A halogen-free flame-retardant high-temperature polyamide composition and its preparation method and application

By using a combination adsorbent of molecular sieve and sepiolite in halogen-free flame retardant high-temperature polyamide, the precipitation and corrosion problems during high-temperature processing are solved, the phosphorus content and corrosiveness are significantly reduced, the mechanical properties of the material are maintained, and the mechanical properties of the material are solved. The safety hazards of halogen-free flame-retardant high-temperature nylon under humid and heat conditions.

CN116694068BActive Publication Date: 2024-11-19ZHUHAI WANTONG SPECIAL ENG PLASTICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310478622.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-19
Estimated Expiration
2043-04-28

Smart Images

  • Figure BDA0004206319060000021
    Figure BDA0004206319060000021
  • Figure BDA0004206319060000071
    Figure BDA0004206319060000071
  • Figure BDA0004206319060000072
    Figure BDA0004206319060000072
Patent Text Reader

Abstract

The present invention discloses a halogen-free flame-retardant high-temperature polyamide composition, a preparation method thereof and an application thereof. The halogen-free flame-retardant high-temperature polyamide composition comprises the following components by weight: 35-68 parts of semi-aromatic polyamide; 10-20 parts of halogen-free flame retardant; 15-50 parts of reinforcing filler; 1-3 parts of sepiolite; and 1-3 parts of molecular sieve. The halogen-free flame-retardant high-temperature polyamide composition provided by the present invention can exhibit low precipitation and low metal corrosion under high temperature and high humidity conditions, and is suitable for the field of new energy vehicles with high precipitation resistance and corrosion resistance requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of engineering plastics, and in particular to a halogen-free flame-retardant high-temperature polyamide composition and a preparation method and application thereof. Background Art

[0002] At present, new energy vehicles are developing rapidly. Extended-range and hybrid vehicles are gradually withdrawing from the historical platform. In order to solve energy anxiety, pure electric new energy vehicles have begun to move towards fast charging. Fast charging has put forward higher requirements for voltage and current. At present, the voltage is moving towards 800V, and the current has begun to gradually move from 180A to 360A and 420A. Under the above current and voltage conditions, the temperature rise is obvious when the power is turned on, which will heat the parts to 150-180℃. High-temperature nylon has become the preferred insulating plastic material for customers. Due to the ultra-high voltage value and the potential electrolyte contamination risk commonly existing in new energy vehicles, the hard requirement of CTI≥600V is required, so halogen-free flame-retardant high-temperature nylon must be selected.

[0003] Halogen-free flame-retardant high-temperature nylon cannot use flame retardant synergists such as ammonium polyphosphate due to the high processing temperature (330-350℃). Therefore, the flame retardancy can only be improved by increasing the dosage of diethyl aluminum hypophosphite (ADP). ADP is the best commercial halogen-free flame retardant with the best thermal stability, but there is still a certain degree of decomposition during the processing, which will produce a phosphate structure. At the same time, because high-temperature nylon is used for a long time under harsh conditions such as humidity and heat, there are certain precipitation problems, which will cause corrosion to metals, especially copper and nickel, resulting in serious short-circuit risks. Under conditions of high voltage and high current, there are great safety hazards.

[0004] The precipitation and corrosion of halogen-free flame-retardant high-temperature nylon after high temperature and high humidity are common problems in this industry. There is currently little research in the industry on the above issues, and it is still in its infancy. The existing technology proposes the traditional idea of ​​using zinc borate to stabilize diethyl aluminum hypophosphite and stabilize diethyl aluminum hypophosphite through chelating reaction, but this solution can no longer meet the requirements. Some also propose to use zinc oxide and molecular sieves and other substances with surface adsorption effects to adsorb small molecules to reduce the impact of decomposition products on them. However, although this solution can reduce the precipitation of phosphorus-containing small molecules, it is of no help in solving the precipitation of diethyl aluminum phosphate.

[0005] Therefore, the phenomena of precipitation and corrosion associated with high-temperature processing of halogen-free flame-retardant high-temperature nylon are problems that need to be solved urgently. Summary of the invention

[0006] In order to overcome the above-mentioned defects of the prior art, the present invention proposes a halogen-free flame-retardant high-temperature polyamide composition and its preparation method and application. The specific technical scheme is as follows:

[0007] A halogen-free flame-retardant high-temperature polyamide composition, comprising the following components in parts by weight:

[0008]

[0009] The present application uses molecular sieve and sepiolite in combination, which not only utilizes the simultaneous adsorption of sepiolite and molecular sieve, but also the molecular sieve mainly performs adsorption when the two are used alone, and sepiolite has ionic interaction with phosphate, so the adsorption effect is better. Moreover, the combination of molecular sieve and sepiolite can obtain a significantly higher pH value of the aqueous solution after the plastic particles are soaked, compared with zinc oxide and zinc borate, to prevent the low pH value from causing acidic corrosion to the polyamide composition and the decrease of phosphorus-containing substances in the aqueous solution, indicating that it has good flame retardant precipitation inhibition.

[0010] Furthermore, the specific surface area of ​​the sepiolite is greater than or equal to 50 m 2 / g. The specific surface area of ​​sepiolite is greater than or equal to 50m 2 / g, which increases the specific surface area of ​​sepiolite and makes the adsorption capacity greater.

[0011] Furthermore, the molecular sieve is a 1A-10A type molecular sieve, preferably a 5A type molecular sieve. When the molecular sieve is a 5A type molecular sieve, the adsorption capacity is relatively strong and the influence on other properties is small.

[0012] By adding molecular sieves of a specified level and sepiolite of a specified specific surface area, the phosphoric acid-containing small molecules generated during processing can be effectively adsorbed and a certain degree of adsorption can be exerted on the halogen-free flame retardant to prevent its precipitation under hot and humid conditions. In addition, by adding molecular sieves of a specified level and sepiolite of a specified specific surface area, the corrosive phosphoric acid-containing small molecules can be effectively combined to reduce their corrosion to metals, thereby effectively solving the precipitation and corrosion phenomena associated with high-temperature processing of halogen-free flame-retardant high-temperature nylon.

[0013] Furthermore, the halogen-free flame retardant is diethyl aluminum hypophosphite.

[0014] Furthermore, the reinforcing filler is selected from one or more of fibrous reinforcing materials or flat reinforcing materials.

[0015] Furthermore, the fibrous reinforcing material is selected from one or more of glass fiber and carbon fiber, and the flat plate reinforcing material is selected from one or more of talc and mica.

[0016] Specifically, the semi-aromatic polyamide is derived from the following repeating units: 50 mol% of terephthalic acid-based repeating units and 50 mol% of diamine-based repeating units.

[0017] The diamine-based repeating unit is selected from NH(C2 H 4 NH 2 ) 2 H 2 N[C 2 H 4 NH] 2 C 2 H 4 NH 2 H 2 N[C 2 H 4 NH] 3 C 2 H 4 NH 2 、NH[(CH 2 ) 4 NH 2 ] 2 、NH[(CH 2 ) 5 NH 2 ] 2 、NH[(CH 2 ) 6 NH 2 ] 2 、NH[(CH 2 ) 7 NH 2 ] 2 、NH[(CH 2 ) 8 NH 2 ] 2 、NH[(CH 2 ) 9 NH 2 ] 2 、NH[(CH 2 ) 10 NH 2 ] 2 、NH[(CH 2 ) 11 NH 2 ] 2 、N[(CH 2 ) 12 NH 2 ] 3 、NH[(CH 2 ) 13 NH 2 ] 2 、NH[(CH 2 )14NH 2 ) 2 、NH[(CH 2 ) 15 NH 2 ]2 、NH[(CH 2 ) 16 NH 2 ] 2 、NH[(CH 2 ) 17 NH 2 ] 2 、NH[(CH 2 ) 18 NH 2 ] 2 H 2 N(H 2 C) 10 NH(CH 2 ) 5 NH 2 H 2 N(H 2 C) 10 NH(CH 2 ) 6 NH 2 H 2 N(H 2 C) 10 NH(CH 2 ) 7 NH 2 、 H 2 N(H 2 C) 10 NH(CH 2 ) 8 NH 2 H 2 N(H 2 C) 10 NH(CH 2 ) 9 NH 2 、 H 2 N(H 2 C) 10 NH(CH 2 ) 11 NH 2 H 2 N(H 2 C) 10 NH(CH 2 ) 12 NH 2 H 2 N(H 2 C) 9 NH(CH 2 ) 6 CH(CH 3 )CH 2 NH 2 H 2 N(H2 C) 9 NHCH 2 CH(CH 3 )(CH 2 ) 6 NH 2 NH[(CH 2 ) 6 CH(CH 3 )CH 2 NH 2 ] 2 NH[CH 2 CH(CH 3 )(CH 2 ) 6 NH 2 ] 2 One or more of the .

[0018] The present invention also provides a method for preparing the above-mentioned halogen-free flame-retardant high-temperature polyamide composition, comprising the following steps:

[0019] S1: weighing each component according to the ratio, and premixing each component except the halogen-free flame retardant and the reinforcing filler to obtain a premix;

[0020] S2: feeding the premix of step S1 into an extruder, adding a reinforcing filler into a first side feed port of the extruder, adding a halogen-free flame retardant into a second side feed port of the extruder, performing melt blending and extrusion granulation to obtain the polyamide composition.

[0021] Furthermore, the extruder is a twin-screw extruder, and the processing temperature of the melt blending is 290-330°C.

[0022] The present invention also provides the application of the halogen-free flame-retardant high-temperature polyamide composition in high-voltage connectors and busbars in the field of new energy vehicles.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention significantly reduces the overall content of phosphorus-containing substances in the precipitate of the halogen-free flame-retardant polyamide composition under wet heat aging conditions by simultaneously adding sepiolite and molecular sieve into the halogen-free flame-retardant polyamide system. The pH value of the aqueous solution obtained after long-term boiling of polyamide particles is maintained at about 4.6-5.4, the P element content is significantly reduced, and the phosphorus content of the aqueous solution is within the range of 240-480 PPM. The wet heat aging test after the polyamide composition is mixed with copper powder also shows that the corrosion of the polyamide material to the metal under wet heat conditions is greatly reduced, and the tensile strength retention rate after wet heat aging is 83-92%. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] <Preparation of Examples and Comparative Examples>

[0027] The raw materials used in the examples and comparative examples of the present invention are commercially available or homemade, but are not limited to these materials:

[0028] PA10T: Self-made, according to the ratio, decanediamine, terephthalic acid, benzoic acid end-capping agent and deionized water were added into a reactor with nitrogen atmosphere and pressure of 2.8 MPa, the reactor was heated to 180°C, kept at this temperature for 0.5-1.5 hours, then heated to 235°C, kept at this temperature for 10-15 hours to obtain PA10T;

[0029] PA6T: Homemade, according to the ratio, hexamethylenediamine, terephthalic acid, benzoic acid end-capping agent and deionized water were added into a reactor with nitrogen atmosphere and pressure of 2.8Mpa, the reactor was heated to 180°C, kept at this temperature for 0.5-1.5 hours, then heated to 235°C, kept at this temperature for 10-15 hours to obtain PA6T;

[0030] Halogen-free flame retardant: diethyl aluminum hypophosphite, purchased from Clariant;

[0031] Sepiolite A: Specific surface area 50m 2 / g, brand CLAY 20, purchased from Tolsa, Spain;

[0032] Sepiolite B: Specific surface area 50m 2 / g, brand CLAY 80, purchased from Tolsa, Spain;

[0033] Sepiolite C: Specific surface area 30m 2 / g, brand sepiolite fiber, purchased from Lingshou County Wanzhu Mineral Products Co., Ltd.

[0034] Molecular sieve A: 5A molecular sieve, brand 5A, purchased from Guangdong Xintao Technology;

[0035] Molecular sieve B: 3A molecular sieve, grade 3A, purchased from Guangdong Xintao Technology;

[0036] Glass fiber: brand ECS301HP, purchased from Chongqing International Composite Materials Co., Ltd.;

[0037] Zinc borate: analytical grade, purchased from Anaiji Chemical;

[0038] Zinc oxide: analytical grade, purchased from Anaiji Chemical;

[0039] Copper powder: purchased from Henan Kedifei New Material Technology Co., Ltd.

[0040] The preparation methods of the embodiments of the present invention and the comparative examples are as follows:

[0041] S1: According to the ratios in Tables 1 and 3, weigh the components, and premix the components except the halogen-free flame retardant and the reinforcing filler to obtain a premix;

[0042] S2: putting the premix of step S1 into an extruder, adding the reinforcing filler into a first side feed port of the twin-screw extruder, adding the halogen-free flame retardant into a second side feed port of the twin-screw extruder, performing melt blending and extrusion granulation to obtain a polyamide composition.

[0043] The screw length-diameter ratio of the twin-screw extruder is 52:1, the barrel temperature of the twin-screw extruder is 290-330°C, the screw speed of the twin-screw extruder is 200r / min, and the feeding speed is 350Kg / h.

[0044] <Test Standard>

[0045] The performance test standards of the embodiments and comparative examples of the present invention are as follows:

[0046] Aqueous solution pH test: 9 g of the polyamide composition was placed in a sealed container at 100° C. with 30 ml of distilled water for 72 hours, and then the solution was filtered and the pH value was tested;

[0047] Phosphorus content test of aqueous solution: 9 g of polyamide composition was placed in a sealed container at 100° C. with 30 ml of distilled water for 72 hours, and then the solution was filtered and then the ICP phosphorus content test was performed;

[0048] Tensile strength test after wet heat: Since it is necessary to test the metal corrosion performance of the material, copper powder is added to the formula of the polyamide composition so that the metal corrosion test can be carried out. According to the national standard ISO 527-1 / -2-2012 injection molding standard tensile specimens, they are placed in an environment of 85% humidity and 85°C for 168 hours, and then the tensile strength test is carried out according to ISO 527:2012. Due to the presence of copper powder in the material, once the flame retardant corrodes copper to produce copper ions, voids will be left in place, resulting in a significant decrease in tensile strength. The corrosion to the metal can be compared by comparing the mechanical decrease.

[0049] Table 1. Formula of Examples 1-6 (parts by weight)

[0050] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 PA10T 35 50 50 50 50 PA6T 68 Fiberglass 50 15 30 30 30 30 Halogen-free flame retardant 20 10 18 18 18 18 Sepiolite A 3 1 2 2 Sepiolite B 2 Sepiolite C 2 Molecular sieve A 3 1 2 2 Molecular sieve B 2 2 Copper powder 1 1 1 1 1 1

[0051] Table 2. Performance test results of Examples 1-5

[0052] Test items Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 pH value of aqueous solution 5.4 4.9 5.0 4.6 4.7 4.5 Phosphorus content in aqueous solution / PPM 240 332 301 480 443 526 Initial tensile strength / Mpa 163 126 120 125 129 132 Tensile strength after wet heat aging / Mpa 150 105 108 106 112 104 Tensile strength retention rate / % 92 83 90 85 87 79

[0053] Table 3. Comparative Examples 1-9 formulations (parts by weight)

[0054]

[0055] Table 4. Performance test results of comparative examples 1-9

[0056]

[0057] Compared with Example 3, Comparative Example 1 does not use sepiolite and molecular sieve at the same time. The pH value of the aqueous solution of Comparative Example 1 is reduced, the phosphorus content in the aqueous solution is greatly increased, and the retention rate of tensile strength before and after wet heat aging is reduced, indicating that the metal corrosion of Comparative Example 1 is reduced.

[0058] Compared with Example 3, Comparative Example 2 does not use molecular sieves, the pH value of the aqueous solution of Comparative Example 2 is reduced, the phosphorus content in the aqueous solution is significantly increased, and the retention rate of tensile strength before and after wet heat aging is reduced, indicating that the metal corrosion resistance of Comparative Example 2 is reduced.

[0059] Compared with Example 3, Comparative Example 3 does not use sepiolite, the pH value of the aqueous solution of Comparative Example 3 is reduced, the phosphorus content in the aqueous solution is increased, and the retention rate of tensile strength before and after wet heat aging is reduced.

[0060] Compared with Example 3, Comparative Example 4 has an excess of sepiolite, the pH value of the aqueous solution of Comparative Example 4 is increased, the phosphorus content in the aqueous solution is reduced, and the retention rate of tensile strength before and after wet heat aging is increased, but the mechanical properties of the material are extremely poor and it has no practical use value at all.

[0061] Compared with Example 3, the molecular sieve in Comparative Example 5 is excessive, and the pH value of the aqueous solution in Comparative Example 5 is increased.

[0062] Compared with Example 3, Comparative Example 6 has too little sepiolite, the pH value of the aqueous solution of Comparative Example 6 is reduced, the phosphorus content in the aqueous solution is increased, the retention rate of tensile strength before and after wet heat aging is reduced, and the metal corrosion resistance is reduced.

[0063] Compared with Example 3, Comparative Example 7 has too little molecular sieve, which leads to a decrease in the pH value of its aqueous solution, a significant increase in the phosphorus content in the aqueous solution, and a decrease in the retention rate of tensile strength before and after wet heat aging.

[0064] Compared with Example 3, Comparative Example 8 uses zinc oxide, the pH value of the aqueous solution of Comparative Example 8 is reduced, the phosphorus content in the aqueous solution is increased, and the retention rate of tensile strength before and after wet heat aging is reduced. Its overall performance is not as good as using sepiolite and molecular sieve at the optimal ratio, which is due to the poor ability of zinc oxide itself to neutralize and adsorb acidic small molecules.

[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A halogen-free flame-retardant high-temperature polyamide composition, It is characterized in that By weight, it includes the following components: The specific surface area of ​​the sepiolite is greater than or equal to 50m 2 / g.

2. The halogen-free flame-retardant high-temperature polyamide composition according to claim 1, It is characterized in that The molecular sieve is a 1A-10A type molecular sieve.

3. The halogen-free flame-retardant high-temperature polyamide composition according to claim 1, It is characterized in that The molecular sieve is a 5A type molecular sieve.

4. The halogen-free flame-retardant high-temperature polyamide composition according to claim 1, It is characterized in that The halogen-free flame retardant is diethyl aluminum hypophosphite.

5. The halogen-free flame-retardant high-temperature polyamide composition according to claim 1, It is characterized in that The reinforcing filler is selected from one or more of fibrous reinforcing materials or flat reinforcing materials.

6. The halogen-free flame-retardant high-temperature polyamide composition according to claim 5, It is characterized in that The fibrous reinforcing material is selected from one or more of glass fiber and carbon fiber, and the flat plate reinforcing material is selected from one or more of talc and mica.

7. A method for preparing the halogen-free flame-retardant high-temperature polyamide composition according to any one of claims 1 to 6, It is characterized in that The following steps are involved: S1: weighing each component according to the ratio, and premixing each component except the halogen-free flame retardant and the reinforcing filler to obtain a premix; S2: feeding the premix of step S1 into an extruder, adding a reinforcing filler into a first side feed port of the extruder, adding a halogen-free flame retardant into a second side feed port of the extruder, performing melt blending and extrusion granulation to obtain the polyamide composition.

8. Use of the halogen-free flame-retardant high-temperature polyamide composition according to any one of claims 1 to 6 in the field of new energy vehicles.