Production process of double-sided grain suede leather

Through the steps of retanning, neutralization and fat filling, combined with the leather grinding process, it solves the problem of difficulty in balancing the grain and suede quality of NAPPA leather products, improves the performance and aesthetics of the leather, and achieves high added value and Eco-friendly double-sided leather production.

CN116732254BActive Publication Date: 2024-10-25LONG FENG GE LE MEI FASHION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310821114.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-05
Publication Date
2024-10-25
Estimated Expiration
2043-07-05

AI Technical Summary

Technical Problem

It is difficult for existing NAPPA leather products to take into account the quality of both grain and suede surfaces, resulting in poor hand feel, low quality, low grade, and poor performance in finished products.

Method used

Using steps such as retanning, neutralization and fat filling, combined with the leather grinding process, the uniformity, fineness and mercerization of the leather are improved through chemical and physical mechanical methods, including the use of specific chemicals and process parameters such as liquid ratio and temperature. , pH value and softness and hardness control of leather grinding machine.

Benefits of technology

It achieves the high utilization rate, aesthetics and high added value of grained suede double-sided leather. The suede has fine pile heads, good grain flatness, good mercerizing feel and hygienic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116732254B_ABST
    Figure CN116732254B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of leather processing, and discloses a production process of grain suede double-sided leather, which comprises the following steps: pre-treating wet blue leather to obtain leather, and sequentially retanning, neutralizing, fat-filling and filling the leather before intermediate treatment; grinding the leather after the intermediate treatment; the retanning comprises the following steps: adding water, fat-liquor, formic acid, retanning filler, tannin and aluminum tanning agent into a drum and rotating it; soaking after rotating, adding sodium acetate and baking soda after the soaking, rotating it, draining, washing it with water and then draining it; the neutralization comprises the following steps: adding water, neutralizing tannin and baking soda into the drum, rotating it, draining, washing it with water and then draining it; the product prepared according to the process of the invention is a double-sided leather with both grain and suede, taking into account the quality of the grain and suede, the suede pile is uniform, the grain flatness and fineness are good, the breathability and water vapor permeability are good, and the leather is easy to care for.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of leather processing, in particular to a production process of grain suede double-sided leather. Background Art

[0002] NAPPA leather products, due to the difficulty in processing, usually only one side of the leather, either the grain side or the suede side, is used for the main processing, and it is difficult for the finished product to take into account the performance of both the grain side and the suede side.

[0003] The difficulties in developing and processing NAPPA leather grain suede products are: ① Double-faced leather: It is often difficult to take into account the quality of both the suede and grain of NAPPA leather. Either the quality of the suede is taken care of as much as possible during the process, resulting in coarse grain and color spots; or the quality of the grain is taken care of as much as possible during the process, resulting in coarse suede and color spots; ② Suede mercerization: Suede products with good quality have high requirements for mercerization. How to create an excellent mercerization for double-faced leather is a key problem that needs to be overcome. These problems seriously restrict the performance of NAPPA leather. If they can be overcome through research and development, the added value of NAPPA leather products can be greatly increased, and its economic and environmental benefits will be significant. Summary of the invention

[0004] The purpose of the present invention is to produce NAPPA leather with high utilization rate, beautiful product and high added value in order to solve the technical problem that NAPPA leather products in the prior art are difficult to balance the quality of grain and suede, and the resulting grain and suede double-sided leather products have poor hand feel, low quality and low grade.

[0005] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0006] The production process of grain suede double-sided leather includes the following steps: pre-treating wet blue leather to obtain leather, retanning, neutralizing, fat filling and filling the leather in sequence and then performing intermediate treatment; grinding the leather after the intermediate treatment;

[0007] The retanning comprises the following steps: adding water, fatliquor, formic acid, retanning filler, tannin and aluminum tanning agent into a rotary drum and rotating it; soaking after rotating it, adding sodium acetate and baking soda after soaking, rotating it, draining it, washing it with water and draining it;

[0008] The neutralization comprises the following steps: adding water, neutralizing tannin, and baking soda into the drum, rotating, draining, washing with water, and then draining;

[0009] The greasing and filling process comprises the following steps: adding water, synthetic tanning agent, greasing agent, synthetic oil, emulsifier, mildewproof agent, dispersing aid and formic acid into the drum and rotating; draining the water and then draining the water.

[0010] Preferably, in the retanning, 1% of the leather mass of degreasing agent, 0.6% of the leather mass of formic acid, 4-6% of the leather mass of retanning filler, 6-8% of the leather mass of tannin, 2-4% of the leather mass of aluminum tanning agent, 2% of the leather mass of sodium acetate, and 0.3% of the leather mass of baking soda are added.

[0011] Preferably, in the retanning, the aluminum tanning agent is at least one of the aluminum tanning agent NOVALTAN AL of ZIEMA Chemical, the aluminum tanning agent DESOATEN ALF of Desail Chemical, TRUPOTAN ALP of TUMPLER Chemical, and UKATAN PRE of SCHILL+SEILACHER Chemical;

[0012] The retanning filler is at least one of potassium chromium sulfate dodecahydrate RELATAN T.KAL and synthetic tanning agent UKATANSLH of Cromo Chemicals.

[0013] Specifically, in the retanning process, the temperature of the water added is 45°C, the liquid ratio is 100%, 1% of the leather weight of TFL Chemical's synthetic fatliquor CORIPOL SLG is added, the leather is rotated for 20 minutes, 0.6% of the leather weight of formic acid is added, the leather is rotated for 15 minutes, the pH is adjusted to 3.8-4.0, 4-6% of the leather weight of retanning filler is added, the leather is rotated for 30 minutes, 6-8% of the leather weight of TFL Chemical's chromium-containing tannin is added, the leather is rotated for 30 minutes, 2-4% of the leather weight of aluminum tanning agent is added, the leather is rotated for 90 minutes, and the leather is soaked for 8 hours, rotating for 5 minutes every hour. After the soaking is completed, 2% of the leather weight of sodium acetate is added, the leather is rotated for 90 minutes, 0.3% of the leather weight of baking soda is added, the leather is rotated for 30 minutes, the pH is adjusted to 3.8-4.0, the leather is drained, and the leather is washed with water once.

[0014] Preferably, during the neutralization, 3% of the weight of the leather is added as neutralizing tannin, and 0.5% of the weight of the leather is added as baking soda.

[0015] Preferably, in the neutralization, the neutralized tannin is at least one of the neutralized tannin TANIGAN PAK N LIQ of LANXESS Chemicals, lead base of STAHL Chemicals, PELLUPUR MP3 / C of PULCRA Chemicals, and SELLASOL NG LIQ of TFL Chemicals.

[0016] Specifically, during the neutralization, the temperature of the added water is 40° C., the liquid ratio is 150%, 3% of the weight of the leather is added to neutralize tannin, the leather is rotated for 30 minutes, 0.5% of the weight of the leather is added to baking soda, the leather is rotated for 30 minutes, the pH is adjusted to 5.0-5.5, the leather is drained, and the leather is washed once.

[0017] Preferably, in the fat filling, 20% of synthetic tanning agent by weight of the leather, 3% of fatliquor by weight of the leather, 2% of synthetic oil by weight of the leather, 0.5% of emulsifier by weight of the leather, 0.05% of mildewproofing agent by weight of the leather, 1% of dispersing aid by weight of the leather, and 3% of formic acid by weight of the leather are added.

[0018] Preferably, in the fat filling, the synthetic tanning agent is at least one of the synthetic tanning agent RETENAL RCN-40 of Cromo Chemical, the synthetic tanning agent UKATAN SLH of SCHILL+SEILACHER Chemical, the synthetic tanning agent UKATAN INF of SCHILL+SEILACHER Chemical, and the synthetic tanning agent PELLITAN NS of REPICO Chemical;

[0019] The fatliquor is at least one of the sulfated fatliquor FOSFOL 50 of CROMOGENIA Chemicals and the sulfonated fatliquor Lipsol h60 of SCHILL+SEILACHER Chemicals.

[0020] Specifically, in the fat filling, the temperature of the added water is 50°C, the liquid ratio is 150%, 2% of the leather weight of the synthetic tanning agent RETENAL RCN-40 of Cromo Chemical is added, and the leather is rotated for 30 minutes, 2% of the leather weight of the sulfated fatliquor FOSFOL 50 of CROMOGENIA Chemical is added, 2% of the leather weight of the synthetic oil HPW303 of TFL Chemical is added, 1% of the leather weight of the sulfonated fatliquor Lipsol h60 of SCHILL+SEILACHER Chemical is added, 0.5% of the leather weight of the emulsifier BORRON SAF of TFL Chemical is added, 0.05% of the leather weight of the mildew preventer BK 55 of Shangqiu Boska Chemical is added, and the leather is rotated for 60 minutes, 6% of the leather weight of the synthetic tanning agent UKATAN SLH of SCHILL+SEILACHER Chemical is added, and 6% of the leather weight of the synthetic tanning agent UKATAN INF, add 6% of the leather mass of REPICO Chemical's synthetic tanning agent PELLITAN NS, add 1% of the leather mass of BASF Chemical's dispersing aid TAMOL GA, rotate for 120 minutes, add 1% of the leather mass of formic acid, rotate for 20 minutes, add 1% of the leather mass of formic acid, rotate for 20 minutes, add 1% of the leather mass of formic acid, rotate for 20 minutes, adjust the pH to 3.6-3.8, drain and wash once, and take out the leather.

[0021] Preferably, the leather grinding comprises the following steps: controlling the moisture content of the leather to 20-30% and grinding the leather; using a leather grinding machine to grind the suede of the leather for multiple times during the leather grinding process, and the hardness of the rubber roller of the leather grinding machine is 18-20HA; and dust removal is performed after each leather grinding. The hardness of the rubber roller in the present invention is Shore hardness HA.

[0022] Preferably, the mesh number of the sandpaper used in each leather grinding is larger than the mesh number of the sandpaper used in the previous leather grinding.

[0023] Preferably, after the leather is polished with a leather polishing machine, a grinding wheel is used to polish the suede surface of the leather; and dust removal is performed after the leather polishing with the grinding wheel is completed.

[0024] Preferably, the leather grinding process includes the following steps in sequence:

[0025] ① The first time of leather grinding, use a leather grinding machine to grind the suede surface. The hardness of the leather grinding machine roller is 18-20HA, and 400 mesh sandpaper is used;

[0026] ② One-time dust removal, dust removal on the suede surface;

[0027] ③ The second time of leather grinding, use a leather grinding machine to grind the suede surface, the hardness of the leather grinding machine roller is 18-20HA, and 600 mesh sandpaper is used;

[0028] ④ Secondary dust removal, dust removal on the suede surface;

[0029] ⑤ The third time of leather grinding, use a leather grinding machine to grind the suede surface, the hardness of the leather grinding machine roller is 18-20HA, and 800 mesh sandpaper is used;

[0030] ⑥Three times of dust removal, dust removal on the suede surface;

[0031] ⑦ The fourth grinding, use a 1000-grit grinding wheel to grind the suede surface;

[0032] ⑧ Four times of dust removal to remove dust from the suede surface;

[0033] Specifically, the leather grinding process includes the following steps in sequence:

[0034] ① The first leather grinding: Use a leather grinding machine to grind the suede surface. The hardness of the leather grinding machine roller is 18-20HA, and 400-grit sandpaper is used; the leather feeding speed is 9.3-9.5m / min. Operation method: horizontal two-knife method, the first knife is made on any side of the belly, and the leather feeding position accounts for 4 / 5, and then the other side of the belly is used to receive the knife mark. Remember that the second knife should not pass the middle spine;

[0035] ②One-time dust removal: Use a through-type dust collector to remove dust from the suede surface once;

[0036] ③ The second leather grinding: Use a leather grinding machine to grind the suede surface. The hardness of the leather grinding machine roller is 18-20HA, and 600 mesh sandpaper is used;

[0037] The skin penetration speed is 9.3-9.5m / min. The operation method is two vertical cuts, head first and tail later. The first cut is made with the head first, and the skin penetration position is at the front leg fossa. The second cut is made with the tail first, and the cut mark is taken.

[0038] ④ Secondary dust removal: Use a through-type dust collector to remove dust from the suede surface once;

[0039] ⑤ The third leather grinding: Use a leather grinding machine to grind the suede surface. The hardness of the leather grinding machine roller is 18-20HA, and 800 mesh sandpaper is used;

[0040] The skin feeding speed is 9.3-9.5m / min. The operation method is: tail first, 1 knife through.

[0041] ⑥Three times of dust removal: Use a through-type dust collector to remove dust from the suede surface once;

[0042] ⑦ The fourth leather grinding: use a small grinding wheel, 1000 mesh grinding wheel, operation method: conventional small grinding wheel leather grinding method, but pay attention to the four sides of the leather to be ground in place;

[0043] ⑧Fourth dust removal: dust the suede surface.

[0044] Preferably, the pre-treatment includes one or more of wet blue leather sorting, wet grinding, water recovery and degreasing; the intermediate treatment includes one or more of mounting and standing, squeezing water, hanging and drying, vibration softening, stretching softening, trimming, water spraying and wrapping and standing.

[0045] Specifically, in the wet blue leather sorting process, the wet blue leather is specifically the wet blue leather of sheepskin. The specific sorting method is well known to those skilled in the art and will not be described in detail here.

[0046] Specifically, a small grinding wheel is used for wet grinding. In terms of technique, attention should be paid to grinding away the meat residue on the sides of the abdomen, and lightly grinding the middle spine. Only the obvious meat residue needs to be ground away. It is better to be light than heavy. The entire meat residue should be ground clean, and the middle spine should not be over-ground.

[0047] Preferably, the water return process comprises the following steps: adding water, leather, degreasing agent, and emulsifier BORRON SAF into a rotating drum, rotating and draining the water, and washing and draining the water; adding 1% of the leather weight degreasing agent and 1% of the leather weight emulsifier BORRON SAF into the returned water; the degreasing agent in the returned water is SUPRALAN DT-C produced by Zschimmer Chemical.

[0048] Specifically, the temperature of the water added to the return water is 40° C., the liquid ratio is 300% (in the present invention, the liquid ratio is calculated based on the weight of the leather processed in the drum), 1% of the weight of the leather is added as a degreasing agent, 1% of the weight of the leather is added as an emulsifier BORRON SAF, the leather is rotated for 90 minutes, the water is drained, and the leather is washed once.

[0049] Preferably, the degreasing process includes the following steps: adding water, degreasing agent, Baibang CC and EDTA into a rotating drum, rotating and draining the water; during the degreasing, adding 1% of the leather weight of the degreasing agent, adding 1% of the leather weight of Baibang CC, and adding 1% of the leather weight of EDTA; during the degreasing, the degreasing agent is SUPRALAN DT-C, a degreasing agent produced by Zschimmer Chemical.

[0050] Specifically, in the degreasing, the temperature of the added water is 40°C, the liquid ratio is 100%, 1% of the leather weight of the degreasing agent, 1% of the leather weight of PULCRA Chemical's Baibang CC, 1% of the leather weight of Luoyang Langjie Company's EDTA are added, the leather is rotated for 90 minutes, drained, and washed with water once.

[0051] Specifically, during the horse-riding and resting process, the usual horse-riding method is selected and the horse-riding is left to rest for 8 hours;

[0052] Specifically, during the squeezing process, the squeezing pressure is 10kg, the gap between the knife and the roller is 10-15, the meat side is facing up and the grain side is facing down, two horizontal cuts are made without returning the knife; pay special attention to the first cut into the skin, the skin is inserted a little more, and only about 20 cm wide belly is left outside;

[0053] Specifically, during the hanging and drying process, the usual hanging and drying method is selected, and the leather is collected when the humidity of the pole is 10-12 degrees;

[0054] Specifically, during the softening process, a softening machine is used, adjusted to 4 pressures, 1 pass, single skin is fed, grain side facing up, and the skin is spread out by hand without curling;

[0055] Specifically, the softening machine is used in the softening process, with single sheet operation, grain side facing downward, two-knife method, and no curling;

[0056] Specifically, use a through-type water sprayer during the water spraying process, with two rows of water, open the first and third rows, 1 time, single skinning, no need to stack the skins, velvet side up, grain side down, no need to worry about line marks, pass horizontally, and after joining the skins, velvet side faces velvet side, and mount.

[0057] Specifically, during the wrapping and standing process, the wrapping is left to stand for 4-8 hours. When making large quantities (large areas of leather), it can be left to stand overnight. The moisture content at the end of standing can be controlled between 20-25%.

[0058] Working principle:

[0059] The chemical materials and specific processes used in the three steps of retanning, filling and fat-liquoring of the present invention play the following roles: 1. excellent leather uniformity is shaped, and the problem of thin and loose leather edges and bellies is solved; 2. chemical methods are used to improve the fineness and consistency of suede pile and the flatness of grain patterns; 3. the chemical materials used themselves have a certain bleaching effect, such as UKATAN SLH used in the present invention, which makes the color of the leather (prepared embryo) of the present invention whiter and has the basis for dyeing light and bright colors, while the color of general suede prepared embryos is similar to blue wet leather, which is relatively deep and dark, and bright colors such as milky white, bright yellow, and light pink cannot be dyed. The obtained by the present invention can be dyed with these colors, and the finished product after dyeing has uniform and bright color.

[0060] The effects of the leather grinding process of the present invention are as follows: by using physical and mechanical effects, that is, with the help of a leather grinding machine, the fineness of the suede surface and the consistency of the suede guide are improved, but in this process, there are many control factors, such as the moisture retention range (if the moisture is too low, the suede will definitely be coarse; if the moisture is too high, the mechanical effect is not good and the suede grinding will be uneven), the selection of the hardness of the roller of the leather grinding machine (the harder the roller, the easier it is to cause the middle ridge to be ground, and the softer the roller, the better the uniformity of the suede grinding), the selection of the sandpaper mesh number, the number of leather grinding times, and the dust removal effect (if the dust removal is not clean, it is easy to cause irreversible padding problems in the next leather grinding), all of which will affect the final quality.

[0061] The invention starts from wet blue leather and undergoes a series of processes to produce a dual-purpose leather for a shoe upper having both a grain surface and a suede surface. The product advantages of the invention are as follows: 1. The product obtained by the invention is a double-faced leather. For subsequent coating, a corresponding beautiful coating style can be made on one side of the grain surface or the suede surface according to customer needs, wherein different colors can be coated on the grain surface and the suede surface to produce a contrasting coating and form a contrasting effect; for downstream shoe factories, both sides can be cut and used according to their own needs; 2. The leather has good hygienic performance, good breathability and water vapor permeability, and is easy to care for; 3. The leather embryo produced by the process of the invention has uniform and beautiful color after dyeing, and the suede pile is uniform and consistent, and the grain surface has good flatness and fineness.

[0062] The product prepared by the present invention has a good mercerization feeling. Under the irradiation of light, the leather suede presents tiny gloss points, which are as shiny as silk. The gloss points will change with the change of angle and intensity, so that the leather surface presents a unique visual effect under different light. This mercerization feeling usually gives people a sense of elegance and nobility, making the leather products look more refined and fashionable.

[0063] Beneficial effects:

[0064] The product prepared according to the process of the present invention is a double-faced leather having both grain and suede, taking into account the quality of both the grain and suede, with fine and evenly distributed suede pile and good grain flatness; good breathability and water vapor permeability, easy to care for; and good mercerization. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 This is a process flow chart of Example 1 of the present invention;

[0066] Figure 2 This is a schematic diagram of the finished leather obtained after coating the grain suede double-sided leather obtained in Example 2 of the present invention. DETAILED DESCRIPTION

[0067] The present invention is further described below with reference to specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0068] The specific manufacturers of some of the chemical materials involved in the present invention are shown in the following table:

[0069] name factory Aluminium tanning agent NOVALTAN AL ZIHAI CHEMICALS Aluminium tanning agent DESOATEN ALF Desail Chemical TRUPOTAN ALP Thomson Chemical UKATAN PRE SCHILL+SEILACHER Chemicals RELATAN T.KAL Potassium Chromium Sulfate Dodecahydrate Cromo Chemicals Synthetic fatliquor CORIPOL SLG TFL Chemicals Chrome tannins TFL Chemicals Neutralizing Tannin TANIGAN PAK N LIQ LANXESS Chemicals Lead STAHL Chemicals PELLUPUR MP3 / C PULCRA Chemicals SELLASOL NG LIQ TFL Chemical Synthetic tanning agent RETENAL RCN-40 Cromo Chemicals Synthetic tanning agent UKATAN SLH SCHILL+SEILACHER Chemicals Synthetic tanning agent UKATAN INF SCHILL+SEILACHER Chemicals Synthetic tanning agent PELLITAN NS REPICO Chemicals Sulfated fatliquor FOSFOL 50 CROMOGENIA Chemicals Sulfonated fatliquor Lipsol h60 SCHILL+SEILACHER Chemicals Synthetic oil HPW 303 TFL Chemicals Antifungal agent BK 55 Shangqiu Boska Chemical Emulsifier BORRON SAF TFL Chemicals Dispersing agent TAMOL GA BASF Chemicals Degreasing agent SUPRALAN DT-C ZIHAI CHEMICALS Baibang CC PULCRA Chemicals EDTA Luoyang Langjie Company

[0070] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0071] There is no particular restriction on the purity of all raw materials in the present invention. The present invention preferably uses industrial purity or conventional purity used in the field of leather preparation.

[0072] The brands and abbreviations of all raw materials of the present invention are conventional brands and abbreviations in the art. Each brand and abbreviation is clear and definite in the field of its related use. Those skilled in the art can purchase them from the market or prepare them by conventional methods according to the brands, abbreviations and corresponding uses.

[0073] The abbreviations of all processes of the present invention are conventional abbreviations in the field, and each abbreviation is clear and unambiguous in the field of its relevant use. Those skilled in the art can understand its conventional process steps based on the abbreviations, such as blue wet leather sorting, wet grinding, water return, degreasing, riding and standing, squeezing water, hanging and airing, vibrating and softening, stretching and softening, trimming, water spraying, and wrapping and standing.

[0074] In the following examples, the liquid ratios involved in each step and the percentages of each chemical used are based on the mass of the leather processed in the drum, and the percentages calculated are based on the mass of the leather.

[0075] Example 1

[0076] like Figure 1As shown, the production process of the grain suede double-sided leather includes the following steps:

[0077] 1. Wet blue leather sorting.

[0078] 2. Wet grinding: Use a small grinding wheel for wet grinding. Pay attention to grinding the meat residue on the sides and abdomen cleanly. Grind the middle spine lightly. Only the obvious meat residue needs to be removed. Grind the whole meat residue cleanly, and do not grind over the middle spine.

[0079] 3. Return water: temperature 40℃, liquid ratio 300 (calculated based on tare weight), add 1% of ZIMA Chemical's degreasing agent SUPRALAND T-C, add 1% of TFL Chemical's emulsifier BORRON SAF, rotate for 90 minutes, drain, and wash once.

[0080] 4. Degreasing: temperature 40℃, liquid ratio 100%, add 1% of SUPRALAN DT-C degreasing agent from Sima Chemical, 1% of Baibang CC from PULCRA Chemical, 1% of EDTA from Luoyang Langjie Company, rotate for 90 minutes, drain, and wash once.

[0081] 5. Retanning: Temperature 45℃, liquid ratio 100%, add TFL Chemical's synthetic fatliquor CORIPOL SLG 1%, rotate for 20 minutes, add formic acid 0.6%, rotate for 15 minutes, adjust pH 3.8-4.0, add Cromo Chemical's potassium chromium sulfate dodecahydrate RELATAN T.KAL 6%, rotate for 30 minutes, add TFL Chemical's chromium-containing tannin HN 6%, rotate for 30 minutes, add Sima Chemical's aluminum tanning agent NOVALTAN AL 2%, rotate for 90 minutes, overnight for 8 hours, rotate for 5 minutes every hour. After overnight, add sodium acetate 2%, rotate for 90 minutes, add baking soda 0.3%, rotate for 30 minutes, adjust pH 3.8-4.0, drain, and wash once.

[0082] 6. Neutralization: temperature 40℃, liquid ratio 150%, add 3% of neutralizing tannin TANIGAN PAK N LIQ from LANXESS Chemical, rotate for 30 minutes, add 0.5% of baking soda, rotate for 30 minutes, adjust pH 5.0-5.5, drain, and wash once.

[0083] 7. Fat filling: temperature 50℃, liquid ratio 150%, add 2% of Cromo Chemical's synthetic tanning agent RETENAL RCN-40, rotate for 30 minutes, add 2% of sulfated fatliquor FOSFOL 50 from CROMOGENIA Chemical, add 2% of synthetic oil HPW 303 from TFL Chemical, add 1% of sulfonated fatliquor Lipsol h60 from SCHILL+SEILACHER Chemical, add 0.5% of emulsifier BORRON SAF from TFL Chemical, add 0.05% of mildew preventer BK 55 from Shangqiu Boska Chemical, rotate for 60 minutes, add 6% of synthetic tanning agent UKATAN SLH from SCHILL+SEILACHER Chemical, add 6% of synthetic tanning agent UKATAN INF from SCHILL+SEILACHER Chemical, add 6% of synthetic tanning agent PELLITAN NS from REPICO Chemical, add 6% of dispersing aid TAMOL GA from BASF Chemical 1%, rotate for 120 minutes, add formic acid 1%, rotate for 20 minutes, add formic acid 1%, rotate for 20 minutes, add formic acid 1%, rotate for 20 minutes, adjust pH 3.6-3.8, drain and wash once, and remove the skin.

[0084] 8. Mount the horse and let it stand still.

[0085] 9. Squeeze out the water.

[0086] 10. Hang to dry.

[0087] 11. Vibrate to soften.

[0088] 12. Softening: The equipment is a horizontal double-knife softening machine, single-sheet operation, grain side down, two-knife method, no curling.

[0089] 13. Trimming

[0090] 14. Water spraying: The equipment is a through-type water spraying machine with two rows of water. Open the first and third rows, 1 time, single skinning, no need to stack the skins, velvet side up, grain side down, no need to worry about line marks, pass horizontally, velvet side to velvet side after skinning, and mount.

[0091] 15. Wrap and let stand: Wrap and let stand for 4-8 hours (when making large quantities, it can be left overnight). At the end of standing, the moisture content should be controlled between 20-25%.

[0092] 16. Grinding: The moisture content before grinding is 20-30%. The specific operation is as follows:

[0093] ① The first leather grinding: the equipment is a large leather grinding machine, the hardness of the rubber roller (the roller of the leather grinding machine) is 18-20HA, 400 mesh sandpaper, the leather feeding speed is 9.3-9.5m / min, the operation method is: the horizontal two-knife method, the first knife is made on any side of the belly, the leather feeding position accounts for 4 / 5, and then the other side of the belly is used to feed the skin, and the knife mark is taken. Remember that the second knife cannot pass the middle spine;

[0094] ② Dust removal: through-type dust removal machine, 1 time; check that the large meat residue is basically ground clean;

[0095] ③ The second leather grinding: the equipment is a large leather grinding machine, the hardness of the rubber roller is 18-20HA, the sandpaper is 600 mesh, the leather feeding speed is 9.3-9.5m / min, the operation method is: vertical two-knife method, first head and then tail, the first knife head is advanced, the leather feeding position is to the front leg fossa, the second knife tail is advanced to receive the knife mark;

[0096] ④Dust removal: through-type dust removal machine, 1 time; check that the large meat residue is ground clean;

[0097] ⑤The third leather grinding: the equipment is a large leather grinding machine, the hardness of the rubber roller is 18-20HA, 800 mesh sandpaper, the leather feeding speed is 9.3-9.5m / min, and the operation method is: tail first, 1 knife pass.

[0098] ⑥ Dust removal: pass through dust collector, 1 time; check the fineness and uniformity of pile;

[0099] ⑦ The fourth leather grinding: the equipment is a small grinding wheel, 1000 mesh sand, the operation method is the conventional small grinding wheel leather grinding method, but pay attention to the four sides of the leather to be ground in place;

[0100] ⑧Dust removal.

[0101] 17. Quality inspection;

[0102] 18. Store in warehouse.

[0103] Example 2

[0104] The production process of grain suede double-sided leather includes the following steps:

[0105] 1. Wet blue leather sorting.

[0106] 2. Wet grinding: Use a small grinding wheel for wet grinding. Pay attention to grinding the meat residue on the sides and abdomen cleanly. Grind the middle spine lightly. Only the obvious meat residue needs to be removed. Grind the whole meat residue cleanly, and do not grind over the middle spine.

[0107] 3. Return water: temperature 40℃, liquid ratio 300% (calculated based on tare weight), add 1% of ZIMA Chemical's degreasing agent SUPRALAND T-C, add 1% of TFL Chemical's emulsifier BORRON SAF, rotate for 90 minutes, drain, and wash once.

[0108] 4. Degreasing: Temperature 40℃, liquid ratio 100%, add 1% of SUPRALAN DT-C degreasing agent from Sima Chemical, 1% of Baibang CC from PULCRA Chemical, 1% of EDTA from Luoyang Langjie Company, rotate for 90 minutes, drain, and wash once;

[0109] 5. Retanning: temperature 45℃, liquid ratio 100%, add TFL Chemical's synthetic fatliquor CORIPOL SLG 1%, rotate for 20 minutes, add formic acid 0.6%, rotate for 15 minutes, adjust pH 3.8-4.0, add Cromo Chemical's potassium chromium sulfate dodecahydrate RELATAN T.KAL 4%, rotate for 30 minutes, add TFL Chemical's chromium-containing tannin HN 8%, rotate for 30 minutes, add Sima Chemical's aluminum tanning agent NOVALTAN AL 4%, rotate for 90 minutes, overnight for 8 hours, rotate for 5 minutes every hour. After overnight, add sodium acetate 2%, rotate for 90 minutes, add baking soda 0.3%, rotate for 30 minutes, adjust pH 3.8-4.0, drain, and wash once.

[0110] 6. Neutralization: temperature 40℃, liquid ratio 150%, add 3% of neutralizing tannin TANIGAN PAK N LIQ from LANXESS Chemical, rotate for 30 minutes, add 0.5% of baking soda, rotate for 30 minutes, adjust pH 5.0-5.5, drain, and wash once.

[0111] 7. Fat filling: temperature 50℃, liquid ratio 150%, add 2% of Cromo Chemical's synthetic tanning agent RETENAL RCN-40, rotate for 30 minutes, add 2% of sulfated fatliquor FOSFOL 50 from CROMOGENIA Chemical, add 2% of synthetic oil HPW 303 from TFL Chemical, add 1% of sulfonated fatliquor Lipsol h60 from SCHILL+SEILACHER Chemical, add 0.5% of emulsifier BORRON SAF from TFL Chemical, add 0.05% of mildew preventer BK 55 from Shangqiu Boska Chemical, rotate for 60 minutes, add 6% of synthetic tanning agent UKATAN SLH from SCHILL+SEILACHER Chemical, add 6% of synthetic tanning agent UKATAN INF from SCHILL+SEILACHER Chemical, add 6% of synthetic tanning agent PELLITAN NS from REPICO Chemical, add TAMOL dispersing agent from BASF Chemical GA1%, rotate for 120 minutes, add formic acid 1%, rotate for 20 minutes, add formic acid 1%, rotate for 20 minutes, add formic acid 1%, rotate for 20 minutes, adjust pH 3.6-3.8, drain and wash once, and remove the skin.

[0112] 8. Mount and let stand: Mount normally and let stand for 8 hours.

[0113] 9. Water squeezing: The water squeezing pressure is 10KG, the gap between the knife and the roller is 10-15, the meat side is facing up, the grain side is facing down, two horizontal cuts are made, and the knife does not return. Pay special attention to the first cut into the skin, the skin should go in a little more, and only about 20 cm wide belly is left outside.

[0114] 10. Hanging to dry: Hang to dry normally, check the humidity at 10-12 degrees, and collect the skin.

[0115] 11. Vibration and softening: The equipment is a vibration and softening machine, adjusted to 4 pressures, 1 pass, single sheet in, grain side up, spread by hand, no curling.

[0116] 12. Softening: The equipment is a horizontal softening machine, single sheet operation, grain side down, two knife method, no curling.

[0117] 13. Trim the edges.

[0118] 14. Water spraying: The equipment is a through-type water spraying machine with two rows of water. Open the first and third rows, 1 time, single skinning, no need to stack the skins, velvet side up, grain side down, no need to worry about line marks, pass horizontally, velvet side to velvet side after skinning, and mount.

[0119] 15. Wrap and let stand: Wrap and let stand for 4-8 hours (when making large quantities, it can be left overnight). At the end of standing, the moisture content should be controlled between 20-25%.

[0120] 16. Grinding: The moisture content before grinding is 20-30%. The specific operation is as follows:

[0121] ① The first leather grinding: the equipment is a large leather grinding machine, the hardness of the rubber roller is 18-20HA, the sandpaper is 400 mesh, the leather feeding speed is 9.3-9.5m / min, the operation method is: the horizontal two-knife method, the first knife is made on any side of the belly, and the leather feeding position accounts for 4 / 5, and then the other side of the belly is used to feed the leather, and the knife mark is taken. Remember that the second knife cannot pass the middle spine;

[0122] ② Dust removal: through-type dust removal machine, 1 time; check that the large meat residue is basically ground clean;

[0123] ③ The second leather grinding: the equipment is a large leather grinding machine, the hardness of the rubber roller is 18-20HA, the sandpaper is 600 mesh, the leather feeding speed is 9.3-9.5m / min, the operation method is: vertical two-knife method, first head and then tail, the first knife head is advanced, the leather feeding position is to the front leg fossa, the second knife tail is advanced to receive the knife mark;

[0124] ④Dust removal: through-type dust removal machine, 1 time; check that the large meat residue is ground clean;

[0125] ⑤ The third leather grinding: the equipment is a large leather grinding machine, the hardness of the rubber roller is 18-20HA, 800 mesh sandpaper, the leather feeding speed is 9.3-9.5m / min, the operation method is: tail first, 1 knife through;

[0126] ⑥ Dust removal: pass through dust collector, 1 time; check the fineness and uniformity of pile;

[0127] ⑦ The fourth leather grinding: the equipment is a small grinding wheel, 1000 mesh sand, the operation method is the conventional small grinding wheel leather grinding method, but pay attention to the four sides of the leather to be ground in place;

[0128] ⑧Dust removal.

[0129] 17. Quality inspection.

[0130] 18. Store in warehouse.

[0131] In this embodiment, the parameters (usage amount) of the chemical materials involved in the retanning process are mainly adjusted, which brings about the following changes: the leather body becomes relatively softer, the suede quality remains the same, but the grain flatness and fineness are improved.

[0132] like Figure 2 As shown, it is a schematic diagram of the finished leather obtained after coating of the grain suede double-sided use leather obtained in Example 2 of the present invention; this figure is a picture of the finished leather processed by the grain suede double-sided use leather (also referred to as white blank in the art) obtained by processing in Example 2 according to a conventional coating process, and the upper half of the figure is the suede and the lower half is the grain.

[0133] Example 3

[0134] The production process of grain suede double-sided leather includes the following steps:

[0135] 1. Wet blue leather sorting.

[0136] 2. Wet grinding: The equipment is to use a small grinding wheel for wet grinding. Pay attention to grinding the meat residue on the side and abdomen cleanly, and grind the middle spine lightly. Only the obvious meat residue needs to be ground cleanly, and it is better to be light than heavy. Grind the whole meat residue cleanly, and do not grind over the middle spine.

[0137] 3. Return water: temperature 40℃, liquid ratio 300% (calculated based on tare weight), add 1% of ZIMA Chemical's degreasing agent SUPRALAND T-C, add 1% of TFL Chemical's emulsifier BORRON SAF, rotate for 90 minutes, drain, and wash once.

[0138] 4. Degreasing: temperature 40℃, liquid ratio 100%, add 1% of SUPRALAN DT-C degreasing agent from Sima Chemical, 1% of Baibang CC from PULCRA Chemical, 1% of EDTA from Luoyang Langjie Company, rotate for 90 minutes, drain, and wash once.

[0139] 5. Retanning: Temperature 45℃, liquid ratio 100%, add TFL Chemical's synthetic fatliquor CORIPOL SLG 1%, rotate for 20 minutes, add formic acid 0.6%, rotate for 15 minutes, adjust pH 3.8-4.0, add Cromo Chemical's potassium chromium sulfate dodecahydrate RELATAN T.KAL 6%, rotate for 30 minutes, add TFL Chemical's chromium-containing tannin HN 6%, rotate for 30 minutes, add Sima Chemical's aluminum tanning agent NOVALTAN AL 2%, rotate for 90 minutes, overnight for 8 hours, rotate for 5 minutes every hour. After overnight, add sodium acetate 2%, rotate for 90 minutes, add baking soda 0.3%, rotate for 30 minutes, adjust pH 3.8-4.0, drain, and wash once.

[0140] 6. Neutralization: temperature 40℃, liquid ratio 150%, add 3% of neutralizing tannin TANIGAN PAK N LIQ from LANXESS Chemical, rotate for 30 minutes, add 0.5% of baking soda, rotate for 30 minutes, adjust pH 5.0-5.5, drain, and wash once.

[0141] 7. Fat filling: temperature 50℃, liquid ratio 150%, add 2% of Cromo Chemical's synthetic tanning agent RETENAL RCN-40, rotate for 30 minutes, add 2% of sulfated fatliquor FOSFOL 50 from CROMOGENIA Chemical, add 2% of synthetic oil HPW 303 from TFL Chemical, add 1% of sulfonated fatliquor Lipsol h60 from SCHILL+SEILACHER Chemical, add 0.5% of emulsifier BORRON SAF from TFL Chemical, add 0.05% of mildew preventer BK 55 from Shangqiu Boska Chemical, rotate for 60 minutes, add 6% of synthetic tanning agent UKATAN SLH from SCHILL+SEILACHER Chemical, add 6% of synthetic tanning agent UKATAN INF from SCHILL+SEILACHER Chemical, add 6% of synthetic tanning agent PELLITAN NS from REPICO Chemical, add TAMOL dispersing agent from BASF Chemical GA1%, rotate for 120 minutes, add formic acid 1%, rotate for 20 minutes, add formic acid 1%, rotate for 20 minutes, add formic acid 1%, rotate for 20 minutes, adjust pH 3.6-3.8, drain and wash once, and remove the skin.

[0142] 8. Mount the horse and let it stand still.

[0143] 9. Water squeezing: The water squeezing pressure is 10KG, the gap between the knife and the roller is 10-15, the meat side is facing up, the grain side is facing down, two horizontal cuts are made, and the knife does not return. Pay special attention to the first cut into the skin, the skin should go in a little more, and only about 20 cm wide belly is left outside.

[0144] 10. Hanging to dry: Hang to dry normally, check the humidity at 10-12 degrees, and collect the skin.

[0145] 11. Vibration and softening: The equipment is a vibration and softening machine, adjusted to 4 pressures, 1 pass, single sheet in, grain side up, spread by hand, no curling.

[0146] 12. Pull and soften.

[0147] 13. Trim the edges.

[0148] 14. Water spraying: The equipment is a through-type water spraying machine with two rows of water. Open the first and third rows, 1 time, single skinning, no need to stack the skins, velvet side up, grain side down, no need to worry about line marks, pass horizontally, velvet side to velvet side after skinning, and mount.

[0149] 15. Wrap and let stand: Wrap and let stand for 4-8 hours (when making large quantities, it can be left overnight). At the end of standing, the moisture content should be controlled between 20-25%.

[0150] 16. Grinding: The moisture content before grinding is 20-30%. The specific operation is as follows:

[0151] ① The first leather grinding: the equipment is a large leather grinding machine, the hardness of the rubber roller is 18-20HA, the sandpaper is 400 mesh, the leather feeding speed is 9.3-9.5m / min, the operation method is: the horizontal two-knife method, the first knife is made on any side of the belly, and the leather feeding position accounts for 4 / 5, and then the other side of the belly is used to feed the leather, and the knife mark is taken. Remember that the second knife cannot pass the middle spine;

[0152] ② Dust removal: through-type dust removal machine, 1 time; check that the large meat residue is basically ground clean;

[0153] ③ The second leather grinding: the equipment is a large leather grinding machine, the hardness of the rubber roller is 18-20HA, the sandpaper is 600 mesh, the leather feeding speed is 9.3-9.5m / min, the operation method is: vertical two-knife method, first head and then tail, the first knife head is advanced, the leather feeding position is to the front leg fossa, the second knife tail is advanced to receive the knife mark;

[0154] ④Dust removal: through-type dust removal machine, 1 time; check that the large meat residue is ground clean;

[0155] ⑤ The third leather grinding: the equipment is a large leather grinding machine, the rubber roller hardness is 18-20HA, 1000 mesh sand, the leather feeding speed is 9.3-9.5m / min, the operation method is: tail first, 1 knife through;

[0156] ⑥Dust removal: Use a pass-through dust collector, 1 time; check the fineness and uniformity of the pile.

[0157] 17. Quality inspection.

[0158] 18. Store in warehouse.

[0159] In this embodiment, the leather grinding process is mainly adjusted, and the original third and fourth leather grinding processes are condensed into one time, saving one leather grinding and one dust removal process. The advantages are: reducing production costs, although the fineness of the suede surface is slightly reduced, it can still meet the use requirements of many customers for suede / grain double-face leather.

[0160] The leather obtained in Example 1, Example 2 and Example 3 was tested, and the test items and results are shown in the following table:

[0161]

[0162] As can be seen from the above table, the product prepared by the process of the invention has good grain flatness, suede fineness and suede mercerization, making it unique in touch and beautiful in appearance. The suede of the product prepared by the process of the invention has a delicate and soft touch, similar to the silky and soft feel of plush, comfortable and warm.

[0163] In addition, the product prepared by the process of the present invention also has excellent tear resistance, indicating that it has good durability and longevity, and can maintain beauty and comfort for a long time. That is, the quality can be guaranteed whether it is facing daily wear and tear or years of use.

[0164] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. The production process of grain suede double-sided leather comprises the following steps: The wet blue leather is pre-treated to obtain leather, and the leather is sequentially retanned, neutralized, fat-liquored and filled before intermediate treatment; the leather after the intermediate treatment is then buffed; the characteristics are: The retanning comprises the following steps: adding water, fatliquor, formic acid, retanning filler, tannin and aluminum tanning agent into a rotary drum and rotating it; soaking after rotating it, adding sodium acetate and baking soda after soaking, rotating it, draining it, washing it with water and draining it; The neutralization comprises the following steps: adding water, neutralizing tannin, and baking soda into the drum, rotating, draining, washing with water, and then draining; The fat filling comprises the following steps: adding water, synthetic tanning agent, fatliquor, synthetic oil, emulsifier, mildew preventive, dispersing aid, and formic acid into the drum and rotating; draining, washing with water and then draining; In the retanning, 1% of the weight of the leather is added as a degreasing agent, 0.6% of the weight of the leather is added as formic acid, 4-6% of the weight of the leather is added as a retanning filler, 6-8% of the weight of the leather is added as tannin, 2-4% of the weight of the leather is added as an aluminum tanning agent, 2% of the weight of the leather is added as sodium acetate, and 0.3% of the weight of the leather is added as baking soda; in the retanning, the aluminum tanning agent is at least one of the aluminum tanning agent NOVALTAN AL of ZIEMA Chemical, the aluminum tanning agent DESOATENALF of Desail Chemical, TRUPOTAN ALP of Thomson Chemical, and UKATAN PRE of SCHILL+SEILACHER Chemical; The retanning filler is at least one of potassium chromium sulfate dodecahydrate RELATAN T.KAL and synthetic tanning agent UKATAN SLH of Cromo Chemicals; In the fat filling, 20% of the leather weight of synthetic tanning agent, 3% of the leather weight of fatliquor, 2% of the leather weight of synthetic oil, 0.5% of the leather weight of emulsifier, 0.05% of the leather weight of mildewproof agent, 1% of the leather weight of dispersing aid, and 3% of the leather weight of formic acid are added; In the fat filling, the synthetic tanning agent is at least one of the synthetic tanning agent RETENAL RCN-40 of Cromo Chemical, the synthetic tanning agent UKATAN SLH of SCHILL+SEILACHER Chemical, the synthetic tanning agent UKATAN INF of SCHILL+SEILACHER Chemical, and the synthetic tanning agent PELLITAN NS of REPICO Chemical; The fatliquor is at least one of the sulfated fatliquor FOSFOL 50 of CROMOGENIA Chemicals and the sulfonated fatliquor Lipsol h60 of SCHILL+SEILACHER Chemicals.

2. The process for producing grain suede double-sided leather according to claim 1, characterized in that: During the neutralization, 3% of the weight of the leather is added as neutralizing tannin, and 0.5% of the weight of the leather is added as baking soda.

3. The production process of grain suede double-sided leather according to claim 2, characterized in that: In the neutralization, the neutralized tannin is at least one of the neutralized tannin TANIGAN PAK N LIQ of LANXESS Chemicals, lead alkali of STAHL Chemicals, PELLUPUR MP3 / C of PULCRA Chemicals, and SELLASOL NG LIQ of TFL Chemicals.

4. The process for producing grain suede double-sided leather according to claim 1, characterized in that: The leather grinding comprises the following steps: controlling the moisture content of the leather to 20-30% and performing leather grinding; during the leather grinding process, a leather grinding machine is used to grind the suede surface of the leather for multiple times, and the hardness of the roller of the leather grinding machine is 18-20HA; Dust removal is carried out after each leather grinding.

5. The process for producing grain suede double-sided leather according to claim 4, characterized in that: The mesh number of the sandpaper used for each leather grinding is larger than the mesh number of the sandpaper used for the previous leather grinding.

6. The process for producing grain suede double-sided leather according to claim 5, characterized in that: After using the leather grinding machine to grind the leather, use the grinding wheel to grind the suede of the leather; after the grinding wheel is completed, dust is removed.