A kind of thermal insulation coating for decorative board and preparation method thereof
By modifying hollow glass microspheres and hydroxyl-terminated silicone-modified epoxy resin, its compatibility and adhesion are enhanced, solving the problem of poor compatibility between hollow glass microspheres and organic resins, and significantly improving the performance of thermal insulation coatings. Insulation and anti-cracking properties.
Patent Information
- Application Number
- CN202310683966.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-06-10
AI Technical Summary
The poor compatibility between hollow glass microspheres and organic resins results in reduced thermal insulation performance and insufficient cracking resistance of thermal insulation coatings, limiting its application.
By modifying hollow glass beads and hydroxyl-terminated silicone-modified epoxy resin, hydroxyl groups are introduced to enhance compatibility and adhesion, and hydrogen bonding is used to further improve compatibility and adhesion to form hydrogen bonds. to enhance the combination of the two.
The thermal insulation performance, adhesion and cracking resistance of the thermal insulation coating are significantly improved, meeting actual engineering needs.
Smart Images

Figure BDA0004277930010000091 
Figure BDA0004277930010000101
Abstract
Description
Technical Field
[0001] The present application relates to the field of decorative board technology, and in particular to a thermal insulation coating for decorative boards and a preparation method thereof. Background Art
[0002] Decorative board coatings refer to coatings that are sprayed or applied on the surface of decorative boards for beautification or functional purposes. They are the decisive factors for the quality and performance of decorative boards. Decorative board thermal insulation coatings are a new type of thermal insulation material, a type of coating that achieves thermal insulation through low thermal conductivity and high thermal resistance. Thermal insulation coatings are generally divided into barrier-type thermal insulation coatings, reflective thermal insulation coatings, and radiant thermal insulation coatings. The mechanism of barrier-type thermal insulation coatings for decorative boards is to prevent heat conduction by adding thermal insulation fillers. The coating formed after the coating is applied is full of voids, which reduces the thermal conductivity coefficient.
[0003] Hollow glass microspheres are tiny, hollow spherical powders. They are a new ultra-light inorganic non-metallic material with excellent performance. They are light in weight, large in volume, low in thermal conductivity, high in compressive strength, and have good dispersibility, fluidity, and chemical stability. They also have excellent properties such as insulation, self-lubrication, heat preservation, sound insulation, non-absorbent, fire resistance, and corrosion resistance. They are often used in thermal insulation coatings as thermal insulation fillers.
[0004] However, due to the poor compatibility between hollow glass microspheres and organic resins, the thermal insulation performance of the resulting thermal insulation coating is reduced, the anti-cracking performance is weak, and it is difficult to meet the needs of actual engineering projects, which greatly limits its application. Therefore, it is urgent to improve the compatibility between hollow glass microspheres and organic resins and improve the performance of thermal insulation coatings. Summary of the invention
[0005] In order to improve the compatibility between hollow glass microspheres and organic resins, the present application provides a thermal insulation coating for decorative panels and a preparation method thereof.
[0006] The present application provides a thermal insulation coating for decorative panels, which adopts the following technical solution:
[0007] A thermal insulation coating for decorative panels and a preparation method thereof. The raw materials include, by weight: 30-50 parts of hydroxyl-terminated silicone-modified epoxy resin, 5-20 parts of calcium sulfate whiskers, 20-40 parts of hydroxyl-modified hollow glass microspheres, 10-20 parts of sepiolite fibers, 3-21 parts of calcium hydroxide, 3-13 parts of nano titanium dioxide, 1-5 parts of thickeners, 1-3 parts of leveling agents, 1-3 parts of defoamers, 3-5 parts of dispersants, 1-3 parts of multifunctional additives, 3-5 parts of curing agents, 30-60 parts of ethanol, and 20-50 parts of deionized water.
[0008] By adopting the above technical scheme, the hollow glass microspheres are modified to generate hydroxyl groups on their surface, thereby improving the compatibility of the hollow glass microspheres in organic resins; at the same time, a modified epoxy resin with hydroxyl-terminated silicone is used to make the epoxy resin chain structure have Si-O segments and hydroxyl groups, thereby enhancing the stability of the epoxy resin, improving the crack resistance, and enhancing the interfacial adhesion, which can effectively improve the compatibility between the epoxy resin and the hollow glass microspheres; at the same time, a large number of hydroxyl groups are introduced on the surfaces of both, which can effectively form hydrogen bonds, and under the action of hydrogen bonds, the compatibility and adhesion between the two are further enhanced, thereby effectively improving the thermal insulation, adhesion, crack resistance and other properties of the thermal insulation coating.
[0009] Preferably, the hydroxyl-terminated silicone-modified epoxy resin is composed of the following components: hydroxyl-terminated polydimethylsiloxane, bisphenol A epoxy resin, and a catalyst, and the weight ratio of the three is 1: (8-10): (0.3-0.7).
[0010] By adopting the above technical scheme, bisphenol A epoxy resin is modified by using hydroxyl-terminated polydimethylsiloxane. Under the action of a catalyst, the terminal hydroxyl polydimethylsiloxane reacts chemically with the epoxy resin functional group, so that the epoxy resin chain structure produces Si-O chain segments, thereby enhancing the stability of the epoxy resin. There are no other atoms and groups around the oxygen atom of the Si-O bond, the bond angle and bond length are large, the distance between adjacent non-bonded atoms is larger than that of the Si-Si bond, and the internal rotation is easier than that of the CO chain. Therefore, the flexibility of the epoxy resin chain segment is increased, the bending strength is reduced, the device's ability to resist stress dispersion and impact is enhanced, and the anti-cracking performance of the epoxy resin is effectively increased.
[0011] Preferably, the hydroxyl-modified hollow glass microspheres are composed of the following components in parts by weight: 8-16 parts of hollow glass microspheres, 40-60 parts of sodium hydroxide, 4-8 parts of hydroxyl-terminated polydimethylsiloxane, 0.5-0.7 parts of catalyst, 10-20 parts of deionized water, and 10-20 parts of ethanol.
[0012] By adopting the above technical scheme, sodium hydroxide is used to make the surface of the hollow glass microspheres rough and produce hydroxyl groups, and then the hydroxylated hollow glass microspheres are further modified by hydroxyl-terminated polydimethylsiloxane to obtain hollow glass microspheres containing a large number of Si-O segments and hydroxyl groups on the surface. This not only effectively improves the compatibility and adhesion of the hollow glass microspheres in the organic resin, but also further improves the comprehensive mechanical properties of the thermal insulation coating.
[0013] Preferably, the mass ratio of the hollow glass microspheres to the hydroxyl-terminated polydimethylsiloxane is 1:(0.5-0.7).
[0014] Preferably, the catalyst is dibutyltin dilaurate.
[0015] By adopting the above technical solution and using dibutyltin dilaurate as a catalyst, the hydroxyl-terminated polydimethylsiloxane can be effectively promoted to react with the hydroxyl groups on the surface of the epoxy resin and the hydroxylated hollow glass microspheres to produce Si-O segments.
[0016] Preferably, the multifunctional adjuvant is AMP-95 regulator.
[0017] By adopting the above technical solution and using AMP-95 regulator as a multifunctional additive, the dispersion ability of the coating can be improved, the pH value and other properties can be stabilized, and the service life of the coating can be extended.
[0018] The present application also provides a method for preparing a thermal insulation coating for a decorative panel, which adopts the following technical solution:
[0019] A method for preparing a thermal insulation coating for a decorative plate comprises the following steps:
[0020] S1. At 40-60°C, 30-50 parts by weight of hydroxyl-terminated silicone-modified epoxy resin, 5-20 parts of calcium sulfate whiskers, 20-40 parts of hydroxyl-modified hollow glass microspheres, 10-20 parts of sepiolite fibers, 3-5 parts of dispersant, 30-60 parts of ethanol, and 20-50 parts of deionized water are stirred at a stirring speed of 1000-1500 rpm to obtain a mixture A;
[0021] S2. Add 3-21 parts of calcium hydroxide, 3-13 parts of nano-titanium dioxide, and 1-5 parts of a thickener to the mixture A, and stir at a stirring speed of 600-800rpm to obtain a mixture B;
[0022] S3. At a stirring speed of 300-400 rpm, add 1-3 parts of leveling agent, 1-3 parts of defoaming agent, 1-3 parts of multifunctional additive, and 3-5 parts of curing agent to mixed material B in sequence, mix well, and obtain a thermal insulation coating for decorative panels.
[0023] By adopting the above technical scheme, the compatibility and adhesion between the hollow glass microspheres and the epoxy resin are enhanced by using hydroxyl-modified hollow glass microspheres and hydroxyl-terminated silicone-modified epoxy resin, thereby effectively improving the thermal insulation, adhesion, anti-cracking and other properties of the thermal insulation coating.
[0024] Preferably, the method for preparing the hydroxyl-terminated silicone-modified epoxy resin comprises the following steps:
[0025] S1. Weigh hydroxyl-terminated polydimethylsiloxane, bisphenol A epoxy resin, and catalyst in a weight ratio of 1:(8-10):(0.3-0.7);
[0026] S2. After mixing the hydroxyl-terminated polydimethylsiloxane and bisphenol A epoxy resin, heat to 120-150°C and stir for 5-15 minutes; then add the catalyst and react at a temperature of 120-150°C and a vacuum degree of -0.1-0.1MPa for 2-4 hours, and obtain a hydroxyl-terminated silicone-modified epoxy resin after cooling.
[0027] By adopting the above technical scheme, bisphenol A epoxy resin is modified by using hydroxyl-terminated polydimethylsiloxane. Under the action of a catalyst, the terminal hydroxyl polydimethylsiloxane reacts chemically with the epoxy resin functional group, so that Si-O segments are present in the epoxy resin chain structure, thereby effectively enhancing the compatibility and interfacial adhesion of the epoxy resin.
[0028] Preferably, the method for preparing the hydroxyl-modified hollow glass microspheres comprises the following steps:
[0029] S1. Add 8-16 parts of hollow glass microspheres to 40-60 parts of sodium hydroxide by weight, stir for 3-9h, and filter out the hollow glass microspheres; first pickle the hollow glass microspheres, then wash the hollow glass microspheres with water until the pH of the washing waste liquid reaches 6-7, and vacuum dry the obtained hollow glass microspheres to obtain pretreated hollow glass microspheres;
[0030] S2. Add 4-8 parts of hydroxyl-terminated polydimethylsiloxane to 10-20 parts of deionized water and 10-20 parts of ethanol, stir evenly, and adjust the pH of the solution to 4-6; obtain an organosilicon solution;
[0031] S3. Add the pretreated hollow glass microspheres in S1 to the organosilicon solution in S2, add 0.5-0.7 parts of catalyst, stir for 6-18 hours, and then perform vacuum drying reaction at 60-80° C. to obtain hydroxyl-modified hollow glass microspheres.
[0032] By adopting the above technical scheme, the surface of the hollow glass microspheres is first roughened and hydroxyl groups are formed using sodium hydroxide, and then the hydroxylated hollow glass microspheres are further modified using organosilicon hydroxyl-terminated polydimethylsiloxane, thereby effectively improving the compatibility and adhesion of the hollow glass microspheres in the organic resin.
[0033] Preferably, the vacuum drying reaction time in S3 is 15-25 hours.
[0034] In summary, the present application includes at least one of the following beneficial technical effects:
[0035] 1. By adopting the above technical scheme, the hollow glass microspheres are modified to generate hydroxyl groups on their surface, thereby improving the compatibility of the hollow glass microspheres in organic resins; at the same time, the modified epoxy resin of hydroxyl-terminated silicone is adopted, so that there are Si-O segments and hydroxyl groups in the epoxy resin chain structure, so that the stability of the epoxy resin is enhanced, the crack resistance is improved, and the interfacial adhesion is enhanced, which can effectively improve the compatibility between the epoxy resin and the hollow glass microspheres; at the same time, a large number of hydroxyl groups are introduced on the surfaces of both, which can effectively form hydrogen bonds, and under the action of hydrogen bonds, the compatibility and adhesion between the two are further enhanced, thereby effectively improving the thermal insulation, adhesion, crack resistance and other properties of the thermal insulation coating;
[0036] 2. By adopting the above technical scheme, bisphenol A epoxy resin is modified by using hydroxyl-terminated polydimethylsiloxane. Under the action of a catalyst, the terminal hydroxyl polydimethylsiloxane reacts chemically with the epoxy resin functional group to generate Si-O segments in the epoxy resin chain structure, thereby enhancing the stability of the epoxy resin. There are no other atoms and groups around the oxygen atom of the Si-O bond, the bond angle and bond length are large, the distance between the adjacent non-bonded atoms thereon is larger than that of the Si-Si bond, and the internal rotation is easier than that of the CO chain. Therefore, the flexibility of the epoxy resin segment is increased, the bending strength is reduced, the device's ability to resist stress dispersion and impact is enhanced, and the anti-cracking performance of the epoxy resin is effectively increased;
[0037] 3. By adopting the above technical scheme, sodium hydroxide can be used to make the surface of the hollow glass microspheres rough and produce hydroxyl groups, and then the hydroxylated hollow glass microspheres are further modified by hydroxyl-terminated polydimethylsiloxane to obtain hollow glass microspheres containing a large number of Si-O segments and hydroxyl groups on the surface, which not only effectively improves the compatibility and adhesion of the hollow glass microspheres in the organic resin, but also further improves the comprehensive mechanical properties of the thermal insulation coating. DETAILED DESCRIPTION
[0038] The present application is further described in detail below with reference to the embodiments.
[0039] Preparation Example
[0040] Preparation Example 1 Preparation of hydroxyl-terminated silicone-modified epoxy resin
[0041] Preparation Example 1.1
[0042] S1. Weigh 5 g of hydroxyl-terminated polydimethylsiloxane, 40 g of bisphenol A epoxy resin, and 1.5 g of catalyst dibutyl tin dilaurate;
[0043] S2. After mixing the hydroxyl-terminated polydimethylsiloxane and bisphenol A epoxy resin, heat to 120°C at a stirring speed of 400 rpm and stir for 5 minutes; then add the catalyst dibutyltin dilaurate and react for 2 hours at a temperature of 120°C and a vacuum degree of -0.1 MPa. After cooling, obtain a hydroxyl-terminated silicone-modified epoxy resin.
[0044] Preparation Example 1.2
[0045] S1. Weigh 5 g of hydroxyl-terminated polydimethylsiloxane, 40 g of bisphenol A epoxy resin, and 1.5 g of catalyst dibutyl tin dilaurate;
[0046] S2. After mixing the hydroxyl-terminated polydimethylsiloxane and bisphenol A epoxy resin, heat to 145°C at a stirring speed of 450 rpm and stir for 10 minutes; then add the catalyst dibutyltin dilaurate and react for 3 hours at a temperature of 135°C and a vacuum degree of 0 MPa. After cooling, a hydroxyl-terminated silicone-modified epoxy resin is obtained.
[0047] Preparation Example 1.3
[0048] S1. Weigh 5 g of hydroxyl-terminated polydimethylsiloxane, 40 g of bisphenol A epoxy resin, and 1.5 g of catalyst dibutyl tin dilaurate;
[0049] S2. After mixing the hydroxyl-terminated polydimethylsiloxane and bisphenol A epoxy resin, heat to 150°C at a stirring speed of 500 rpm and stir for 15 minutes; then add the catalyst dibutyltin dilaurate and react at a temperature of 150°C and a vacuum degree of 0.1 MPa for 4 hours. After cooling, a hydroxyl-terminated silicone-modified epoxy resin is obtained.
[0050] Preparation Example 1.4
[0051] The difference between Preparation Example 1.4 and Preparation Example 1.1 is that 5 g of hydroxyl-terminated polydimethylsiloxane, 45 g of bisphenol A epoxy resin, and 2.5 g of catalyst dibutyltin dilaurate were weighed in Preparation Example 1.4.
[0052] Preparation Example 1.5
[0053] The difference between Preparation Example 1.5 and Preparation Example 1.1 is that 5 g of hydroxyl-terminated polydimethylsiloxane, 50 g of bisphenol A epoxy resin, and 3.5 g of catalyst dibutyltin dilaurate were weighed in Preparation Example 1.5.
[0054] Preparation Example 1.6
[0055] The difference between Preparation Example 1.6 and Preparation Example 1.1 is that 5 g of hydroxyl-terminated polydimethylsiloxane, 30 g of bisphenol A epoxy resin, and 0.5 g of catalyst dibutyltin dilaurate were weighed in Preparation Example 1.6.
[0056] Preparation Example 1.7
[0057] The difference between Preparation Example 1.7 and Preparation Example 1.1 is that 5 g of hydroxyl-terminated polydimethylsiloxane, 60 g of bisphenol A epoxy resin, and 4.5 g of catalyst dibutyltin dilaurate were weighed in Preparation Example 1.7.
[0058] Preparation Example 2 Preparation of hydroxyl-modified hollow glass microspheres
[0059] Preparation Example 2.1
[0060] S1. 8 g of hollow glass microspheres were added to 40 g of sodium hydroxide, stirred at a temperature of 25 ° C and a stirring speed of 600 rpm for 3 hours, and the hollow glass microspheres were taken out after filtration; the hollow glass microspheres were first acid-washed with a 1% mass fraction of acetic acid aqueous solution, and then washed with deionized water until the pH of the washing waste liquid reached 6, and the obtained hollow glass microspheres were vacuum dried at a temperature of 70 ° C for 8 hours to obtain pretreated hollow glass microspheres;
[0061] S2. 4 g of hydroxyl-terminated polydimethylsiloxane was added to 10 g of deionized water and 10 g of ethanol and stirred evenly, and the pH of the solution was adjusted to 4 with a 1% aqueous acetic acid solution to obtain a silicone solution;
[0062] S3. The pretreated hollow glass microspheres in S1 were added to the organosilicon solution in S2, and 0.5 g of the catalyst dibutyltin dilaurate was added, and the mixture was stirred at 25° C. and 300 rpm for 6 h; then vacuum dried at 60° C. for 15 h to obtain hydroxyl-modified hollow glass microspheres.
[0063] Preparation Example 2.2
[0064] S1. Add 12g of hollow glass microspheres to 50g of sodium hydroxide, stir for 6h at a temperature of 30°C and a stirring speed of 650rpm, and take out the hollow glass microspheres after filtering; firstly pickle the hollow glass microspheres with an acetic acid aqueous solution having a mass fraction of 1%, and then wash the hollow glass microspheres with deionized water until the pH of the washing waste liquid reaches 6.5, and vacuum dry the obtained hollow glass microspheres at a temperature of 75°C for 10h to obtain pretreated hollow glass microspheres;
[0065] S2. 6 g of hydroxyl-terminated polydimethylsiloxane was added to 15 g of deionized water and 15 g of ethanol and stirred evenly, and the pH of the solution was adjusted to 5 with a mass fraction of 1% acetic acid aqueous solution to obtain a silicone solution;
[0066] S3. The pretreated hollow glass microspheres in S1 were added to the organosilicon solution in S2, and 0.6 g of dibutyltin dilaurate as a catalyst was added, and the mixture was stirred at 30° C. and 350 rpm for 12 h; the mixture was then vacuum dried at 70° C. for 15 h to obtain hydroxyl-modified hollow glass microspheres.
[0067] Preparation Example 2.3
[0068] S1. Add 16g of hollow glass microspheres to 60g of sodium hydroxide, stir for 9h at a temperature of 35°C and a stirring speed of 700rpm, and take out the hollow glass microspheres after filtering; firstly pickle the hollow glass microspheres with a mass fraction of 1% acetic acid aqueous solution, and then wash the hollow glass microspheres with deionized water until the pH of the washing waste liquid reaches 7, and vacuum dry the obtained hollow glass microspheres at a temperature of 80°C for 12h to obtain pretreated hollow glass microspheres;
[0069] S2. 8 g of hydroxyl-terminated polydimethylsiloxane was added to 20 g of deionized water and 20 g of ethanol and stirred evenly, and the pH of the solution was adjusted to 6 with a mass fraction of 1% acetic acid aqueous solution to obtain a silicone solution;
[0070] S3. The pretreated hollow glass microspheres in S1 were added to the organosilicon solution in S2, and 0.7 g of dibutyltin dilaurate as a catalyst was added, and the mixture was stirred at 35° C. and 400 rpm for 18 h; the mixture was then vacuum dried at 80° C. for 15 h to obtain hydroxyl-modified hollow glass microspheres.
[0071] Preparation Example 2.4
[0072] The difference between Preparation Example 2.4 and Preparation Example 2.1 is that the hollow glass microspheres weighed in Preparation Example 2.4 are 8 g, and the mass of hydroxyl-terminated polydimethylsiloxane is 4.8 g.
[0073] Preparation Example 2.5
[0074] The difference between Preparation Example 2.5 and Preparation Example 2.1 is that the hollow glass microspheres weighed in Preparation Example 2.5 are 8 g, and the mass of hydroxyl-terminated polydimethylsiloxane is 5.6 g.
[0075] Preparation Example 2.6
[0076] The difference between Preparation Example 2.6 and Preparation Example 2.1 is that in Preparation Example 2.6, 8 g of hollow glass microspheres were weighed, and the mass of hydroxyl-terminated polydimethylsiloxane was 2.4 g.
[0077] Preparation Example 2.7
[0078] The difference between Preparation Example 2.7 and Preparation Example 2.1 is that in Preparation Example 2.7, 8 g of hollow glass microspheres were weighed, and the mass of hydroxyl-terminated polydimethylsiloxane was 7.2 g.
[0079] Preparation Example 2.8
[0080] The difference between Preparation Example 2.8 and Preparation Example 2.1 is that the vacuum drying time in S3 of Preparation Example 2.8 is 20 hours.
[0081] Preparation Example 2.9
[0082] The difference between Preparation Example 2.9 and Preparation Example 2.1 is that the vacuum drying time in S3 of Preparation Example 2.9 is 25 hours.
[0083] Preparation Example 2.10
[0084] The difference between Preparation Example 2.10 and Preparation Example 2.1 is that the vacuum drying time in S3 of Preparation Example 2.10 is 10 hours.
[0085] Preparation Example 2.11
[0086] The difference between Preparation Example 2.11 and Preparation Example 2.1 is that the vacuum drying time in S3 of Preparation Example 2.11 is 30 hours.
[0087] Example
[0088] Example 1
[0089] S1. At 40°C, 30 g of the hydroxyl-terminated silicone-modified epoxy resin obtained in Preparation Example 1.1, 5 g of calcium sulfate whiskers, 20 g of the hydroxyl-modified hollow glass microspheres obtained in Preparation Example 2.1, 10 g of sepiolite fiber, 3 g of dispersant, 30 g of ethanol, and 20 g of deionized water were stirred at a stirring speed of 1000 rpm for 45 min to obtain a mixture A;
[0090] S2. Add 3g of calcium hydroxide, 3g of nano-titanium dioxide and 1g of thickener to the mixture A and stir at a stirring speed of 600rpm for 30min to obtain a mixture B;
[0091] S3. At a stirring speed of 300 rpm, 1g of leveling agent, 1g of defoamer, 1g of multifunctional additive AMP-95 regulator, and 3g of curing agent were added to the mixture B in sequence, and stirring was continued for 1h to obtain a decorative panel with an insulating coating;
[0092] In this embodiment, the dispersant used is sodium dodecylbenzene sulfonate; the thickener used is hydroxymethyl cellulose; the leveling agent used is an organosilicon leveling agent; the defoaming agent used is BYK-025 organosilicon defoaming agent; and the curing agent used is triethylenetetramine.
[0093] Example 2
[0094] S1. At 50°C, 40g of the hydroxyl-terminated silicone-modified epoxy resin obtained in Preparation Example 1.1, 12g of calcium sulfate whiskers, 30g of the hydroxyl-modified hollow glass microspheres obtained in Preparation Example 2.1, 15g of sepiolite fiber, 4g of dispersant, 45g of ethanol, and 35g of deionized water were stirred at a stirring speed of 1250rpm for 40min to obtain a mixture A;
[0095] S2. 12 g of calcium hydroxide, 8 g of nano-titanium dioxide and 3 g of thickener were added to the mixture A and stirred at a stirring speed of 700 rpm for 25 min to obtain a mixture B;
[0096] S3. At a stirring speed of 350rpm, 2g of leveling agent, 2g of defoamer, 2g of multifunctional additive AMP-95 regulator, 4g of curing agent were added to the mixture B, and stirring was continued for 1.5h to obtain a decorative panel with an insulation coating;
[0097] In this embodiment, the dispersant used is sodium dodecylbenzene sulfonate; the thickener used is hydroxymethyl cellulose; the leveling agent used is an organosilicon leveling agent; the defoaming agent used is BYK-025 organosilicon defoaming agent; and the curing agent used is triethylenetetramine.
[0098] Example 3
[0099] S1. At 60°C, 50 g of the hydroxyl-terminated silicone-modified epoxy resin obtained in Preparation Example 1.1, 20 g of calcium sulfate whiskers, 40 g of the hydroxyl-modified hollow glass microspheres obtained in Preparation Example 2.1, 20 g of sepiolite fiber, 5 g of dispersant, 60 g of ethanol, and 50 g of deionized water were stirred at a stirring speed of 1500 rpm for 35 min to obtain a mixture A;
[0100] S2. Add 21g of calcium hydroxide, 13g of nano-titanium dioxide, and 5g of thickener to the mixture A, and stir at a stirring speed of 800rpm for 20min to obtain a mixture B;
[0101] S3. At a stirring speed of 400 rpm, 3g of leveling agent, 3g of defoamer, 3g of multifunctional additive AMP-95 regulator, 5g of curing agent were added to the mixture B, and stirring was continued for 2h to obtain a decorative panel with an insulating coating;
[0102] In this embodiment, the dispersant used is sodium dodecylbenzene sulfonate; the thickener used is hydroxymethyl cellulose; the leveling agent used is an organosilicon leveling agent; the defoaming agent used is BYK-025 organosilicon defoaming agent; and the curing agent used is triethylenetetramine.
[0103] Embodiment 4-9
[0104] The difference between Example 4-9 and Example 1 is that the hydroxyl-terminated silicone-modified epoxy resin used in Examples 4-9 comes from Preparation Examples 1.2 to 1.7.
[0105] Examples 10-19
[0106] The difference between Examples 10-19 and Example 1 is that the hydroxyl-modified hollow glass microspheres used in Examples 10-19 are from Preparation Examples 2.2 to 2.11.
[0107] Comparative Example
[0108] Comparative Example 1
[0109] The difference between Comparative Example 1 and Example 1 is that the resin used in Comparative Example 1 is unmodified bisphenol A epoxy resin with a mass of 30 g.
[0110] Comparative Example 2
[0111] The difference between Comparative Example 2 and Example 1 is that the hollow glass microspheres used in Comparative Example 2 are unmodified hollow glass microspheres with a mass of 20 g.
[0112] Performance testing
[0113] Clean and wet several calcium silicate boards; spray the thermal insulation coatings for decorative boards prepared in Examples 1-19 and Comparative Examples 1-2 on the wetted calcium silicate boards respectively, and perform curing after spraying for 10 hours at a temperature of 80°C to obtain decorative boards for testing.
[0114] 1. The prepared decorative panel for testing is placed on a heating table. The heating temperature of the heating table is set to 300°C. The dry film thickness of the thermal insulation coating is 9 mm. After heating for 30 minutes, the surface temperature of the thermal insulation coating is measured using a contact point thermometer to determine the heat resistance and thermal insulation performance of the coating. The results are shown in Table 1.
[0115] 2. The adhesion of the thermal insulation coatings for decorative panels obtained in Examples 1-19 and Comparative Examples 1-2 was tested using GB / T 9286-1998 “Scratch test for paints and varnishes”. The results are shown in Table 1.
[0116] 3. The aging resistance of the thermal insulation coatings for decorative panels obtained in Examples 1-19 and Comparative Examples 1-2 was tested using GB / T 1766-2008 “Rating Method for Aging of Paint and Varnish Coatings”. The results are shown in Table 1.
[0117] The specific test results are as follows:
[0118] Table 1 Performance test results
[0119]
[0120]
[0121] It can be seen from the test results of Examples 1-3 and Comparative Examples 1-2 that the decorative panel thermal insulation coating obtained in the present application has a surface temperature lower than 55°C after being heated at 300°C for 30 minutes, indicating that the thermal insulation coating provided in the present application has strong heat resistance and thermal insulation performance; the adhesion of the coating reaches level 1, indicating that the thermal insulation coating provided in the present application has strong adhesion; and it is not prone to bubbling, falling off, and cracking, and has strong aging resistance.
[0122] It can be seen from the test results of Examples 1, 4, 5 and Comparative Example 1 that the process parameters for preparing hydroxyl-terminated silicone-modified epoxy resins provided in the present application are beneficial to improving the thermal insulation performance, adhesion and aging resistance of the coating; when unmodified bisphenol A epoxy resin is used instead of hydroxyl-terminated silicone-modified epoxy resin, the thermal insulation performance, adhesion and aging resistance of the obtained thermal insulation coating are reduced.
[0123] It can be seen from the test results of Examples 1, 6, 7 and Examples 8, 9 that when the hydroxyl-terminated organosilicon-modified epoxy resin is prepared, the weight ratio of the hydroxyl-terminated polydimethylsiloxane, bisphenol A epoxy resin and catalyst is 1:
[0124] (8-10): When the weight ratio of the three is lower than or higher than this ratio, the obtained hydroxyl-terminated silicone-modified epoxy resin is used in thermal insulation coatings, resulting in reduced thermal insulation performance and adhesion, and local cracking.
[0125] It can be seen from the test results of Examples 1, 10, 11 and Comparative Example 2 that the process parameters for preparing hydroxyl-modified hollow glass microspheres provided in the present application are beneficial to improving the thermal insulation performance, adhesion and aging resistance of the coating; when unmodified hollow glass microspheres are used instead of hydroxyl-modified hollow glass microspheres, the thermal insulation performance, adhesion and aging resistance of the obtained thermal insulation coating are reduced.
[0126] It can be seen from the test results of Examples 1, 12, 13 and Examples 14, 15 that when the mass ratio of hollow glass microspheres used to prepare hydroxyl-modified hollow glass microspheres to hydroxyl-terminated polydimethylsiloxane is in the range of 1: (0.5-0.7), the prepared hydroxyl-modified hollow glass microspheres are beneficial to improving the thermal insulation performance, adhesion and aging resistance of the coating; when the weight ratio of the two is lower than or exceeds this ratio, the obtained hydroxyl-modified hollow glass microspheres are used in the thermal insulation coating, resulting in a decrease in thermal insulation performance and adhesion, and local cracking or falling off.
[0127] It can be seen from the test results of Examples 1, 16, 17 and Examples 18, 19 that when the vacuum drying reaction time used in S3 for preparing hydroxyl-modified hollow glass microspheres in the present application is within 15-25 hours, it is beneficial to improve the thermal insulation performance, adhesion and aging resistance of the coating. However, when it is less than 15 hours or more than 25 hours, the obtained hydroxyl-modified hollow glass microspheres are used in the thermal insulation coating, resulting in a decrease in thermal insulation performance and adhesion, and local cracking or falling off.
[0128] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A thermal insulation coating for decorative panels, characterized in that: The raw materials include, by weight: 30-50 parts of hydroxyl-terminated silicone modified epoxy resin, 5-20 parts of calcium sulfate whiskers, 20-40 parts of hydroxyl-modified hollow glass microspheres, 10-20 parts of sepiolite fibers, 3-21 parts of calcium hydroxide, 3-13 parts of nano titanium dioxide, 1-5 parts of thickeners, 1-3 parts of leveling agents, 1-3 parts of defoamers, 3-5 parts of dispersants, 1-3 parts of multifunctional additives, 3-5 parts of curing agents, 30-60 parts of ethanol, and 20-50 parts of deionized water; The hydroxyl-terminated organosilicon-modified epoxy resin is composed of the following components: hydroxyl-terminated polydimethylsiloxane, bisphenol A epoxy resin, and catalyst, and the weight ratio of the three is 1: (8-10): (0.3-0.7); The hydroxyl-modified hollow glass microspheres are composed of the following components in parts by weight: 8-16 parts of hollow glass microspheres, 40-60 parts of sodium hydroxide, 4-8 parts of hydroxyl-terminated polydimethylsiloxane, 0.5-0.7 parts of a catalyst, 10-20 parts of deionized water, and 10-20 parts of ethanol; The method for preparing the thermal insulation coating for the decorative plate comprises the following steps: S1. At 40-60°C, 30-50 parts by weight of hydroxyl-terminated silicone-modified epoxy resin, 5-20 parts of calcium sulfate whiskers, 20-40 parts of hydroxyl-modified hollow glass microspheres, 10-20 parts of sepiolite fibers, 3-5 parts of dispersant, 30-60 parts of ethanol, and 20-50 parts of deionized water are stirred at a stirring speed of 1000-1500 rpm to obtain a mixture A; S2. Add 3-21 parts of calcium hydroxide, 3-13 parts of nano titanium dioxide, and 1-5 parts of thickener to the mixture A, and stir at a stirring speed of 600-800rpm to obtain a mixture B; S3. At a stirring speed of 300-400 rpm, add 1-3 parts of leveling agent, 1-3 parts of defoaming agent, 1-3 parts of multifunctional additive, and 3-5 parts of curing agent to mixed material B in sequence, mix well, and obtain a thermal insulation coating for decorative panels.
2. The thermal insulation coating for decorative panels according to claim 1, characterized in that: The mass ratio of the hollow glass microspheres to the hydroxyl-terminated polydimethylsiloxane is 1:(0.5-0.7).
3. The thermal insulation coating for decorative panels according to claim 1, characterized in that: The catalyst is dibutyltin dilaurate.
4. The thermal insulation coating for decorative panels according to claim 1, characterized in that: The multifunctional auxiliary agent is AMP-95 regulator.
5. The method for preparing a thermal insulation coating for a decorative plate according to claim 1, characterized in that: The preparation method of the hydroxyl-terminated silicone-modified epoxy resin comprises the following steps: S1. Weigh hydroxyl-terminated polydimethylsiloxane, bisphenol A epoxy resin, and catalyst in a weight ratio of 1: (8-10): (0.3-0.7); S2. After mixing the hydroxyl-terminated polydimethylsiloxane and bisphenol A epoxy resin, heat to 120-150°C and stir for 5-15 minutes; then add the catalyst and react at a temperature of 120-150°C and a vacuum degree of -0.1-0.1MPa for 2-4 hours, and obtain a hydroxyl-terminated silicone-modified epoxy resin after cooling.
6. The method for preparing a thermal insulation coating for a decorative plate according to claim 1, characterized in that: The preparation method of the hydroxyl-modified hollow glass microspheres comprises the following steps: S1. Add 8-16 parts of hollow glass microspheres to 40-60 parts of sodium hydroxide by weight, stir for 3-9h, and filter out the hollow glass microspheres; first pickle the hollow glass microspheres, then wash the hollow glass microspheres with water until the pH of the washing waste liquid reaches 6-7, and vacuum dry the obtained hollow glass microspheres to obtain pretreated hollow glass microspheres; S2. Add 4-8 parts of hydroxyl-terminated polydimethylsiloxane to 10-20 parts of deionized water and 10-20 parts of ethanol, stir evenly, and adjust the pH of the solution to 4-6; obtain an organosilicon solution; S3. Add the pretreated hollow glass microspheres in S1 to the organosilicon solution in S2, add 0.5-0.7 parts of catalyst, stir for 6-18 hours, and then perform vacuum drying reaction at 60-80° C. to obtain hydroxyl-modified hollow glass microspheres.
7. The method for preparing a thermal insulation coating for a decorative plate according to claim 6, characterized in that: The vacuum drying reaction time in S3 is 15-25 hours.