A method for preparing aircraft carbon / ceramic brake discs using waste carbon discs

High-density, wear-resistant carbon/ceramic brake discs are formed by high-temperature graphitization and composite treatment of carbon/ceramic materials on waste carbon discs, which solves the fluctuation of friction resistance of existing carbon/carbon brake discs in wet and dry conditions. problem, and effectively utilize waste resources, extending the service life and reducing production costs.

CN116751064BActive Publication Date: 2024-10-18YANTAI KAIBO COMPOSITE MATERIAL TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310698608.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-13
Publication Date
2024-10-18
Estimated Expiration
2043-06-13

AI Technical Summary

Technical Problem

The friction resistance of existing carbon/carbon materials in aircraft brake discs fluctuates greatly in wet and dry conditions, and waste carbon disc resources are not fully utilized, resulting in huge consumption and high costs.

Method used

By subjecting waste carbon discs to high-temperature graphitization to increase density, and preparing friction layers of carbon/ceramic materials on both sides of the middle layer, combined with CVI gas phase infiltration and siliconization treatments, a composite structure of carbon/ceramic brake discs is formed, and To repair keyway and surface defects on the surface, ultra-high temperature adhesive and short carbon fiber putty should be used for repair and coating.

Benefits of technology

It improves the density and wear resistance of the brake disc, reduces the wet decay rate and wear rate, extends the service life, shortens the production cycle, and reduces energy consumption and production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A method for preparing aircraft carbon / ceramic brake discs using waste carbon discs relates to the field of aircraft brake disc preparation. The preparation steps of the method include: placing the waste carbon disc in a high-temperature vacuum furnace, heating it to 1200°C under nitrogen protection, then heating it to 2200°C to 2400°C under argon protection for high-temperature graphitization treatment, keeping the temperature for 2 hours, cooling it to below 200°C and taking it out of the furnace; placing the obtained product in a vacuum furnace for CVI vapor infiltration deposition to increase the density to more than 1.78g / cm 3 , and obtain an intermediate layer; prepare friction layers on both sides of the intermediate layer to obtain a carbon / ceramic brake disc blank; and perform CVI gas phase infiltration to increase density and siliconization on the carbon / ceramic brake disc blank to obtain a carbon / ceramic brake disc. The aircraft carbon / ceramic brake disc prepared by the present invention has light weight and wear resistance, and the static friction coefficient is increased from 0.12 to 0.15 of the waste carbon disc to 0.25, the wet attenuation rate is reduced from 40% to less than 10%, the wear rate is reduced from 4‰ to less than 2‰, and the production cost is reduced by 40-50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of brake discs for aircraft, and more particularly to a method for preparing carbon / ceramic brake discs by utilizing waste carbon material brake discs. Background Art

[0002] High-speed aircraft are all equipped with brakes so that the aircraft can land safely. The brake discs used in the brakes used in existing aircraft are generally made of carbon / carbon materials. The carbon / carbon material brake discs (referred to as carbon discs) have good braking performance, but also have corresponding defects. For example, the friction resistance in dry and wet states has large fluctuations. In particular, the above-mentioned carbon discs are key and vulnerable consumable parts of aircraft, and the usage is huge. A large number of scrapped carbon discs are generated every year. At present, it is estimated that there are hundreds of thousands of waste carbon discs in stock in my country. Waste carbon discs contain a considerable proportion of carbon fiber filaments and are expensive. Therefore, how to utilize the above-mentioned waste carbon discs while improving the performance of the brake discs is still an unresolved problem. Solving this problem has economic and strategic significance for the development of national defense science and technology, resource conservation and many other aspects. Summary of the invention

[0003] The invention aims to disclose a method for preparing a carbon / ceramic brake disc for aircraft with good comprehensive performance by utilizing existing waste carbon discs.

[0004] The steps for implementing the method of using waste carbon discs to prepare aircraft carbon / ceramic brake discs of the present invention are:

[0005] a. Put the waste carbon plate into a high-temperature vacuum furnace, heat it to 1200℃ under nitrogen protection, then heat it to 2200℃~2400℃ under argon protection for high-temperature graphitization treatment, keep it warm for 2 hours, and cool it to below 200℃ before taking it out of the furnace;

[0006] b. Place the product obtained in step a into a vacuum furnace and perform CVI vapor infiltration deposition to increase the density to greater than 1.78 g / cm 3 , get the middle layer;

[0007] c. preparing friction layers on both sides of the middle layer to obtain a carbon / ceramic brake disc blank;

[0008] d. The carbon / ceramic brake disc blank is subjected to CVI vapor infiltration to increase density and siliconization to obtain a carbon / ceramic brake disc.

[0009] After the step a, the keyway and surface defects of the obtained product are repaired. The keyway repair process is: the carbon fiber prepreg cloth is pasted to the damaged part of the keyway of the waste carbon plate with an ultra-high temperature adhesive and then placed in an isostatic pressing furnace. After the temperature is increased to 80°C to 90°C at a heating rate of 1.2°C to 2.0°C / minute, it is pressurized to 1.8 to 2.5Mpa with nitrogen, and the temperature is continued to be increased to 180°C to 200°C. The temperature and pressure are kept for 1 to 2 hours, and the product is cooled with the furnace. The surface defects are repaired by coating the surface with short carbon fiber putty to make it smooth, and then high-temperature treatment is performed at 1600°C.

[0010] The composition of the ultra-high temperature adhesive is calculated by weight percentage: 5-12% silicon powder, 3-5% aluminum powder, 5-10% titanium oxide powder, 5-8% boron nitride powder, and the remainder is thermosetting phenolic resin, and the sum of the contents of each component is 100%; the composition of the short carbon fiber putty is calculated by weight percentage: 25-35% thermosetting phenolic resin, 20-30% graphite powder, 10-15% silicon powder, 3-5% titanium oxide powder, 2-4% zirconium oxide and 15-25% chopped carbon fiber, and the length of the chopped carbon fiber is 2-10 mm.

[0011] The preparation process steps of the friction layer are: coating an ultra-high temperature adhesive on the surface of the middle layer, pasting the carbon / carbon plate on the two surfaces of the middle layer, placing it in an isostatic pressing furnace after compaction, evacuating the furnace, raising the thermometer to 70°C to 90°C at a heating rate of 1°C to 2°C / minute, pressurizing it with nitrogen to a pressure of 1.5 to 2.6 MPa, and then continuing to raise the temperature to 180°C to 200°C, keeping the temperature and pressure for 2 hours, and cooling it with the furnace to obtain a brake disc blank; or the preparation process steps of the friction layer are: coating the ultra-high temperature adhesive on the surface of the middle layer, pasting the carbon fiber prefabricated board on the two surfaces of the middle layer, placing it on a flat hot press for hot pressing, the molding pressure is 5 to 10 MPa, the pressing mold temperature is 100°C to 200°C, and then subjected to a high temperature treatment of 1600°C to 1800°C, and cooling to obtain a brake disc blank.

[0012] In the step d, the process requirements for increasing the density by CVI gas infiltration are: placing the brake disc blank into a vacuum furnace, inputting natural gas, heating it to 1000°C~1040°C, the pressure in the furnace is 3000~6000Pa, and depositing it for 200~400 hours; the siliconizing treatment is: placing the carbon / ceramic brake disc blank with increased density into a vacuum furnace, embedding the carbon / ceramic brake disc blank with silicon powder, increasing the temperature to 1450°C~1700°C, the siliconizing time is 1.5~2.5 hours, and then cooling it down and taking it out of the furnace to obtain a carbon / ceramic brake disc.

[0013] An anti-oxidation coating is prepared on the non-friction surface of the carbon / ceramic brake disc, and the anti-oxidation coating consists of a base layer and a sealing layer.

[0014] The components and preparation method of the base layer are as follows: 15-17% silicon powder, 10-20% aluminum powder, 35-45% water-soluble phenolic resin, 10-14% urea and 4-8% titanium oxide powder are mixed by weight to obtain a base slurry, the base slurry is applied to the non-friction surface of the carbon / ceramic brake disc, and the base layer is obtained by sintering at a high temperature of 1600°C in a high-temperature furnace.

[0015] The preparation method of the components of the sealing layer is as follows: 30-40% of boric acid, 20-30% of aluminum dihydrogen phosphate, 16-20% of silica sol, 9-13% of graphite powder and 6-9% of boron carbide are mixed by weight to obtain a sealing slurry, the sealing slurry is coated on the surface of the base layer, and the sealing layer is obtained by high-temperature treatment at 600°C in a high-temperature furnace.

[0016] The above technical scheme disclosed in the present invention provides a multi-layer composite carbon / ceramic brake disc using a waste carbon disc as an intermediate layer and carbon / ceramic friction layers on both sides. The carbon / ceramic brake disc prepared by the above preparation method has a higher density than the original carbon / carbon brake disc, but is 10-20% lower than the density of the ceramic brake disc of the original technology. It has light weight and wear resistance. The static friction coefficient is increased from 0.12-0.15 of the waste carbon disc to 0.25, the wet attenuation rate is reduced from 40% to less than 10%, the wear rate is reduced from 4‰ to less than 2‰, the service life of the brake disc is increased from 400-800 times to more than 1000 times, the production preparation cycle is shortened from 4-5 months to 2-2.5 months, the production efficiency is doubled while saving a lot of energy, and the production cost is reduced by 40-50%. DETAILED DESCRIPTION

[0017] A detailed description of specific embodiments of the present invention is given below. It should be particularly pointed out that the description of the specific embodiments of the present invention is for the purpose of facilitating a comprehensive understanding of the technology of the present invention and should not be regarded as limiting the scope of protection of the claims of the present invention.

[0018] The technical solution for implementing the specific embodiment of the present invention is that a method for preparing aircraft carbon / ceramic brake discs using waste carbon discs comprises the following steps:

[0019] a. Place the waste carbon plate in a high-temperature furnace, heat it to 1200℃ under nitrogen protection, then heat it to 2200℃~2400℃ under argon protection for high-temperature graphitization treatment, keep it at this temperature for 2 hours, and then cool it to below 200℃ and take it out of the furnace;

[0020] b. Place the product obtained in step a into a vacuum furnace and perform CVI vapor infiltration deposition to increase the density to greater than 1.78 g / cm 3 , get the middle layer;

[0021] c. preparing friction layers on both sides of the middle layer to obtain a carbon / ceramic brake disc blank;

[0022] d. The carbon / ceramic brake disc blank is subjected to CVI vapor infiltration to increase density and siliconization to obtain a carbon / ceramic brake disc.

[0023] In the above technical solution, after step a, the carbon structure in the waste carbon plate is graphitized in an orderly manner at a very high temperature, so that the structural strength of the waste carbon plate is greatly improved, and under the protection of a specific argon gas, the reaction at a very high temperature is avoided. In step b, the product obtained in step a is subjected to CVI vapor infiltration deposition carbon, so that the density of the product is increased to a density greater than 1.78g / cm 3 This density is greater than the average density of the original carbon plate when it leaves the factory (1.75g / cm 3 ) Index: Through step C, friction layers are formed on both sides of the middle layer, and the friction layers are carbon / ceramic materials, so as to obtain a carbon / ceramic brake disc blank with a composite structure. In step c, the carbon / ceramic brake disc blank is first subjected to CVI gas phase infiltration to increase the density, so that the density of the friction layer is greater than 1.5g / cm 3 The carbon / ceramic brake disc blank is then siliconized to obtain a surface layer containing SiC on the friction layer surface. The density of the surface layer is greater than 1.9 g / cm 3 When the siliconizing time is sufficient, the friction layer is entirely infiltrated by silicon, and the friction layer entirely contains SiC, and finally the carbon / ceramic brake disc of the present invention is obtained.

[0024] When the waste carbon disc is assembled on the original brake device, it has the original slot key structure, which may be damaged during long-term use, or the friction surface of the waste carbon disc contains defects, such as holes, pits, missing meat or tiny cracks, etc. Therefore, when preparing the brake disc of the present invention, the waste carbon disc needs to be repaired to facilitate assembly during subsequent use. The above-mentioned repair method is: use ultra-high temperature adhesive to stick carbon fiber prepreg cloth to the damaged part of the keyway of the waste carbon plate and then place it in an isostatic pressing furnace. The carbon fiber prepreg cloth is made by impregnating the carbon fiber cloth in an impregnation liquid. The composition of the impregnation liquid is 50% phenolic resin and 5% alcohol by weight. The impregnation liquid has a high carbon content and good fluidity and permeability; after heating to 80℃~90℃ at a heating rate of 1.2℃~2.0℃ / minute, pressurize it with nitrogen to 1.8~2.5Mpa, continue to heat to 180℃~200℃, keep warm and pressurized for 1~2h, and cool it to room temperature with the furnace and take it out of the furnace. If the surface defects mentioned above exist on the surface of the waste carbon plate, it also needs to be repaired. The modification is to use short-cut carbon fiber putty to coat the surface flat, and then perform high-temperature heat treatment at 1600℃. The composition of the above-mentioned ultra-high temperature adhesive is calculated by weight percentage: 5-12% silicon powder, 3-5% aluminum powder, 5-10% titanium oxide powder, 5-8% boron nitride powder, and the balance is thermosetting phenolic resin, and the sum of the contents of each component is 100%. After high-temperature treatment, the ultra-high temperature adhesive forms a carbon / ceramic structure layer containing ceramic components, which has good structural strength at high temperatures, as well as good wear resistance and thermal conductivity. The composition of the above-mentioned chopped carbon fiber putty is calculated by weight percentage: 25-35% thermosetting phenolic resin, 20-30% graphite powder, 10-15% silicon powder, 3-5% titanium oxide powder, 2-4% zirconium oxide powder and 15-25% chopped carbon fiber, and the length of the chopped carbon fiber is 2-10 mm. The chopped carbon fiber putty forms a carbon / ceramic material after high temperature treatment, which has excellent compatibility with the carbon / carbon material of the original waste carbon tray, including density, heat conduction and strength.

[0025] The process conditions of step b are as follows: placing the product of step a in a vacuum furnace, using natural gas as the carbon source, under the conditions of furnace pressure of 3000-6000 Pa and furnace temperature of 1000°C-1040°C, the infiltration time is 200-400 hours, until the density is greater than 1.78 g / cm 3 Through the above-mentioned process steps of increasing the density of the waste carbon disc, the key is to repair the carbon loss and possible internal micro cracks of the waste carbon disc during long-term use, and on the other hand, increase the density of the thinner waste carbon disc, especially the increased density can reach the center of the waste carbon disc, and finally greatly improve the comprehensive performance of the waste carbon disc such as strength and thermal conductivity.

[0026] The step c is to prepare friction layers on both sides of the middle layer, which can make the brake disc not only meet the thickness requirements of the brake device, but also make the brake disc have better friction resistance on both sides. The preparation process steps of the friction layer are: coating the surface of the middle layer with ultra-high temperature adhesive, pasting the carbon / carbon plate on the two surfaces of the middle layer, and placing it in an isostatic pressing furnace after compaction. The furnace is evacuated, and the thermometer is raised to 70°C to 90°C at a heating rate of 1°C to 2°C / minute. Then, it is pressurized with nitrogen to a pressure of 1.5 to 2.6Mpa, and then the temperature is continued to be raised to 180°C to 200°C, and the heat and pressure are kept for 2 hours, and the brake disc blank is obtained by cooling with the furnace. Alternatively, the process steps for preparing the friction layer are: after coating the surface of the intermediate layer with ultra-high temperature adhesive, the carbon fiber prefabricated board is pasted on the two surfaces of the intermediate layer, and is placed on a flat hot press for hot pressing, the molding pressure is 5-10Mpa, the pressing mold temperature is 100℃-200℃, and then subjected to high temperature treatment at 1600℃-1800℃, and the brake disc blank can also be obtained. The thickness of the above-mentioned carbon / carbon plate and carbon fiber prefabricated board is selected so that the thickness of the entire brake disc meets the original technical requirements of the brake device, and the preferred thickness is 1.5-2.5mm to ensure the long-term use of the friction layer. The composition of the ultra-high temperature adhesive has been described above. In the above two process steps, the ultra-high temperature adhesive can penetrate into the interior of the carbon / carbon plate and the carbon fiber prefabricated board under the pressure in the process steps, so that the friction layer of the brake disc contains ceramic components after high temperature treatment, that is, the friction layer as a whole has been presented as a carbon / ceramic material with good wear resistance and oxidation resistance.

[0027] In order to further improve the performance of the brake disc, in the step d, the process requirements for increasing the density of the carbon / ceramic brake disc blank by CVI gas phase infiltration are as follows: the brake disc blank is placed in a vacuum furnace, natural gas is input, the temperature is raised to 1000℃~1040℃, the pressure in the furnace is 3000~6000Pa, and the deposition is carried out for 200~400 hours, so that the density of the friction layer is greater than 1.5g / cm 3 . The above steps further increase the carbon content of the friction layer and improve the strength of the friction layer. Then, the carbon / ceramic brake disc blank with increased density is placed in a vacuum furnace and siliconized using the RMI (reaction melt infiltration) method of the prior art, that is, the carbon / carbon brake disc blank is embedded with silicon powder, the temperature is increased to 1450℃~1700℃, the siliconization time is 1.5~2.5 hours, and then the temperature is lowered and taken out of the furnace. The friction layer contains C / SiC and the density of the friction layer is greater than 1.9g / cm 3In the above process, the molten silicon can not only penetrate into the friction layer, but also part of the silicon can penetrate into the intermediate layer, and at high temperature, the entire brake disc blank can undergo a high temperature reaction again, so that the overall structural strength and the connection strength between the layers are further improved, and finally the brake disc of the present invention is obtained. Structurally, the brake disc has a high-density carbon / carbon intermediate layer and a friction layer of carbon / ceramic material on both sides to form a composite structure brake disc. From the perspective of the entire preparation process of the friction layer, the friction layer is based on a carbon / carbon plate or a carbon fiber prefabricated plate as a skeleton, containing carbon materials and a variety of ceramic components, so that the friction layer has good antioxidant properties, excellent friction resistance and comprehensive performance. From the perspective of density, although the friction layer contains a large amount of ceramic components, the density (greater than 1.9g / cm 3 ) is greater than the density of traditional carbon / carbon brake discs, but because the middle layer occupies a larger proportion in the carbon / ceramic brake disc of the present invention, the average density of the entire carbon / ceramic brake disc is ultimately slightly greater than that of traditional carbon / carbon brake discs, and the average density is much lower than that of expensive traditional ceramic brake discs. Therefore, comprehensively speaking, the carbon / ceramic brake disc of the present invention has the dual advantages of carbon / carbon brake discs and ceramic brake discs, and has the advantages of good heat transfer, light weight, excellent friction resistance and antioxidant properties. In particular, the use of waste carbon / carbon brake discs as the middle layer saves a large amount of carbon fiber materials, and combined with the unique process steps, a large amount of energy in the preparation process is saved, so that the present invention has the advantages of low price and long life.

[0028] The carbon / ceramic brake disc of the present invention has achieved the purpose of the present invention and can be directly set in the brake device of the aircraft as a dynamic disc or / and a static disc. During long-term use, the huge braking energy will cause the carbon / ceramic brake disc to be repeatedly exposed to a high temperature. The high temperature makes the non-friction surface of the carbon / ceramic brake disc (and the outer surface of the annular ring of the brake disc) easy to oxidize and corrode the brake disc, affecting the service life of the carbon / ceramic brake disc. Therefore, in order to further improve the performance and service life of the carbon / ceramic brake disc, an anti-oxidation coating is prepared on the non-friction surface of the carbon / ceramic brake disc. The anti-oxidation layer is composed of a base layer and a sealing layer. The components and preparation method of the base layer are as follows: A base slurry is obtained by mixing 15-17% silicon powder, 10-20% aluminum powder, 35-45% water-soluble phenolic resin, 10-14% urea and 4-8% titanium oxide powder in a ratio of 15-17%. After the base slurry is applied to the non-friction surface of the carbon / ceramic brake disc, it is sintered at 1600°C in a high-temperature furnace to obtain a base layer; the composition and preparation steps of the sealing layer are: a sealing slurry is obtained by mixing 30-40% boric acid, 20-30% aluminum dihydrogen phosphate, 16-20% silica sol, 9-13% graphite powder, and 6-9% boron carbide aqueous solution in weight percentage. After the sealing slurry is applied to the surface of the base layer, it is subjected to a high-temperature treatment of 600°C in a high-temperature furnace to obtain a sealing layer. The above-mentioned specific base layer has good adaptability and connection performance with the brake disc, and the sealing layer has good isolation performance for the base layer, so that the anti-oxidation coating can isolate oxygen and protect the non-friction surface of the carbon / ceramic brake disc at high temperature, which can further improve the service life of the carbon / ceramic brake disc.

[0029] After the above-mentioned brake disc is assembled in the brake device, in actual use, there is a large radial force between the middle layer and the friction layer in the brake disc. In long-term use, the interface between the layers may produce a small dislocation or a small crack, which may affect the service life of the brake disc. Therefore, after step b of the above-mentioned preparation process, multiple protrusions are formed on the two surfaces of the middle layer. In step c, the multiple protrusions will be squeezed and embedded in the friction layer to form a tight fit. On the one hand, the multiple protrusions will prevent the possibility of relative displacement between the friction layer and the middle layer, and on the other hand, increase the total contact area between the middle layer and the friction layer, thereby further improving the connection strength between the middle layer and the friction layer, so that the service life of the brake disc is further improved. The cross-sectional shape of the above-mentioned protrusions is preferably circular, and the multiple protrusions are symmetrically distributed on the surface of the middle layer to evenly distribute the force. The height of the above-mentioned protrusions can be selected so as not to affect the performance of the friction layer. The preferred height of the protrusions is 1 / 3 to 1 / 4 of the thickness of the friction layer.

Claims

1. A method for preparing aircraft carbon / ceramic brake discs using waste carbon discs, characterized in that The preparation steps of the method are: a. Put the waste carbon plate into a high-temperature vacuum furnace, heat it to 1200℃ under nitrogen protection, then heat it to 2200℃~2400℃ under argon protection for high-temperature graphitization treatment, keep it warm for 2 hours, and cool it to below 200℃ before taking it out of the furnace; b. Place the product obtained in step a into a vacuum furnace and perform CVI vapor infiltration deposition to increase the density to greater than 1.78 g / cm 3 , get the middle layer; c. preparing friction layers on both sides of the middle layer, and bonding the middle layer and the friction layer with an ultra-high temperature adhesive to obtain a carbon / ceramic brake disc blank; The preparation process of the friction layer is as follows: coating an ultra-high temperature adhesive on the surface of the middle layer, pasting the carbon / carbon plate on the two surfaces of the middle layer, placing it in an isostatic pressing furnace after compaction, evacuating the furnace, raising the temperature to 70°C to 90°C at a heating rate of 1°C to 2°C / min, pressurizing with nitrogen to a pressure of 1.5 to 2.6 MPa, and then continuing to raise the temperature to 180°C to 200°C, keeping the temperature and pressure for 2 hours, and cooling with the furnace to obtain a brake disc blank; or The preparation process steps of the friction layer are as follows: after coating the surface of the middle layer with an ultra-high temperature adhesive, the carbon fiber prefabricated plate is pasted on the two surfaces of the middle layer, and is placed on a flat hot press for hot pressing, the molding pressure is 5-10MPa, the pressing mold temperature is 100℃-200℃, and then subjected to high temperature treatment at 1600℃-1800℃, and after cooling, a brake disc blank is obtained; d. Perform CVI gas infiltration to increase density and siliconize the carbon / ceramic brake disc blank to obtain a carbon / ceramic brake disc; The composition of the ultra-high temperature adhesive is as follows by weight percentage: 5-12% silicon powder, 3-5% aluminum powder, 5-10% titanium oxide powder, 5-8% boron nitride powder, and the remainder is thermosetting phenolic resin, and the sum of the contents of each component is 100%.

2. The method for preparing aircraft carbon / ceramic brake discs using waste carbon discs according to claim 1, characterized in that After step a, the keyway and surface defects of the obtained product are repaired. The keyway repair process is: the carbon fiber prepreg cloth is pasted on the damaged part of the keyway of the waste carbon plate with an ultra-high temperature adhesive and then placed in an isostatic pressing furnace. After the temperature is increased by 80°C to 90°C at a heating rate of 1.2°C to 2.0°C / minute, it is pressurized to 1.8 to 2.5MPa with nitrogen, and the temperature is continued to be increased to 180°C to 200°C. The temperature and pressure are kept for 1 to 2 hours, and the furnace is cooled; the surface defects are repaired by coating the surface with short carbon fiber putty and then performing high-temperature treatment at 1600°C.

3. The method for preparing aircraft carbon / ceramic brake discs using waste carbon discs according to claim 2, characterized in that: The composition of the short carbon fiber putty is as follows by weight percentage: 25-35% of thermosetting phenolic resin, 20-30% of graphite powder, 10-15% of silicon powder, 3-5% of titanium oxide powder, 2-4% of zirconium oxide powder and 15-25% of short carbon fiber, and the length of the short carbon fiber is 2-10 mm.

4. The method for preparing aircraft carbon / ceramic brake discs using waste carbon discs according to claim 1, characterized in that: In the step d, the process requirements for increasing density by CVI gas phase infiltration are: placing the brake disc blank into a vacuum furnace, inputting natural gas, heating to 1000°C to 1400°C, the pressure in the furnace is 3000 to 6000 Pa, and depositing for 200 to 400 hours; The siliconizing treatment is as follows: placing the carbon / ceramic brake disc blank with increased density into a vacuum furnace, embedding the carbon / ceramic brake disc blank with silicon powder, increasing the temperature to 1450°C to 1700°C, siliconizing time for 1.5 to 2.5 hours, then cooling down and taking out of the furnace to obtain the carbon / ceramic brake disc.

5. The method for preparing aircraft carbon / ceramic brake discs using waste carbon discs according to claim 1, characterized in that: An anti-oxidation coating is prepared on the non-friction surface of the carbon / ceramic brake disc, and the anti-oxidation coating consists of a base layer and a sealing layer.

6. The method for preparing aircraft carbon / ceramic brake discs using waste carbon discs according to claim 5, characterized in that: The components and preparation method of the base layer are as follows: 15-17% silicon powder, 10-20% aluminum powder, 35-45% water-soluble phenolic resin, 10-14% urea and 4-8% titanium oxide powder are mixed by weight to obtain a base slurry, the base slurry is applied to the non-friction surface of the carbon / ceramic brake disc, and the base layer is obtained by sintering at a high temperature of 1600°C in a high-temperature furnace.

7. The method for preparing aircraft carbon / ceramic brake discs using waste carbon discs according to claim 5, characterized in that: The preparation method of the components of the sealing layer is as follows: 30-40% boric acid, 20-30% aluminum dihydrogen phosphate, 16-20% silica sol, 9-13% graphite powder, and 6-9% boron carbide aqueous solution are mixed to obtain a sealing slurry, the sealing slurry is coated on the surface of the base layer, and the sealing layer is obtained by high-temperature treatment at 600°C in a high-temperature furnace.

8. The method for preparing aircraft carbon / ceramic brake discs using waste carbon discs according to any one of claims 1 to 7, characterized in that: The two surfaces of the intermediate layer are provided with a plurality of protrusions, which are squeezed and embedded into the friction layer to form a tight fit.

Citation Information

Patent Citations

  • Carbon material brake disc made of waste carbon material disc and used for airplane and preparation method of carbon material brake disc

    CN115353406A

  • Composite-structure lightweight ceramic brake disc and preparation method thereof

    CN115385711A

  • Carbon / ceramic brake disc with sandwich structure

    CN115823151A