A small molecule anti-mud agent
By synthesizing a small molecule linear polymer anti-mud agent in a polycarboxylate water-reducing agent and using functional groups such as ether bonds and amino groups to adsorb clay, the problem of the polycarboxylate water-reducing agent being sensitive to mud content has been solved and the concrete has been significantly improved. Excellent fluidity and slump, achieving low-cost and efficient anti-mud effect.
Patent Information
- Application Number
- CN202310591704.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-05-24
AI Technical Summary
Polycarboxylate superplasticizers are sensitive to mud content, resulting in poor fluidity, large slump loss and reduced strength of concrete. Existing methods to improve mud resistance are costly and the dosage is too large.
Small molecule linear polymers are synthesized through condensation reactions of materials with different functional groups to prepare anti-mud agents. The process is simple and low-cost. Functional groups such as ether bonds, amino groups and hydroxyl groups are used to improve dispersion efficiency, adsorb clay, and improve anti-mud effects.
It significantly improves the adsorption effect of anti-mud agent on various clays, improves the fluidity and slump of concrete, reduces costs, and achieves anti-mud effect with low dosage.
Smart Images

Figure GDA0004354818550000041 
Figure GDA0004354818550000042 
Figure GDA0004354818550000051
Abstract
Description
Technical Field
[0001] The invention relates to the field of concrete admixtures, in particular to a small molecule anti-mud agent. Background Art
[0002] As a necessary admixture for concrete, polycarboxylate water reducer has the characteristics of low dosage, high water reduction rate, good slump retention, designable molecular structure, and no pollution. However, it is extremely sensitive to mud content, which leads to poor concrete fluidity, large slump loss, and reduced strength. With the widespread application of machine-made sand, construction waste, etc. in concrete materials, their mud content has affected the quality of concrete. How to improve the anti-mud performance of polycarboxylate water reducer has become a technical problem in the concrete industry, which has important theoretical significance and engineering value.
[0003] At present, the main methods to improve the anti-mud performance are: on the one hand, compounding anti-mud agents in polycarboxylic acid water-reducing agents, and on the other hand, synthesizing anti-mud polycarboxylic acid water-reducing agents, which generally use cationic monomers to participate in the polymerization reaction of water-reducing agents or anti-mud agents. The anti-mud effect is significant, but there are common problems of high cost and excessive dosage. Summary of the invention
[0004] The purpose of the present invention is to provide a small molecule anti-mud agent, which utilizes materials with different functional groups to carry out condensation reaction to synthesize a small molecule straight-chain polymer, which has the characteristics of low dosage, simple preparation, low cost, etc.
[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0006] A small molecule anti-mud agent comprises the following substances in parts by weight: 60-80 parts of anti-mud agent mother solution, 10-20 parts of sulfate, and 10-20 parts of polyol.
[0007] Furthermore, the preparation process of the anti-mud agent mother solution comprises the following steps:
[0008] S1. In a reaction apparatus equipped with a stirrer, a thermometer and a reflux condenser, add a certain amount of water, melamine, urea, sodium sulfite, formaldehyde, add caustic soda to adjust the pH of the system to 9-10 and stir evenly;
[0009] S2. Reaction at 80-85℃ for 2 hours;
[0010] S3. Add citric acid to adjust the pH to 4-5, and continue the reaction at 80°C;
[0011] S4. During the constant temperature process, take samples to determine the product molecular weight. When the product molecular weight is between 1200 and 1500, the reaction ends. Add caustic soda to adjust the pH to 8-9.
[0012] Furthermore, the preparation process of the anti-mud agent mother solution comprises the following steps:
[0013] S1. In a reaction apparatus equipped with a stirrer, a thermometer and a reflux condenser, add a certain amount of water, melamine, urea, aminosulfonic acid, formaldehyde, add caustic soda to adjust the pH of the system to 9-10 and stir evenly;
[0014] S2. Reaction at 80-85℃ for 2 hours;
[0015] S3. Add citric acid to adjust the pH to 4-5, and continue the reaction at 80°C;
[0016] S4. During the constant temperature process, take samples to determine the product molecular weight. When the product molecular weight is between 1200 and 1500, the reaction ends. Add caustic soda to adjust the pH to 8-9.
[0017] Furthermore, the preparation process of the anti-mud agent mother solution comprises the following steps:
[0018] S1. In a reaction apparatus equipped with a stirrer, a thermometer and a reflux condenser, add a certain amount of water, melamine, urea, sodium p-aminobenzenesulfonate, formaldehyde, add caustic soda to adjust the pH of the system to 9-10, and stir evenly;
[0019] S2. Reaction at 80-85℃ for 2 hours;
[0020] S3. Add citric acid to adjust the pH to 4-5, and continue the reaction at 80°C;
[0021] S4. During the constant temperature process, take samples to determine the product molecular weight. When the product molecular weight is between 1200 and 1500, the reaction ends. Add caustic soda to adjust the pH to 8-9.
[0022] Compared with the prior art, the beneficial effects of the present invention are:
[0023] 1. The present invention uses formaldehyde, melamine, sulfonating agent, and urea to synthesize a small molecular linear oligomer through hydroxymethylation, sulfonation, condensation and other reactions under alkaline adjustment. The oligomer contains functional groups such as ether bonds, amino groups, hydroxyl groups and sulfonic acid groups, and the molecular weight is similar to the side chain PEO in PCE. The amino group is tightly adsorbed between the montmorillonite layers through hydrogen bonds, which prevents the PCE side chain intercalation and improves the dispersion efficiency of PCE.
[0024] 2. The anti-mud agent of the present invention has a simple synthesis and preparation process, and the raw materials are cheap and readily available.
[0025] 3. The anti-mud agent of the present invention has a significant anti-mud effect and has a good adsorption effect on various clays such as illite, kaolinite, montmorillonite, etc. DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the application equally.
[0027] Example 1: A small molecule anti-mud agent, comprising the following substances in parts by weight: 80 parts of anti-mud agent mother solution, 10 parts of sodium pyrosulfite, and 10 parts of sorbitol are stirred evenly to obtain 1 # Small molecule anti-mud agent.
[0028] The preparation process of the anti-mud agent mother solution comprises the following steps:
[0029] S1. In a reaction apparatus equipped with a stirrer, a thermometer and a reflux condenser, 850 parts of water, 126 parts of melamine, 6 parts of urea, 113 parts of sodium sulfite, 243 parts of formaldehyde, and a caustic soda tablet was added to adjust the pH of the system to 9 and stirred evenly;
[0030] S2. Reaction at 80℃ for 2 hours;
[0031] S3. Add citric acid to adjust the pH to 5 and continue the reaction at 80°C;
[0032] S4. During the constant temperature process, samples were taken to determine the molecular weight of the product. When the molecular weight of the product was between 1200 and 1400, the reaction was terminated and caustic soda was added to adjust the pH to 9.
[0033] The molecular structure of the prepared anti-mud agent mother solution is
[0034]
[0035] Example 2: A small molecule anti-mud agent, comprising the following substances in parts by weight: 70 parts of anti-mud agent mother solution, 20 parts of sodium sulfite, and 10 parts of polyglycerol are stirred evenly to obtain 2 # Small molecule anti-mud agent.
[0036] The preparation process of the anti-mud agent mother solution comprises the following steps:
[0037] S1. In a reaction apparatus equipped with a stirrer, a thermometer and a reflux condenser, 774 parts of water, 126 parts of melamine, 6 parts of urea, 90 parts of sulfamic acid, 243 parts of formaldehyde were added, and the pH of the system was adjusted to 10 by adding caustic soda and stirring;
[0038] S2. Reaction at 85℃ for 2 hours;
[0039] S3. Add citric acid to adjust the pH to 4 and continue the reaction at 80°C;
[0040] S4. During the constant temperature process, samples were taken to determine the molecular weight of the product. When the molecular weight of the product was between 1400 and 1500, the reaction was terminated and caustic soda was added to adjust the pH to 8.
[0041] The molecular structure of the prepared anti-mud agent mother solution is
[0042]
[0043] Example 3: A small molecule anti-mud agent, comprising the following substances in parts by weight: 72 parts of anti-mud agent mother solution, 15 parts of potassium sulfate, and 13 parts of diethylene glycol are stirred evenly to obtain 2 # Small molecule anti-mud agent.
[0044] The preparation process of the anti-mud agent mother solution comprises the following steps:
[0045] S1. In a reaction apparatus equipped with a stirrer, a thermometer and a reflux condenser, 1137 parts of water, 126 parts of melamine, 6 parts of urea, 208 parts of sodium p-aminobenzenesulfonate, 243 parts of formaldehyde, and a caustic soda tablet was added to adjust the pH of the system to 9.3 and stirred evenly;
[0046] S2. Reaction at 83℃ for 2 hours;
[0047] S3. Add citric acid to adjust the pH to 4.8 and continue the reaction at 80°C;
[0048] S4. During the constant temperature process, samples were taken to determine the molecular weight of the product. When the molecular weight of the product was between 1300 and 1500, the reaction was terminated and caustic soda was added to adjust the pH to 8.4.
[0049] The molecular structure of the prepared anti-mud agent mother solution is
[0050]
[0051] Example 4: Performance Test
[0052] 1. Cement paste fluidity test
[0053] The samples synthesized in the above embodiment were tested according to the cement paste fluidity test method in GB / T8077-2012 "Concrete admixture homogeneity test method", cement is Shanshui P.O42.5, 295.5g, montmorillonite is montmorillonite KSF (Aladdin reagent), 4.5g, water 87g, PCE synthesized by our company, 40% content, 0.8g, anti-mud agent 0.20g. The test results are shown in Table 1.
[0054] Table 1
[0055]
[0056] From the data in Table 1, it can be seen that the initial and 1-hour fluidity losses of the pure slurry are greatly improved by adding various anti-mud agents, and the anti-mud effect is significant.
[0057] 2. Concrete performance test
[0058] The test concrete mix proportions are shown in Table 2.
[0059] Table 2
[0060] Material cement Fly ash Mineral powder Machine-made sand Stone water Usage / m3 240 80 80 900 900 170
[0061] Among them, the sand content is 4.0%.
[0062] The concrete test results are shown in Table 3.
[0063] Table 3
[0064] Sample No. Solid content (%) Initial slump (mm) 1h slump (mm) PCE 0.25 210 140 <![CDATA[PCE + Anti-sludging Agent 1 # > 0.25+0.03 225 195 <![CDATA[PCE + Anti-sludging agent 2 # > 0.25+0.03 230 220 <![CDATA[PCE + Anti-sludging Agent 3 # > 0.25+0.03 230 230
[0065] From the data in Table 3, it can be seen that after adding various anti-mud agents, the initial slump and 1h slump of concrete are significantly improved, showing good anti-mud performance.
Claims
1. A small molecule anti-mud agent, characterized in that: The material comprises the following parts by weight: 60-80 parts of anti-mud agent mother solution, 10-20 parts of sulfate, and 10-20 parts of polyol; The preparation process of the anti-mud agent mother solution comprises the following steps: S1. In a reaction apparatus equipped with a stirrer, a thermometer and a reflux condenser, add a certain amount of water, melamine, urea, sodium sulfite, formaldehyde, add caustic soda to adjust the pH of the system to 9-10 and stir evenly; S2. Reaction at 80-85℃ for 2 hours; S3. Add citric acid to adjust the pH to 4-5, and continue the reaction at 80°C; S4. During the constant temperature process, take samples to determine the product molecular weight. When the product molecular weight is between 1200 and 1500, the reaction ends. Add caustic soda to adjust the pH to 8-9.
2. A small molecule anti-mud agent, characterized in that: The material comprises the following parts by weight: 60-80 parts of anti-mud agent mother solution, 10-20 parts of sulfate, and 10-20 parts of polyol; The preparation process of the anti-mud agent mother solution comprises the following steps: S1. In a reaction apparatus equipped with a stirrer, a thermometer and a reflux condenser, add a certain amount of water, melamine, urea, aminosulfonic acid, formaldehyde, add caustic soda to adjust the pH of the system to 9-10 and stir evenly; S2. Reaction at 80-85℃ for 2 hours; S3. Add citric acid to adjust the pH to 4-5, and continue the reaction at 80°C; S4. During the constant temperature process, take samples to determine the product molecular weight. When the product molecular weight is between 1200 and 1500, the reaction ends. Add caustic soda to adjust the pH to 8-9.
3. A small molecule anti-mud agent, characterized in that: The material comprises the following parts by weight: 60-80 parts of anti-mud agent mother solution, 10-20 parts of sulfate, and 10-20 parts of polyol; The preparation process of the anti-mud agent mother solution comprises the following steps: S1. In a reaction apparatus equipped with a stirrer, a thermometer and a reflux condenser, add a certain amount of water, melamine, urea, sodium p-aminobenzenesulfonate, formaldehyde, add caustic soda to adjust the pH of the system to 9-10 and stir evenly; S2. Reaction at 80-85℃ for 2 hours; S3. Add citric acid to adjust the pH to 4-5, and continue the reaction at 80°C; S4. During the constant temperature process, take samples to determine the product molecular weight. When the product molecular weight is between 1200 and 1500, the reaction ends. Add caustic soda to adjust the pH to 8-9.