A pickling method for chromium stainless steel discs
By optimizing the pickling process of chromium stainless steel wire rods, and using a mixture of hydrochloric acid and hydrofluoric acid, along with low-toxicity corrosion inhibitors dodecylamine polyoxyethylene ether and hexamethylenetetramine solution, the problems of unstable quality and highly toxic corrosion inhibitors in the existing process were solved, achieving low-cost and efficient pickling results.
Patent Information
- Application Number
- CN202310694660.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-12
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-06-12
AI Technical Summary
The existing pickling process for chromium stainless steel discs has problems such as unstable quality, untimely matching of pickling process after product development and changes in annealing process, inability to effectively pickle some products, high pickling cost, and the use of highly toxic or extremely toxic chemical reagents as corrosion inhibitors.
The oxide scale of chromium stainless steel wire rods was removed by using a hydrochloric acid-hydrofluoric acid mixture at 80℃~85℃. A non-toxic or low-toxic dodecylamine polyoxyethylene ether and hexamethylenetetramine mixture was used as a corrosion inhibitor for passivation, cleaning, neutralization, rust prevention treatment and drying. The pickling solution preparation and testing process were optimized.
It reduces pickling costs, meets the needs of capacity expansion, improves pickling effect, reduces pickling defects and loss rate, and uses non-toxic or low-toxic corrosion inhibitors to achieve a more stable pickling process.
Smart Images

Figure CN116752147B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal pickling technology, and specifically relates to a pickling method for chromium stainless steel discs. Background Technology
[0002] Currently, existing pickling lines for chromium stainless steel discs use an HCl+HF+corrosion inhibitor+neutralization+passivation process. However, this process does not meet the needs of future capacity expansion, and suffers from inconsistent quality and variety requirements. Furthermore, the pickling process is not timely in response to changes in new product development and annealing processes. Moreover, some varieties (102Cr17Mo, 416, 6Cr13Mo, etc.) cannot be effectively pickled using existing processes, resulting in pickling costs significantly higher than those of competitors. To address these issues, optimization of the existing process is urgently needed. Currently, stainless steel disc pickling commonly employs processes such as H2SO4 pre-washing—HF+HNO3 mixed acid pickling, and HF+HCl+corrosion inhibitor mixed acid pickling. In the HF+HCl process, a corrosion inhibitor must be added, but these inhibitors are generally highly toxic or extremely toxic chemicals, and there are no specific usage methods. Summary of the Invention
[0003] To address at least one of the problems in the background art, the present invention proposes a pickling method for chromium stainless steel discs.
[0004] To achieve the above objectives, the present invention adopts the following technical solution:
[0005] A method for pickling chromium stainless steel discs includes the following steps:
[0006] The chromium stainless steel wire rod is placed in the pickling solution and the oxide scale is washed off with a hydrochloric acid-hydrofluoric acid mixture at the target temperature. Then, the residual hydrochloric acid-hydrofluoric acid solution and corrosion inhibitor are washed off with water. Finally, the wire rod is passivated, cleaned, neutralized, treated with rust prevention solution and dried.
[0007] Preferably, the corrosion inhibitor is a mixed solution of dodecylamine polyoxyethylene ether and hexamethylenetetramine.
[0008] Preferably, the target temperature is 80℃~85℃.
[0009] Preferably, the passivation process includes the following steps:
[0010] Passivation is performed in nitric acid solution for 1–2 minutes.
[0011] Preferably, the cleaning process after passivation includes the following steps:
[0012] Immerse the chromium stainless steel disc in the cleaning tank for 0.5-1 minute;
[0013] Use a water gun to clean the chromium stainless steel disc until there is no black ash adhering to the surface of the chromium stainless steel disc.
[0014] Preferably, the neutralization process includes the following steps:
[0015] The residual acid in chromium stainless steel wire rods was neutralized in a sodium carbonate solution at a temperature of 70-80℃ when the pH was ≥12.
[0016] Preferably, the rust inhibitor treatment includes the following steps:
[0017] Immerse the chromium stainless steel coil in a rust-preventive solution at a temperature of 70℃~80℃ for 20~30 seconds.
[0018] Preferably, the drying process includes the following steps:
[0019] Bake at 100℃ for 4–6 minutes.
[0020] Preferably, the preparation of the pickling solution includes the following steps:
[0021] Add water and hydrochloric acid to the pickling tank, turn on the circulation pump to stir, then add hydrofluoric acid, then heat to 75-80℃, then add dodecylamine polyoxyethylene ether and hexamethylenetetramine solution, and finally complete the preparation of the slow-release agent.
[0022] The volume ratio of the water, hydrochloric acid, hydrofluoric acid, dodecylamine polyoxyethylene ether, and hexamethylenetetramine solution is (771-840):(1078-1155):(462-539):(1-1.5):(50-100).
[0023] Preferably, the method also includes periodically sampling the pickling solution to detect the concentrations of hydrogen ions, fluoride ions, and iron ions in the pickling solution.
[0024] The beneficial effects of this invention are:
[0025] 1. This invention prepares a new corrosion inhibitor for pickling chromium stainless steel discs. Specifically, it uses non-toxic or low-toxic dodecylamine polyoxyethylene ether (1210), hexamethylenetetramine, hydrochloric acid and hydrofluoric acid. The resulting corrosion inhibitor greatly reduces costs in practical applications.
[0026] 2. The corrosion inhibitor of the present invention has optimized the raw materials to meet the needs of capacity expansion.
[0027] Other features and advantages of the invention will be set forth in the following description, and will be apparent in part from the description, or may be learned by practicing the invention. The objects and other advantages of the invention may be realized and obtained by means of the structures pointed out in the description and the drawings. Attached Figure Description
[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0029] Figure 1 A schematic flowchart of a pickling method for chromium stainless steel discs according to the present invention is shown. Detailed Implementation
[0030] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0031] A method for pickling chromium stainless steel discs, such as Figure 1 As shown, it includes the following steps:
[0032] The chromium stainless steel wire rod is placed in the pickling solution and cleaned with a hydrochloric acid-hydrofluoric acid mixture at the target temperature (80℃~85℃). Then, the residual hydrochloric acid-hydrofluoric acid solution and corrosion inhibitor are washed off with water. Finally, passivation, cleaning, neutralization, rust prevention treatment and drying are carried out in sequence.
[0033] It should be noted that the corrosion inhibitor is a mixed solution of dodecylamine polyoxyethylene ether and hexamethylenetetramine. Moreover, the mass fraction (1210) of dodecylamine polyoxyethylene ether is ≥99%, and the concentration of hexamethylenetetramine is 250 g / L.
[0034] It should be further noted that in the pickling method of chromium stainless steel discs, the mass fraction of hydrochloric acid is 33%, the mass fraction of hydrofluoric acid is 45%, and the mass fraction of nitric acid used for passivation is 60%.
[0035] Furthermore, an acid pickling solution generally needs to be prepared before pickling, and the preparation process is as follows:
[0036] Add water and hydrochloric acid to the pickling tank, turn on the circulation pump to stir, then add hydrofluoric acid, then heat to 75-80℃, then add dodecylamine polyoxyethylene ether and hexamethylenetetramine solution, and finally complete the preparation of the slow-release agent.
[0037] The volume ratio of water, hydrochloric acid, hydrofluoric acid, dodecylamine polyoxyethylene ether, and hexamethylenetetramine solution is (771-840): (1078-1155): (462-539): (1-1.5): (50-100).
[0038] It should be noted that, in one embodiment, the pickling tank is 2.2m wide, 7.0m long and 2.0m high, the water height is 55-60cm, the hydrochloric acid height is 70-75cm, the hydrofluoric acid height is 25-35cm, the volume of dodecylamine polyoxyethylene ether (1210) is 10-15L and the volume of hexamethylenetetramine is 300-1000L.
[0039] It should be further explained that the preparation of the pickling solution of the present invention differs from that of the original pickling solution in the following ways: First, the corrosion inhibitor is different; the corrosion inhibitor in the original pickling solution belongs to Beite Company. Second, the proportion of hydrofluoric acid in the pickling solution is 1.5 to 2.5 times that of the original pickling solution. The resulting effect is that it can directly pickle 410, 30Cr13, 40Cr13, 50Cr13, 6Cr13Mo, 102Cr17Mo, 8Cr17Mo, BJC003, 416, 420F1 and other wire rods with a low pickling loss rate. After the oxide scale is removed by pickling, pickling continues for 4 to 6 hours, and the pickling loss rate is less than 2%. Even if the pickling equipment malfunctions during the pickling process, the wire rods can still be soaked in the pickling tank for 4 to 6 hours without any pickling defects on the surface. The original pickling solution cannot directly wash high carbon steels and free-cutting steels such as 6Cr13Mo, 102Cr17Mo, 8Cr17Mo, BJC003, 416, and 420F1. The pickling loss rate is usually greater than 2%, and the pickling time exceeds 60 minutes, resulting in pickling defects.
[0040] Furthermore, in the pickling process of this invention, when the temperature is 75-80℃, the coils are lowered into the water and pickled while the temperature is increased. The pickling temperature is controlled at 80-85℃. According to the steel grade and pickling temperature, the pickling time is specified in Table 1. After pickling for a period of time, the coils are taken out of the pickling solution and observed to see if they are clean. If they are not clean, pickling continues. If they are clean, subsequent cleaning, passivation, rinsing, neutralization, rust prevention, and drying are carried out.
[0041] Table 1: Pickling Time Reference Table
[0042]
[0043] Furthermore, before passivation, rinsing is generally performed, specifically by soaking the tank in water for 2-3 minutes. Water is then added by overflow, and after one tank of acid is used up, it is drained and refilled.
[0044] Furthermore, the passivation process is carried out using a (1+1) nitric acid solution (65% nitric acid to water in a volume ratio of 1:1) for 1 to 2 minutes.
[0045] Furthermore, when cleaning after passivation, the chromium stainless steel disc needs to be soaked in the cleaning tank for 0.5-1 minute, and then cleaned with a water gun for more than 5 minutes at a water pressure of 1.5 MPa until there is no black ash adhering to the surface of the chromium stainless steel disc.
[0046] Further, neutralization is carried out, including the following steps:
[0047] The residual acid in chromium stainless steel wire rods was neutralized in a sodium carbonate solution at a temperature of 70-80℃ when the pH was ≥12.
[0048] Further, rust inhibitor treatment is performed, including the following steps:
[0049] Immerse the chromium stainless steel coil in a rust-inhibiting solution at 70-80℃ for 20-30 seconds. The rust-inhibiting solution is a commercially available, standard product.
[0050] Further, drying is carried out, including the following steps:
[0051] Bake at 100℃ for 4–6 minutes.
[0052] Furthermore, this invention also requires periodically sampling the pickling solution to detect the concentrations of hydrogen ions, fluoride ions, and iron ions in the pickling solution. Specifically, 300-500 ml of pickling solution is taken every morning from 7:00 to 8:00, and then the total hydrogen ion concentration (total acidity) is measured in mol / L, the total fluoride ion concentration is measured in mol / L, and the iron ion concentration is measured in mg / ml.
[0053] It should be noted that after testing the total acidity of the pickling solution, hydrochloric acid, hydrofluoric acid, and corrosion inhibitors can be added according to the concentration of each ion. Taking a pickling tank with a width of 2.2m, a length of 7.0m, and a height of 2.0m as an example, the following steps are included:
[0054] When the total acidity of the pickling tank is 3-4 mol / L, add hydrochloric acid (33% by mass) to the height of the liquid level (15-30 cm) during the morning and evening shifts.
[0055] When the total fluoride ion concentration is <2 mol / L, add 1000 L of hydrofluoric acid.
[0056] When the total acidity is <2 mol / L, drain the acid solution with a height of 50-60 cm, add hydrochloric acid (mass fraction 33%) with a height of 50 cm, add 1000 L of hydrofluoric acid, and 200 L (250 g / L) of hexamethylenetetramine solution.
[0057] When the iron ion concentration in the acid solution is ≥200mg / ml, the total acidity is <2mol / L, and the total fluoride ion concentration is <2mol / L, stop the acid washing, drain the acid washing solution, and clean the acid tank.
[0058] It should be noted that this pickling method was first used on January 21, 2022, for pickling chromium stainless steel wire rods in a certain region. The monthly pickling volume of various specifications of 30Cr13, 410, 40Cr13, 50Cr13, 6Cr13Mo, 102Cr17Mo, BCJ003, 8Cr17Mo, 416, and 420F1 chromium stainless steel wire rods is 2000-2500 tons. The pickling time for 30Cr13, 410, 40Cr13, and 50Cr13 wire rods is 30-50 minutes; for 6Cr13Mo, it is 40-60 minutes; for 102Cr17Mo, BCJ003, and 8Cr17Mo, it is 60-80 minutes; and for 416 and 420F1, it is 20-30 minutes. The pickling temperature is 82-86℃. In 2022, the pickling method of this invention was used to pickle 410, 30Cr13, 40Cr13, 50Cr13, 6Cr13Mo, 102Cr17Mo, 8Cr17Mo, BJC003, 416, and 420F1, with an average cost of 160 yuan / ton. In 2021, Beite Company was responsible for pickling, and the average pickling cost for 410, 30Cr13, 40Cr13, and 50Cr13 was 160 yuan / ton. Direct pickling of 6Cr13Mo, 102Cr17Mo, 8Cr17Mo, BJC003, 416, and 420F1 did not remove the oxide scale; they required alkaline explosion before pickling. The alkaline explosion cost 400 yuan / ton, and the pickling cost was greater than 500 yuan / ton.
[0059] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method of pickling chromium stainless disc rounds, characterized by, Includes the following steps: The chromium stainless steel wire rod is placed in the pickling solution. At the target temperature, the oxide scale of the chromium stainless steel wire rod is washed off with a mixture of hydrochloric acid and hydrofluoric acid. Then, the residual hydrochloric acid-hydrofluoric acid solution and corrosion inhibitor on the wire rod are washed off with water. Then, passivation, cleaning, neutralization, rust prevention treatment and drying are carried out in sequence. The corrosion inhibitor is a mixed solution of dodecylamine polyoxyethylene ether and hexamethylenetetramine; The target temperature is 80℃~85℃; The preparation of the pickling solution includes the following steps: Add water and hydrochloric acid to the pickling tank, turn on the circulation pump to stir, then add hydrofluoric acid, then heat to 75-80℃, and then add dodecylamine polyoxyethylene ether and hexamethylenetetramine solution; the volume ratio of water, hydrochloric acid, hydrofluoric acid, dodecylamine polyoxyethylene ether and hexamethylenetetramine solution is (771-840): (1078-1155): (462-539): (1-1.5): (50-100).
2. A method of pickling chromium stainless disc circles according to claim 1, characterized in that, The passivation process includes the following steps: Passivation is performed in nitric acid solution for 1-2 minutes.
3. The pickling method for chromium stainless steel discs according to claim 1, characterized in that, The cleaning process following passivation includes the following steps: Immerse the chromium stainless steel disc in the cleaning tank for 0.5-1 minute; Use a water gun to clean the chromium stainless steel disc until there is no black ash adhering to the surface of the chromium stainless steel disc.
4. The pickling method for chromium stainless steel discs according to claim 1, characterized in that, The neutralization process includes the following steps: The residual acid in chromium stainless steel wire rods was neutralized in a sodium carbonate solution at a temperature of 70-80℃ when the pH was ≥12.
5. The pickling method for chromium stainless steel discs according to claim 1, characterized in that, The rust inhibitor treatment includes the following steps: Immerse the chromium stainless steel coil in a rust-preventive solution at a temperature of 70℃~80℃ for 20~30 seconds.
6. The pickling method for chromium stainless steel discs according to claim 1, characterized in that, The drying process includes the following steps: Bake at 100℃ for 4–6 minutes.
7. A method for pickling chromium stainless steel discs according to any one of claims 1-6, characterized in that, It also includes periodically sampling the pickling solution and testing the concentrations of hydrogen ions, fluoride ions, and iron ions in the pickling solution.
Citation Information
Patent Citations
Direct chromium stainless-steel pickling agent
CN101029400A