application.

[0030] The foregoing and other aspects, embodiments, and features of the teachings of the present invention will be more fully understood from the following description in conjunction with the accompanying drawings. Other additional aspects of the invention, such as features and / or beneficial effects of exemplary embodiments, will become apparent from the following description or may be learned through practice of specific embodiments according to the teachings of the present invention. Attached Figure Description

[0031] The accompanying drawings are not intended to be drawn to scale. In the drawings, the corresponding operational steps in each figure are labeled with text. For clarity, not every step is described in every figure. Embodiments of various aspects of the invention will now be described by way of example and with reference to the accompanying drawings, wherein:

[0032] Figure 1 This is a schematic diagram of a high-throughput glass material fabrication system based on fused deposition modeling technology.

[0033] Figure 2 This is a flowchart of the method for calculating and predicting the softening point temperature of glass.

[0034] Figure 3 It is a 5×5 bulk glass array sample with different components prepared in one setup. Detailed Implementation

[0035] To better understand the technical content of the present invention, specific embodiments are described below in conjunction with the accompanying drawings.

[0036] In this invention, various aspects of the invention are described with reference to the accompanying drawings, in which numerous illustrative embodiments are shown. The embodiments of the invention are not necessarily intended to encompass all aspects of the invention. It should be understood that the various concepts and embodiments described above, as well as those described in more detail below, can be implemented in any of many ways, because the concepts and embodiments disclosed herein are not limited to any particular implementation. Furthermore, some aspects of the invention disclosed may be used alone or in any suitable combination with other aspects of the invention disclosed.

[0037] The key innovation of the method described in this invention lies in the fact that, when faced with fused deposition modeling of a series of glasses with different compositions, the computer software system establishes a calculation and prediction model based on machine learning technology for the composition and softening point temperature of a decimal oxide glass. This model can calculate and predict the softening point temperature of the prepared multi-component glass, providing more scientific and effective guidance for setting the nozzle printing temperature, and resulting in bulk glass material samples with good forming quality. With a single setup and multiple runs, high-throughput preparation of multi-component discrete bulk glass material samples can be achieved quickly, simply, and efficiently.

[0038] like Figure 1 As shown, a high-throughput glass material fabrication system based on fused deposition modeling technology includes:

[0039] (1) A batching unit, which includes a powder feeder 2, a raw material powder cylinder 3 is mounted above the powder feeder 2, each raw material powder cylinder is provided with a powder feeding pipe 4, the powder feeding pipe 4 is connected to the powder mixer 5, and a batching feeding pipe 6 is provided below the powder mixer 5, the batching feeding pipe 6 is connected to a screw feeder 7.

[0040] (2) Melting unit, which includes furnace body 8, crucible 9 in the middle of furnace body 8, opening 9 at the top of crucible 9 for feeding material into crucible 9 by spiral feeder 7, and first heating element 10 on both sides of furnace body 8.

[0041] (3) A printing unit, which includes a printing nozzle 14, a second heating element 13 on the printing nozzle 14, the printing nozzle 14 being connected to a glass liquid pipeline 12, the other end of the glass liquid pipeline 12 being connected to the crucible 9, a printing platform 15 being provided below the printing nozzle 14, and a third heating element 17 being provided at the bottom of the printing platform 15.

[0042] (4) Control unit, which includes a computer software console 1, which controls the powder ratio, powder flow rate, powder mixing time, and screw feed flow rate in the batching unit; controls the crucible heating regime in the melting unit; and controls the nozzle printing parameters and glass processing dimensions in the printing unit. The key feature of setting the nozzle printing parameters is the ability to calculate and generate the corresponding glass softening point temperature for each glass component.

[0043] The specific implementation steps of this system include:

[0044] Step 1: Set or generate the following operating parameters in the control unit:

[0045] Glass component ratio and weight: Number each glass component ratio (formulation), select the required components in each glass component ratio, set the glass component ratio and glass preparation weight, select the name of the raw material powder required to introduce the component and enter the purity, perform raw material powder dosage calculation, and generate the raw material powder dosage corresponding to each glass component ratio.

[0046] The maximum number of components that can be selected in each glass component ratio is 10. The maximum number of glass component ratios that can be set at one time is 25. The glass preparation weight is set according to the glass processing size, with a setting range of 50-80 grams.

[0047] Pneumatic powder feeding flow rate: Set the pneumatic powder feeding flow rate of the powder feeder 2 to pneumatically convey each raw material powder in the raw material powder cylinder 3 to the powder mixer 5 through the powder feeding pipeline 4. The pneumatic feeding flow rate can be set according to the amount of each raw material powder in the raw material powder cylinder 3. The pneumatic powder feeding flow rate setting range is 0.2-5g / min.

[0048] Powder mixing time: Set the mixing time of the raw material powder in the powder mixer 5. The powder mixing time can be set according to the total amount of raw material powder conveyed in the raw material powder cylinder 3. The setting range is 5-10 minutes.

[0049] Spiral feeding flow rate: The feeding flow rate from the spiral feeder 7 to the crucible 9 is set as the spiral feeding flow rate. The spiral feeding flow rate can be set according to the total amount of raw material powder conveyed in the raw material powder cylinder 3, and the setting range is 6-10g / min.

[0050] Crucible heating regime: This includes setting the heating rate and target temperature of crucible 9. The heating rate can be set within the range of 5-10℃ / min, and the target temperature can be set to a maximum of 1500℃.

[0051] Nozzle printing parameters: Set the heating rate, printing temperature, and printing speed of the printing nozzle 14, as well as the heating rate and heating temperature of the printing platform 15. The heating rate of the printing platform 15 is set within the range of 5-10℃ / min, and the heating temperature is set within the range of 600-700℃. The heating rate of the printing nozzle 14 is set within the range of 5-10℃ / min. Before setting the printing temperature of the printing nozzle 14, the glass softening point temperature can be calculated and generated in the control panel 1. This generates the glass softening point temperature corresponding to each glass component ratio. The printing temperature of the printing nozzle 14 must be set higher than the glass softening point temperature, increasing it by 250-300℃, with a maximum setting of 1300℃. The printing speed of the printing nozzle 14 is set within the range of 1-3mm / s.

[0052] Glass processing dimensions: Set the length, width, and height of the printed block glass sample 16. The length, width, and height dimensions are all set within the range of 1-4cm.

[0053] Step 2: Start the operation in the control panel 1. The crucible 8, printing nozzle 14 and printing platform 15 start heating according to the set heating regime under the action of the external first heating element 11, second heating element 13 and third heating element 17 respectively. The control panel 1 displays the real-time heating temperature of the crucible 9, printing nozzle 14 and printing platform 15. After reaching the set heating temperature, temperature control and heat preservation begin.

[0054] The temperature control accuracy of the crucible 9 and the printing nozzle 14 is controlled within ±1℃. Depending on the glass melting temperature, the crucible 9 can be made of different materials, such as platinum, corundum, or high-purity alumina ceramic. Similarly, depending on the set heating temperature, the printing nozzle 14 can be made of different materials, such as platinum, corundum, or high-purity alumina ceramic.

[0055] Step 3: After the crucible 9 is kept at the target temperature for 5 minutes, the powder feeder 2 starts to run. The raw material powder in each raw material powder cylinder 3 is pneumatically and quantitatively fed into the powder mixer 5 through the powder feeding pipeline 4 according to the set pneumatic powder feeding flow rate. After the amount of raw material powder fed into each raw material powder cylinder 3 reaches the calculated amount, the powder feeder 2 stops running.

[0056] The powder feeding method adopts a pneumatic feeding system using an inert gas, enabling high-precision conveying of raw material powder in each powder cylinder 3. All powder cylinders 3 can be controlled individually or in combination. When the amount of raw material powder conveyed in each powder cylinder 3 is less than 10g, the feeding accuracy is ±1.5%; when the amount exceeds 10g, the feeding accuracy is ±1%. To ensure good flowability of the raw material powder, the powder is spherical or near-spherical with a particle size range of 15-100μm. The maximum number of powder cylinders 3 can be set to 10, enabling automatic and precise conveying of raw material powders with different compositions and particle sizes of up to 10 components.

[0057] Step four: The powder mixer 5 starts running. The powder mixer 5 mixes the fed raw material powder evenly according to the set powder mixing time. After the mixing time is reached, the powder mixer 5 stops running.

[0058] The powder mixer 5 employs either stirring or pressure-relief mixing methods, enabling the uniform mixing of raw material powders of different components in a specific ratio. When the raw material powder content in the powder cylinder 3 is less than 2%, the mixing uniformity of the raw materials is ±5%; when the raw material powder content is greater than 2%, the mixing uniformity of the raw materials is ±2%.

[0059] Step 5: The screw feeder 7 starts operating. The powder (i.e., the batching material) that is mixed evenly in the powder mixer 5 flows into the screw feeder 7 along the batching feed pipe 6. The screw feeder 7 feeds the material into the crucible 9 in a screw manner according to the set screw feeding flow rate. After feeding is completed, the crucible 9 is subjected to temperature control and heat preservation. The temperature control and heat preservation time can be set according to the total amount of batching material. The temperature control and heat preservation time setting range is 10-20 minutes, so that the material can completely react in the crucible 9 to become molten glass.

[0060] Step six: After the crucible 9 reaches the holding time, the printing nozzle 14 begins to feed. At this time, the molten glass in the crucible 9 is transported to the printing nozzle 14 through the glass liquid pipeline 12. After the glass liquid is continuously heated and softened by the second heating element 13 arranged around the printing nozzle 14, the temperature of the glass liquid at the printing nozzle 14 reaches the set printing temperature of the printing nozzle 14.

[0061] The optimal printing temperature for the printing nozzle 14 must be set 250-300°C higher than the glass softening point. The software system on console 1 can pre-calculate and predict the glass softening point based on the composition of the glass being prepared, thereby guiding the setting of the glass fused deposition nozzle printing temperature parameters. The specific calculation process and method for predicting the softening point of the prepared glass in the software system are as follows: Figure 2 As shown, it includes the following steps:

[0062] (1) Collect glass softening point temperature data under different component ratios of 10 components and construct a ratio-performance dataset;

[0063] (2) To improve the accuracy of model calculations, the ratio-performance dataset needs to be cleaned, including:

[0064] Delete data with the same proportions but different performance.

[0065] Remove duplicate data values ​​from the data, keeping only the first duplicate data entry;

[0066] Retain data where the total proportion of 10 components is ≥95%;

[0067] Data with softening point temperatures between 650-750℃ were selected.

[0068] Data with a SiO2 mass ratio ≥ 40% were selected;

[0069] (3) In order to eliminate the influence of different oxide contents of different orders of magnitude in the sample, it is necessary to standardize the cleaned ratio-performance dataset.

[0070] (4) Based on the standardized ratio-performance dataset, a model for predicting the softening point temperature of glass is constructed. The model structure is shown below:

[0071]

[0072] Where y′ is the glass softening point temperature after standardization, and b i ,b i,k To estimate the coefficients of the model for predicting the softening point temperature, x′ i To represent the content of the i-th oxide in the standardized component, x′ k The content of the k-th oxide in the component after standardization;

[0073] The coefficients to be estimated in this model need to be solved. First, the loss function is constructed using the least squares method:

[0074]

[0075] Since the loss function is differentiable with respect to the coefficients to be estimated, Newton's iteration method is used to solve for the coefficients to be estimated.

[0076] (5) If you want to predict the glass softening point temperature of the new component ratio, you need to standardize the ratio-performance dataset of the new component ratio to be predicted. The mean and variance during the standardization process are the same as the mean and variance during the standardization process in step (3) above. Then, substitute them into the model for predicting the glass softening point temperature above. Finally, perform inverse standardization on the obtained glass softening point temperature to obtain the glass softening point temperature of the new component ratio to be predicted.

[0077] Step 7: The molten glass in the printing nozzle 14 is squeezed out. The printing nozzle 14 starts to move along the xy plane according to the set printing speed and the size contour information of the block glass sample 16. The molten glass is continuously fed through the molten glass pipeline 12. Along the path of the printing nozzle 14, it is coated on the printing platform 15 and hardens and sets after encountering the cooler air, forming a thin contour. After printing one layer of slices, the printing platform 15 moves down one more layer and repeats the above process until the desired block glass sample 16 is printed.

[0078] Step eight, repeating steps one through seven, can achieve high-throughput fabrication of up to 25 different glass component ratios for printed bulk glass samples.

[0079] Step 9: After a batch of bulk glass array samples are prepared in high throughput, the samples are taken out from the worktable 17 and placed in the annealing furnace for annealing.

[0080] Step 10: Process the upper and lower surfaces of the annealed bulk glass sample for subsequent performance characterization tests.

[0081] The present invention will now be described in detail with reference to specific embodiments.

[0082] The specific implementation steps of this system include:

[0083] Step 1: Design and prepare 25 glass oxide formulations with different components as shown in Tables 1-3. The maximum number of components in each glass oxide formulation is 10. Set or generate the following parameters in the control panel:

[0084] Glass composition ratio: Set glass formula numbers 1-25# sequentially. As shown in Tables 1-3, select specific oxide components in each formula, set the specific oxide ratio and glass preparation weight of 60g, select the name of the powder raw material required to introduce the oxide and enter the purity, and execute the calculation of the amount of each powder raw material in the control console.

[0085] Pneumatic powder feeding flow rate: When the amount of raw material powder conveyed in each raw material powder cylinder is greater than 10g, the corresponding pneumatic powder feeding flow rate is set to 4g / min; when the amount of raw material powder conveyed in each raw material powder cylinder is less than 10g, the pneumatic powder feeding flow rate is set to 1g / min.

[0086] Powder mixing time: Set the mixing time of the raw material powder in the mixer to 5 minutes.

[0087] Screw feeder flow rate: Set the screw feeder flow rate to 10g / min.

[0088] Crucible heating regime: Set the heating rate and heating temperature of the crucible. The heating rate is 10℃ / min and the heating temperature is 1450℃.

[0089] Nozzle printing parameters: Before setting the nozzle printing temperature, first calculate and generate the glass softening point temperature in the control panel to generate the glass softening point temperature corresponding to each formula. Then, set the nozzle printing temperature by referencing the glass softening point temperature. The nozzle printing temperature should be set 275℃ higher than the glass softening point temperature. Specific settings are shown in Tables 1-3. The nozzle heating rate is set to 10℃ / min. The specific nozzle printing speed settings are shown in Tables 1-3. The printing platform heating rate is set to 10℃ / min, and the heating temperature is set to 650℃.

[0090] Glass processing dimensions: Set the length, width, and height of the printed block glass sample. Set the length and width to 3cm and the height to 2cm.

[0091] Step two: Start the program in the control panel. The crucible and printing nozzle will begin heating at the set temperature increase rate of 10℃ / min. The control panel will display the current temperatures of the crucible and printing nozzle. Once the crucible and printing nozzle temperatures reach their set heating temperatures, temperature control and heat preservation will begin. The crucible is made of platinum. The nozzle is made of high-purity alumina ceramic.

[0092] Step 3: After the crucible has been kept at the target temperature for 5 minutes, the powder feeder starts operating. All raw material powder cylinders are individually controlled, and the raw material powder within each cylinder is conveyed according to the set powder delivery flow rate. The powder is then pneumatically conveyed to the mixer in a quantitative manner through the powder delivery pipeline. The raw material powder is spherical with a particle size of 50 μm, and argon gas is used. The powder feeder stops operating once the calculated powder delivery amount has been reached in each raw material powder cylinder.

[0093] Step 4: The powder mixer starts running automatically. The powder mixer mixes the raw material powder according to the set powder mixing time. After the mixing time reaches 5 minutes, the powder mixer stops running.

[0094] Step 5: The screw feeder starts operating. The uniformly mixed raw material in the powder mixer flows into the screw feeder along the feeding pipe. The screw feeder slowly feeds the material into the crucible in a spiral manner at a set feeding flow rate of 10g / min. After feeding is completed, the crucible heating temperature is restored to 1450℃ and then controlled and held for 15 minutes, allowing the powder to completely react in the crucible into a molten glass liquid state.

[0095] Step six: After the crucible reaches the 15-minute holding time, the printing nozzle begins feeding. At this time, the molten glass in the crucible is transported to the printing nozzle through a pipe. After the molten glass is continuously heated and softened by the heating element near the printing nozzle, the temperature of the molten glass at the printing nozzle reaches the set printing temperature.

[0096] Step seven: The molten glass in the printing nozzle is expelled by pressure. The printing nozzle moves along the xy plane according to the set printing speed and the size and contour information of the bulk glass sample. Molten glass is continuously fed through the pipeline, and along the path of the printing nozzle, it is coated onto the printing platform and hardens and sets upon encountering the cooler air, forming a thin contour. After printing one layer, the printing platform moves down another layer. The above process is repeated until the desired bulk glass material sample is printed.

[0097] Step eight: Repeat steps one through seven. Depending on the set number of formulations, up to 25 different formulations of discrete bulk glass samples can be fabricated in high throughput. The resulting bulk glass array samples are shown below. Figure 3 As shown.

[0098] Step 9: After a batch of bulk glass array samples has been fabricated in high throughput, the samples are removed from the printing platform and placed in an annealing furnace for annealing.

[0099] Step 10: Grind and polish the upper and lower surfaces of the 25 annealed block glass samples, observe the surface quality of the glass samples, and test the density and elastic modulus of the samples. The test results are shown in Tables 1, 2 and 3.

[0100] Table 1. Component design of the glass formulation and test results of the elastic modulus of 5×5 bulk glass samples prepared in one step.

[0101]

[0102]

[0103] Table 2. Component design of the glass formulation and test results of the elastic modulus of 5×5 block glass samples prepared in one step.

[0104]

[0105] Table 3. Component design of the glass formulation and test results of the elastic modulus of 5×5 block glass samples prepared in one step.

[0106]

[0107]

[0108] As can be seen from Tables 1-3, the preparation method described in this invention can quickly and efficiently produce bulk glass material array samples with 25 different components in high throughput, which greatly improves the preparation efficiency of glass samples. After density and modulus testing, the correlation between glass composition, density and modulus can be quickly established, which greatly improves the efficiency of glass composition optimization verification and screening, and realizes the rapid research and development of new glass materials.

[0109] While the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the invention. Those skilled in the art can make various modifications and refinements without departing from the spirit and scope of the invention. Therefore, the scope of protection of the present invention shall be determined by the claims.

Claims

1. A high-throughput preparation method for multi-component glass materials based on fused deposition modeling technology, characterized in that, include: Step 1: Set or generate the various operating parameters; Step 2: Start-up. The crucible in the melting unit, as well as the printing nozzle and printing platform in the printing unit, begin heating according to the set operating parameters. The control console in the control unit displays the heating temperature in real time. After reaching the set heating temperature, temperature control and heat preservation begin. Step 3: After the crucible has been kept at the target temperature for a period of time, the powder feeder in the batching unit starts to run, and the raw material powder is quantitatively fed into the powder mixer. When the amount of powder fed reaches the calculated amount, the powder feeder stops running. Step four: The powder mixer mixes the fed raw material powder evenly. After the powder mixing time is reached, the powder mixer stops running. Step 5: The evenly mixed powder flows into the screw feeder, which feeds the material into the crucible. After feeding is completed, the crucible is kept at a controlled temperature. The powder reacts completely in the crucible to form molten glass. Step six: The molten glass liquid in the crucible is transported to the printing nozzle, where it is continuously heated and softened by the heating elements around the printing nozzle. At this point, the temperature of the molten glass liquid at the printing nozzle reaches the set printing temperature. Step 7: After the printing nozzle prints one layer of slices on the printing platform according to the preset printing parameters and glass processing dimensions, the printing platform moves down one layer and repeats the above process until the desired printed block glass sample is printed. The printing parameters include setting the heating rate of the printing nozzle, the printing temperature and the printing speed, as well as the heating rate and heating temperature of the printing platform. The printing temperature is the glass softening point temperature + (250-300)℃, and does not exceed 1300℃. The glass softening point temperature is obtained through the following steps: (1) Collect glass softening point temperature data under different component ratios for specific components and construct a ratio-performance dataset; (2) To improve the accuracy of model calculations, the matching-performance dataset needs to be cleaned, including: Delete data with the same proportions but different performance; Remove duplicate data from the dataset, keeping only the first record of each duplicate. Data with a total component ratio ≥ 95% were retained; Data with softening point temperatures between 650-750℃ were selected. Data with a SiO2 mass ratio ≥ 40% were selected; (3) In order to eliminate the influence of different oxide contents of different orders of magnitude in the sample, the ratio-performance dataset after cleaning was standardized. (4) Based on the standardized ratio-performance dataset, a model for predicting the glass softening point temperature is constructed, as shown below: ; in The softening point temperature of the glass after standardization treatment. To predict the coefficients of the softening point temperature model, To represent the content of the i-th oxide in the component after standardization. The content of the k-th oxide in the standardized component is given, where n is the number of components and n≤10; The coefficients to be estimated in the model are solved, and the loss function is constructed based on the least squares method: ; The Newton-Raphson iteration method is used to solve for the coefficients to be estimated. (5) For the glass softening point temperature of the new component ratio to be predicted, the proportion-performance dataset of the new component ratio is standardized and then substituted into the above model for predicting the glass softening point temperature. Finally, the obtained glass softening point temperature is de-standardized to obtain the glass softening point temperature of the new component ratio to be predicted. The number of components of the new component ratio to be predicted is not greater than the number of components of the model for predicting the glass softening point temperature. Step 8: Repeat steps 1 to 7 to complete multiple printed bulk glass samples with different glass composition ratios. Step 9: After a batch of printed bulk glass samples has been prepared, remove them and anneal them.

2. The preparation method according to claim 1, characterized in that, Set or generate various operating parameters in the control unit, including glass component ratio and glass preparation weight, pneumatic powder feeding flow rate, powder mixing time, screw feeding flow rate, crucible heating regime, printing parameters, and glass processing dimensions.

3. The preparation method according to claim 2, characterized in that, The number of components in the glass composition is no more than 10, the number of glass composition ratios set at one time is no more than 25, and the weight of the glass preparation is 50-80 grams.

4. The preparation method according to claim 2, characterized in that, The pneumatic powder delivery flow rate is 0.2-5 g / min.

5. The preparation method according to claim 2, characterized in that, The powder mixing time is 5-10 minutes.

6. The preparation method according to claim 2, characterized in that, The screw feed flow rate is 6-10 g / min.

7. The preparation method according to claim 2, characterized in that, The crucible heating regime includes setting the crucible heating rate and target temperature, wherein the heating rate is 5-10℃ / min and the target temperature does not exceed 1500℃.

8. The preparation method according to claim 1 or 2, characterized in that, The heating rate of the printing platform is 5-10℃ / min, and the heating temperature is 600-700℃; the heating rate of the printing nozzle is 5-10℃ / min, and the printing speed is 1-3mm / s.