Preparation methods and applications of atomically dispersed monolayer phthalocyanine iron-based catalysts for electrochemical ammonia synthesis
By employing a two-stage high-temperature calcination method involving an ionic liquid mixture and ferrophthalocyanine, a monolayer dispersion and pore structure of ferrophthalocyanine catalyst were achieved, improving the ammonia yield and Faraday efficiency in the electrochemical synthesis of ammonia. This solved the problem of low efficiency in existing catalysts and enabled the efficient nitrogen reduction preparation of ammonia.
Patent Information
- Application Number
- CN202310824399.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-06
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-07-06
AI Technical Summary
Existing supported iron phthalocyanine catalysts exhibit low ammonia yield and Faraday efficiency in the electrochemical synthesis of ammonia, making it difficult to achieve efficient NRR reactions.
A two-stage high-temperature calcination method using an ionic liquid mixture and ferrophthalocyanine was adopted. The monolayer dispersion of ferrophthalocyanine was achieved through ultrasonic treatment and stirring. The ionic liquid was used as a carbon source to form a rich pore structure, fix the ferrophthalocyanine molecules, form Fe-N coordination, and improve the activity of the catalyst.
A highly efficient nitrogen reduction method for ammonia production was achieved at room temperature and pressure, exhibiting high ammonia yield and Faraday efficiency, and excellent catalytic performance.
Smart Images

Figure HDA0004324571580000011 
Figure HDA0004324571580000012 
Figure HDA0004324571580000013
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing a single-layer phthalocyanine iron-based catalyst and its application in the electrochemical synthesis of ammonia. Background Technology
[0002] Ammonia is a very important chemical widely used in agriculture, pharmaceuticals, and other industries. Furthermore, its high hydrogen content and easy liquefaction make it a promising green energy source. Currently, the main industrial method for ammonia production is the Haber-Bosch process, which converts nitrogen and hydrogen into ammonia under high temperature and pressure using an iron-based catalyst. This process consumes a large amount of energy and fossil fuels, approximately 1-2% of global energy supply and 5% of global natural gas production annually, causing significant pollution. Therefore, finding a green and sustainable ammonia synthesis technology is a pressing task.
[0003] Electrochemical ammonia synthesis uses abundant N2 from the air and widely available H2O from nature as raw materials. Ammonia is synthesized mildly under the action of a catalyst. The required electricity is renewable, coming from wind, solar, and tidal energy sources, thus avoiding the large-scale consumption of fossil fuels and greenhouse gas emissions, making it an environmentally friendly ammonia synthesis technology. The catalyst is the core of electrochemical ammonia synthesis; therefore, synthesizing inexpensive and high-performance electrocatalysts is crucial. Iron (Fe) is abundant in the Earth's crust, inexpensive, and its activation ability for N2 is comparable to that of the precious metal Ru. Therefore, iron-based catalysts have wide applications in biological and chemical nitrogen fixation. Iron phthalocyanine (FePC), with its metal-nitrogen-caborn (M-NC) structure, exhibits highly efficient catalytic effects in electrochemical ammonia synthesis. Immobilizing the large FePC active centers on a support is a key factor in achieving efficient NRR reactions. Direct grafting of Fe onto the support through coordination or intermolecular π-π interactions are two commonly used methods. However, the existing supported phthalocyanine iron catalysts (Xu, Su Xian, Ding, Yun Xuan, Du, Jian, ACS catalysis, 2022, 12(9): 5502-5509; Xu, Fan Fan, Zhang, Lin Lin, Ding, Xin, Chemical communications, 2019, 55(94): 14111-14114) have problems with low ammonia yield or Faraday efficiency. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis and its application in electrochemical ammonia synthesis. Under the action of this catalyst, both high ammonia yield and high Faraday efficiency are achieved.
[0005] The technical solution adopted in this invention is:
[0006] In a first aspect, the present invention provides a method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, comprising the following steps:
[0007] Step 1: Mix the chloride salt ionic liquid and the bis(trifluoromethanesulfonyl)imide salt ionic liquid, and stir thoroughly at a certain temperature to make them evenly mixed, thus obtaining an ionic liquid mixture;
[0008] Step 2: Weigh a certain amount of FePC (ferrophthalocyanine) and add it to the above ionic liquid mixture. After ultrasonic treatment for 10-60 min, stir the mixture vigorously at 0-30℃ for 0.5-3 h to obtain a mixed sample. The mass percentage content of ferrophthalocyanine in the mixed sample is 0.9%-3.6%.
[0009] Step 3: Place the mixed sample obtained in Step 2 into an inert gas environment for high-temperature calcination to complete the carbonization and pore formation of the ionic liquid. The calcination is divided into two stages. The first stage of calcination carbonizes the ionic liquid, with the calcination temperature controlled at 300-700℃ and the calcination time controlled at 2-10h. The second stage of calcination forms a rich pore structure, with the calcination temperature controlled at 500-900℃ and the calcination time controlled at 2-8h.
[0010] Furthermore, in step one, the chloride ionic liquid is selected from at least one of 1-octylimidazolium chloride, 1-decylimidazolium chloride, 1-dodecylimidazolium chloride, 1,3-diisopropylimidazolium chloride, 1-butyl-3-methylimidazolium chloride, 2-chloro-1,3-dimethylimidazolium chloride, 1-benzyl-3-methylimidazolium chloride, 1-benzyl-2,3-dimethylimidazolium chloride, 1-vinyl-3-methylimidazolium chloride, and 1-allyl-3-methylimidazolium chloride.
[0011] Furthermore, in step one, the bis(trifluoromethanesulfonyl)imide salt ionic liquid is selected from at least one of 1-benzyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-benzyl-2,3-dimethylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, and 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt.
[0012] Furthermore, in step one, the mass ratio of chloride ionic liquid and bis(trifluoromethanesulfonyl)imide ionic liquid is controlled at 1:1 to 1:10.
[0013] Furthermore, in step one, the chloride ionic liquid is 1-butyl-3-methylimidazolium chloride or 1-benzyl-2,3-dimethylimidazolium chloride, and the bis(trifluoromethanesulfonyl)imide salt ionic liquid is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt or 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt; the mass ratio of the chloride ionic liquid to the bis(trifluoromethanesulfonyl)imide salt ionic liquid is controlled at 1:1.5-1:5, and most preferably, the chloride ionic liquid is 1-butyl-3-methylimidazolium chloride, the bis(trifluoromethanesulfonyl)imide salt ionic liquid is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, and the mass ratio of the chloride ionic liquid to the bis(trifluoromethanesulfonyl)imide salt ionic liquid is 1:5.
[0014] Furthermore, in step one, the stirring temperature is controlled at 30-70℃.
[0015] Furthermore, in step two, the mass percentage content of iron phthalocyanine in the mixed sample is 2.2-3.0%, more preferably 2.6-3.0%.
[0016] Furthermore, in step two, the stirring speed is controlled at 300-500 rpm. Even further, in step two, the stirring temperature is 0℃, the stirring rate is 300 rpm, and the stirring time is 24 hours.
[0017] Furthermore, in step three, the inert gas is selected from nitrogen, argon, and helium.
[0018] Furthermore, in step three, the calcination temperature of the first stage is controlled at 500-600℃, preferably 500℃, and the calcination time is 2-3 hours; the calcination temperature of the second stage is controlled at 700-800℃, preferably 700℃, and the calcination time is 2-3 hours; most preferably, the calcination temperature of the first stage is controlled at 500℃ and the calcination time is controlled at 2 hours; the calcination temperature of the second stage is controlled at 700℃ and the calcination time is controlled at 3 hours.
[0019] Secondly, the present invention provides the application of the atomically dispersed monolayer phthalocyanine iron-based catalyst prepared according to the above preparation method in the electrochemical synthesis of ammonia. The specific application is as follows: the atomically dispersed monolayer phthalocyanine iron-based catalyst is fully dispersed in an ethanol solvent, and then a 5% (w / w) Nafion solution is added. After being fully dispersed and uniformly dispersed, a dispersion is obtained. The dispersion is uniformly coated onto an electrode material, and the electrode material coated with the atomically dispersed monolayer phthalocyanine iron-based catalyst is used as the working electrode to carry out the electrochemical synthesis of ammonia.
[0020] Furthermore, the feed ratio of the atomically dispersed monolayer phthalocyanine iron-based catalyst to 5% Nafion solution and ethanol is 1-10 mg: 20-100 μL: 0.9 mL, preferably 1 mg: 50 μL: 0.9 mL.
[0021] Furthermore, the electrode material is carbon paper.
[0022] Furthermore, the coating amount of the dispersion is 40–200 μL / cm². 2 Preferably 100 μL / cm 2 .
[0023] Compared with the prior art, the advantages of the present invention are mainly reflected in:
[0024] (1) In the preparation method of the atomically dispersed monolayer phthalocyanine iron-based catalyst of the present invention, the oxidizing property of the ionic liquid is utilized with the aid of ultrasound to fully peel off the stacked phthalocyanine iron molecules, thereby achieving monolayer dispersion of phthalocyanine iron molecules in the ionic liquid; the carbonized ionic liquid is used as the framework of the carrier to fix the phthalocyanine iron molecules through a two-stage calcination method, and the phthalocyanine iron is fixed by carbon-carbon bonds, thereby achieving high dispersion and high stability of the monolayer active center of the phthalocyanine iron catalyst; the ionic liquid is used as the carbon source in the present invention, which can form a rich pore structure during calcination, which is beneficial to the adsorption of N2; the self-assembly of phthalocyanine metal compounds in the present invention forms Fe-N coordination, thereby improving the activity of the catalyst; at the same time, the monolayer dispersion of phthalocyanine iron has an inhibitory effect on HER.
[0025] (2) The catalyst of the present invention has excellent catalytic and electrochemical performance for the reduction of nitrogen to prepare ammonia at room temperature and pressure. The nitrogen reduction to prepare ammonia reaction under the action of the catalyst has both high ammonia yield and high Faraday efficiency, and has great application prospects. Attached Figure Description
[0026] Figure 1 The following are specific embodiments and comparative examples of the ammonia detection standard curve using a UV-Vis spectrophotometer.
[0027] Figure 2 This is a SEM image of an atomically dispersed monolayer phthalocyanine iron-based catalyst, as shown in Example 1 of the present invention.
[0028] Figure 3 This is a TEM image of an atomically dispersed monolayer phthalocyanine iron-based catalyst, as shown in Example 1 of the present invention.
[0029] Figure 4 The image shown is a HAADF-TEM image of an atomically dispersed monolayer phthalocyanine iron-based catalyst from a specific embodiment of the present invention, 1.
[0030] Figure 5 This is a bilayer capacitance diagram of an atomically dispersed monolayer phthalocyanine iron-based catalyst, as shown in Embodiment 1 of the present invention.
[0031] Figure 6The diagram shows the electrochemical ammonia synthesis performance of an atomically dispersed monolayer phthalocyanine iron-based catalyst, as described in Example 1 of the present invention.
[0032] Figure 7 This is a stability diagram of electrochemical ammonia synthesis using an atomically dispersed monolayer phthalocyanine iron-based catalyst, as shown in Example 1 of the present invention.
[0033] Figure 8 The XRD patterns are of the atomically dispersed monolayer phthalocyanine iron-based catalysts obtained in specific embodiments 1, 5, 6, comparative examples 1 and 4 of the present invention. Detailed Implementation
[0034] The present invention will be illustrated below with specific embodiments. It should be noted that the embodiments are only for further illustration of the present invention and should not be construed as limiting the scope of protection of the present invention, which is not limited thereto in any way. Those skilled in the art can make some non-essential improvements and adjustments based on the above description of the invention.
[0035] In this embodiment, the performance test of nitrogen reduction to ammonia preparation using an atomically dispersed monolayer phthalocyanine iron-based catalyst was performed on a CHI760 electrochemical workstation. The procedure was as follows: First, approximately 2 mg of sample was weighed and dispersed in 0.9 mL of ethanol, then 100 μL of Nafion solution (5 wt%) (DuPont D520) was added, and the mixture was sonicated for 30 min to obtain a uniform dispersion. Then, 100 μL of the dispersion was coated onto carbon paper (1*1 cm). 2 The second step involves using carbon paper loaded with catalyst as the working electrode to conduct an experiment on nitrogen reduction to prepare ammonia.
[0036] Before testing, nitrogen gas was purged into the solution for 30 minutes to saturate it. Linear sweep cyclic voltammetry and chronoamperometry were selected as the testing procedures, and the current at the working electrode at different potentials was monitored using a computer. Then, a standard curve (see [reference]) was used with a UV-Vis spectrophotometer. Figure 1 The concentration of ammonia in the electrolyte after catalysis was tested, and finally the ammonia production rate and Faraday efficiency of the catalyst were calculated.
[0037] Example 1
[0038] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0039] 1) Weigh 50g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-butyl-3-methylimidazolium chloride, and stir at 50℃ for 30min.
[0040] 2) Weigh 1.7g of phthalocyanine iron, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0041] 3) The above mixed sample was placed in a tube furnace and heated at 500°C for 2 hours in a N2 environment, and then heated at 700°C for 3 hours to obtain an atomically dispersed monolayer phthalocyanine iron-based catalyst.
[0042] 4) In this embodiment, the performance test of nitrogen reduction to ammonia preparation using an atomically dispersed monolayer phthalocyanine iron-based catalyst was conducted on a CHI760 electrochemical workstation. The operation procedure was as follows:
[0043] Weigh approximately 2 mg of sample and disperse it in 0.9 mL of ethanol. Then add 100 μL of Nafion solution (5 wt%) and sonicate for 30 min to obtain a uniform dispersion. Then take 100 μL of the dispersion and coat it onto carbon paper (1*1 cm). 2 The catalyst was dried using infrared lamp irradiation. Then, carbon paper containing an atomically dispersed monolayer of phthalocyanine-iron-based catalyst was used as the working electrode, a platinum sheet as the counter electrode, and an Ag / AgCl reference electrode (saturated potassium chloride) as the reference electrode. 0.1M HCl was used as the electrolyte for the nitrogen reduction to ammonia experiment. Before testing, nitrogen gas was bubbled through the solution for 30 minutes to saturate it. Linear sweep cyclic voltammetry and chronoamperometry were used as the testing procedures, and the current at different potentials of the working electrode was monitored by computer. The results were then obtained using a UV-Vis spectrophotometer with a standard curve (see [reference]). Figure 1 The concentration of ammonia in the electrolyte after catalysis was tested, and finally the ammonia production rate and Faraday efficiency of the catalyst were calculated.
[0044] See the SEM image of the atomically dispersed monolayer phthalocyanine iron-based catalyst obtained. Figure 2 TEM images of the atomically dispersed monolayer phthalocyanine iron-based catalyst obtained are shown below. Figure 3 See the HAADF-TEM image of the atomically dispersed monolayer phthalocyanine iron-based catalyst obtained. Figure 4 The double-layer capacitance diagram of the atomically dispersed monolayer phthalocyanine iron-based catalyst is shown in [reference needed]. Figure 5 The electrochemical ammonia synthesis performance of the atomically dispersed monolayer phthalocyanine iron-based catalyst is shown in the figure. Figure 6 The stability diagram of the obtained atomically dispersed monolayer phthalocyanine iron-based catalyst is shown in [reference needed]. Figure 7 .
[0045] SEM images show that the atomically dispersed monolayer phthalocyanine iron-based catalyst exhibits nanoclusters with a good specific surface area. TEM and HAADF-TEM images reveal that Fe is distributed as single atoms, while phthalocyanine iron is dispersed in a monolayer. This atomically dispersed monolayer phthalocyanine iron-based catalyst achieves high dispersion of active centers, contributing to improved activity. The double-layer capacitance curve indicates a high active specific surface area. UV-Vis spectroscopy calculations show that the catalyst achieves an ammonia production rate of 23.23 μg / h under acidic conditions (-0.1 V). -1 mg -1 cat. The efficiency of Faraday's algorithm is 29.54%.
[0046] Example 2
[0047] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0048] 1) Weigh 50g of 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-benzyl-2,3-dimethylimidazolium chloride, and stir at 70℃ for 30min.
[0049] 2) Weigh 0.54g of ferrophthalocyanine, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0050] 3) The above mixed sample was placed in a tube furnace and heated at 500°C for 2 hours in a N2 environment, and then heated at 700°C for 3 hours to obtain an atomically dispersed monolayer phthalocyanine iron-based catalyst.
[0051] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the catalyst achieved an ammonia production rate of 15.63 μg / h under acidic conditions (-0.1V). -1 mg -1 cat. The efficiency of Faraday's algorithm is 20.14%.
[0052] Example 3
[0053] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0054] 1) Weigh 30g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 20g of 1-butyl-3-methylimidazolium chloride, and stir at 50℃ for 30min.
[0055] 2) Weigh 1.14g of ferrophthalocyanine, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0056] 3) The above mixed sample was placed in a tube furnace and heated at 300°C for 2 hours in a N2 environment, and then heated at 700°C for 3 hours to obtain an atomically dispersed monolayer phthalocyanine iron-based catalyst.
[0057] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the catalyst achieved an ammonia production rate of 21.06 μg / h under acidic conditions (-0.1V). -1 mg -1 cat. The efficiency of Faraday is 21.25%.
[0058] Example 4
[0059] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0060] 1) Weigh 50g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-butyl-3-methylimidazolium chloride, and stir at 50℃ for 30min.
[0061] 2) Weigh 0.24g of ferrophthalocyanine, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0062] 3) The above mixed sample was placed in a tube furnace and heated at 600°C for 2 hours in a N2 environment, and then heated at 700°C for 3 hours to obtain an atomically dispersed monolayer phthalocyanine iron-based catalyst.
[0063] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the catalyst achieved an ammonia production rate of 7.25 μg / h under acidic conditions (-0.1V). -1 mg -1 cat. The efficiency of Faraday's algorithm is 6.25%.
[0064] Example 5
[0065] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0066] 1) Weigh 50g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-butyl-3-methylimidazolium chloride, and stir at 50℃ for 30min.
[0067] 2) Weigh 1.7g of phthalocyanine iron, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0068] 3) The above mixed sample was placed in a tube furnace and heated at 450°C for 2 hours in a N2 environment, and then heated at 400°C for 3 hours to obtain an atomically dispersed monolayer phthalocyanine iron-based catalyst.
[0069] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the catalyst achieved an ammonia production rate of 9.16 μg / h under acidic conditions (-0.1V). -1 mg -1 cat The efficiency of Faraday is 25.61%.
[0070] Example 6
[0071] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0072] 1) Weigh 50g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-butyl-3-methylimidazolium chloride, and stir at 50℃ for 30min.
[0073] 2) Weigh 1.7g of phthalocyanine iron, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0074] 3) The above mixed sample was placed in a tube furnace and heated at 500°C for 2 hours in a N2 environment, and then heated at 500°C for 3 hours to obtain an atomically dispersed monolayer phthalocyanine iron-based catalyst.
[0075] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the catalyst achieved an ammonia production rate of 18.67 μg / h under acidic conditions (-0.1V). -1 mg -1 cat. The efficiency of Faraday is 21.74%.
[0076] Comparative Example 1
[0077] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0078] 1) Weigh 50g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-butyl-3-methylimidazolium chloride, and stir at 50℃ for 30min.
[0079] 2) Weigh 0g of phthalocyanine iron, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0080] 3) Place the above mixed sample into a tube furnace and heat it at 500°C for 2 hours in a N2 environment, and then heat it at 700°C for 3 hours.
[0081] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the catalyst achieved an ammonia production rate of 3.23 μg / h under acidic conditions (-0.1V). -1 mg -1 cat. The Faraday efficiency is 1.26%, indicating that the pure support has almost no activity, and Fe is the active center.
[0082] Comparative Example 2
[0083] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0084] 1) Weigh 50g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-butyl-3-methylimidazolium chloride, and stir at 50℃ for 30min.
[0085] 2) Weigh 1.7g of phthalocyanine iron, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0086] 3) Place the above mixed sample into a tube furnace and heat it at 500°C for 2 hours in a N2 environment.
[0087] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the catalyst achieved an ammonia production rate of 12.23 μg / h under acidic conditions (-0.1V). -1 mg -1 cat. The Faraday efficiency was 14.28%. This indicates that secondary calcination in a nitrogen atmosphere helps to create pores in the catalyst, which is beneficial to improving catalyst activity.
[0088] Comparative Example 3
[0089] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0090] 1) Weigh 50g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-butyl-3-methylimidazolium chloride, and stir at 30℃ for 30min.
[0091] 2) Weigh 2.26g of ferrophthalocyanine, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0092] 3) Place the above mixed sample into a tube furnace and heat it at 500°C for 2 hours in a N2 environment, and then heat it at 700°C for 3 hours.
[0093] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the ammonia production rate of this catalyst under acidic conditions (-0.1V) reached 23.01 μg / h. -1 mg -1 cat. The Faraday efficiency was 22.41%. This indicates that high loading leads to iron phthalocyanine stacking, which enhances HER activity and reduces Faraday efficiency.
[0094] Comparative Example 4
[0095] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0096] 1) Weigh 50g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-butyl-3-methylimidazolium chloride, and stir at 50℃ for 30min.
[0097] 2) Weigh 1.7g of phthalocyanine iron, add it to the above solution, sonicate for 20min, and then stir the mixture vigorously at 300rpm for 24h at 0℃.
[0098] 3) Place the above mixed sample into a tube furnace and heat it at 500°C for 2 hours in a N2 environment, and then heat it at 900°C for 3 hours.
[0099] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the catalyst achieved an ammonia production rate of 20.48 μg / h under acidic conditions (-0.1V). -1 mg -1 cat. The Faraday efficiency was 25.92%. This indicates that excessively high temperature pore formation leads to phthalocyanine iron stacking, reducing catalyst activity and Faraday efficiency.
[0100] Comparative Example 5
[0101] A method for preparing an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis, the method comprising the following steps:
[0102] 1) Weigh 50g of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 10g of 1-butyl-3-methylimidazolium chloride, and stir at 50℃ for 30min.
[0103] 2) Weigh 1.7g of ferrophthalocyanine, add it to the above solution, and stir the mixture vigorously at 300rpm for 24h at 0℃.
[0104] 3) Place the above mixed sample into a tube furnace and heat it at 500°C for 2 hours in a N2 environment, and then heat it at 700°C for 3 hours.
[0105] 4) The catalyst performance testing method is the same as in Example 1. Calculations using UV-Vis spectroscopy showed that the catalyst achieved an ammonia production rate of 20.56 μg / h under acidic conditions (-0.1V). -1 mg -1 cat. The Faraday efficiency was 24.86%. This indicates that the iron phthalocyanine that was not ultrasonically exfoliated exhibited stacking, affecting both catalyst activity and Faraday efficiency.
Claims
1. A method for the preparation of an atomically dispersed monolayer iron phthalocyanine based catalyst for the electrochemical synthesis of ammonia, characterized by: The preparation method includes the following steps: Step 1: Mix the chloride ionic liquid and the bis(trifluoromethanesulfonyl)imide ionic liquid, and stir thoroughly at a certain temperature to obtain a homogeneous ionic liquid mixture; the chloride ionic liquid is 1-butyl-3-methylimidazolium chloride or 1-benzyl-2,3-dimethylimidazolium chloride, and the bis(trifluoromethanesulfonyl)imide ionic liquid is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide or 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide; the mass ratio of the chloride ionic liquid to the bis(trifluoromethanesulfonyl)imide ionic liquid is controlled at 1:1.5-1:5; Step 2: Weigh a certain amount of phthalocyanine iron and add it to the above ionic liquid mixture. After ultrasonic treatment for 10-60 min, stir the mixture vigorously at 0-30℃ for 0.5-3 h to obtain a mixed sample. The mass percentage content of phthalocyanine iron in the mixed sample is 0.9%-3.6%. Step 3: The mixed sample obtained in Step 2 is placed in an inert gas environment and calcined at high temperature to complete the carbonization and pore formation of the ionic liquid, thereby obtaining an atomically dispersed monolayer phthalocyanine iron-based catalyst for electrochemical ammonia synthesis. The calcination is divided into two stages. The first stage of calcination carbonizes the ionic liquid, with the calcination temperature controlled at 300-700℃ and the calcination time controlled at 2-10 h. The second stage of calcination forms a rich pore structure, with the calcination temperature controlled at 500-900℃ and the calcination time controlled at 2-8 h.
2. The production method according to claim 1, characterized by: In step one, the chloride ionic liquid is 1-butyl-3-methylimidazolium chloride, the bis(trifluoromethanesulfonyl)imide ionic liquid is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, and the mass ratio of the chloride ionic liquid to the bis(trifluoromethanesulfonyl)imide ionic liquid is 1:
5.
3. The production method according to claim 1 or 2, characterized by: In step two, the mass percentage content of iron phthalocyanine in the mixed sample is 2.2-3.0%.
4. The production method according to claim 3, characterized by: In step two, the mass percentage content of iron phthalocyanine in the mixed sample is 2.6-3.0%.
5. The preparation method according to claim 1 or 2, characterized in that: In step three, the calcination temperature of the first stage is controlled at 500-600℃, and the calcination time is 2-3 hours; the calcination temperature of the second stage is controlled at 700-800℃, and the calcination time is 2-3 hours.
6. The preparation method according to claim 5, characterized in that: The calcination temperature for the first stage is controlled at 500 ℃, and the calcination time is controlled at 2 h; the calcination temperature for the second stage is controlled at 700 ℃, and the calcination time is controlled at 3 h.
7. The application of the atomically dispersed monolayer phthalocyanine iron-based catalyst prepared by the method according to claim 1 or 2 in the electrochemical synthesis of ammonia, wherein the application specifically comprises: fully dispersing the atomically dispersed monolayer phthalocyanine iron-based catalyst in an ethanol solvent, then adding a 5% (w / w) Nafion solution, and after fully dispersing and homogenizing to obtain a dispersion, uniformly coating the dispersion onto an electrode material, and using the electrode material coated with the atomically dispersed monolayer phthalocyanine iron-based catalyst as the working electrode to carry out the electrochemical synthesis of ammonia.
8. The application as described in claim 7, characterized in that: The atomic dispersed monolayer phthalocyanine iron-based catalyst and the mass fraction 5% nafion solution, ethanol feeding ratio is 1~10 mg:20~100 μL:0.9 mL, the electrode material is carbon paper, the dispersion coating amount is 40~200 μL / cm 2 .