A low-tension shield foaming agent and preparation method thereof
By using a combination of surfactant containing methacrylic acid groups and silicon oxygen bonds in the foaming agent for shield structure, the problem of limited surface tension of existing foaming agents is solved, and the effect of high foaming ratio and long half-life is achieved, ensuring that The construction proceeded smoothly and the environmental impact was reduced.
Patent Information
- Application Number
- CN202310516559.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-05-09
AI Technical Summary
When existing foaming agents for shields improve foaming ratio and half-life performance, they usually need to add a variety of additives, resulting in poor environmental protection performance and limited surface tension reduction, which limits its application range.
Low tension is prepared by specific preparation methods using amphoteric surfactants, anionic surfactants and nonionic surfactants, specifically including amphoteric surfactants containing methacrylic acid groups and nonionic surfactants containing silicon oxygen bonds. Foaming agent reduces interface tension and improves foaming performance.
A foaming agent with high foaming ratio and long half-life has been achieved, which reduces the adhesion of clay to the cutting board, and ensures the smooth progress of soil pressure balance shield construction. At the same time, the components are simple, low cost and no environmental pollution, which is suitable for market promotion. .
Smart Images

Figure BDA0004219382420000041 
Figure BDA0004219382420000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of shield construction, and in particular to a foaming agent for low-tension shield construction and a preparation method thereof. Background Art
[0002] At present, China's subway construction is developing rapidly. Earth pressure balance shield technology is often used in subway tunnel construction. The key to this technology is to keep the slag in a plastic flow state to achieve smooth slag discharge, stable excavation surface and moderate thrust. Therefore, it is necessary to improve the slag to meet the excavation requirements. The methods for improving slag during construction include minerals, water-soluble polymers, highly absorbent resins and surfactants. Among them, surfactants, also known as foaming agents, are widely used in earth pressure balance shield construction because they are suitable for various soil types and have the advantages of good lubrication, stable pressure in the soil compartment and improved plastic flow of the soil.
[0003] In recent years, with the development and research of engineering and technical personnel, many different types of foaming agents have been disclosed. However, the following problems are still found in practical applications: (1) In order to improve both the foaming ratio and the half-life time, multiple additives are often added to the existing shield foaming agents, resulting in poor environmental performance of the foaming agents and limited application scope; (2) The existing foaming agents prepared with surfactants have limited ability to reduce surface tension.
[0004] Based on the above, there is an urgent need in this field to develop a new type of foaming agent that can ensure excellent slag modification while having low surface tension characteristics and little impact on the environment. Summary of the invention
[0005] The purpose of the present invention is to provide a low-tension shield foaming agent and a preparation method thereof, so as to solve the problem that traditional foaming agents are limited in reducing interfacial tension. At the same time, the foaming agent prepared by the method has a high foaming ratio, a long foam half-life, simple components, low cost, no environmental pollution, and is conducive to market promotion and application.
[0006] In order to achieve the above object, the present invention first provides a low tension shield foaming agent, which comprises at least, by weight: 4 to 5 parts of amphoteric surfactant; 3 to 4 parts of anionic surfactant; 4 to 5 parts of nonionic surfactant; and 86 to 89 parts of water.
[0007] Wherein, the amphoteric surfactant contains at least one methacrylic acid group; and the nonionic surfactant contains at least one silicon-oxygen bond.
[0008] Preferably, the low-tension shield foaming agent comprises at least, by weight: 4.5 parts of amphoteric surfactant; 3.5 parts of anionic surfactant; 4.5 parts of nonionic surfactant; and 87.5 parts of water.
[0009] Preferably, the amphoteric surfactant is 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt; and the nonionic surfactant is diethylaminomethyltriethoxysilane.
[0010] Preferably, the anionic surfactant comprises sodium lauryl sulfate.
[0011] Preferably, the low-tension shield foaming agent is composed of the following components, measured in parts by weight: 4 to 5 parts of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt; 3 to 4 parts of sodium dodecyl sulfate; 4 to 5 parts of diethylaminomethyltriethoxysilane; and 86 to 89 parts of water.
[0012] Another aspect of the present invention further provides a method for preparing the aforementioned low-tension shield foaming agent, comprising the following steps:
[0013] S1, add 86-89 parts of water to a reaction kettle at room temperature, introduce inert gas, add 4-5 parts of amphoteric surfactant and 3-4 parts of anionic surfactant under stirring, and stir for 15-25 minutes;
[0014] S2, continue to add 4 to 5 parts of non-ionic surfactant, stir for 10 to 15 minutes, and then perform vacuum degassing to obtain the low-tension shield foaming agent;
[0015] Wherein, the amphoteric surfactant contains at least one methacrylic acid group; and the nonionic surfactant contains at least one silicon-oxygen bond.
[0016] Preferably, the inert gas is nitrogen.
[0017] Preferably, the stirring speed in steps S1 and S2 is 50-100 rpm / min.
[0018] Compared with the prior art, the beneficial effects of the present invention are:
[0019] (1) Compared with the existing shield foaming agents, the shield foaming agent of the present invention introduces methacrylic acid groups and siloxane bonds into its components, which helps to reduce the interfacial tension of the foaming agent while also having better foaming performance and stability, thereby solving the problem that the existing shield foaming agents are limited in reducing the interfacial tension, especially the problem that it is difficult to prepare a foaming agent that has low surface tension, high foaming ratio, and long foam half-life.
[0020] (2) The 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt and diethylaminomethyltriethoxysilane components in the shield foaming agent of the present invention can play a synergistic role and significantly reduce the interfacial tension of the foaming agent. The lower interfacial tension can greatly reduce the capillary force, further effectively reduce the adhesion of clay to the cutterhead, and ensure the smooth progress of the earth pressure balance shield construction.
[0021] (3) The shield foaming agent of the present invention has simple ingredients, a simple preparation method, is environmentally friendly, and is suitable for market promotion and application. DETAILED DESCRIPTION
[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Terminology
[0024] In the present invention, "interfacial tension" and "surface tension" can be used interchangeably.
[0025] In order to solve the problem that the conventional foaming agent for shielding has limited interfacial tension reduction in the background technology, the present invention first provides a low-tension foaming agent for shielding, which comprises at least:
[0026] Amphoteric surfactant: 4-5 parts; Anionic surfactant: 3-4 parts; Nonionic surfactant: 4-5 parts; Water: 86-89 parts;
[0027] The amphoteric surfactant contains at least one methacrylic acid group, and the nonionic surfactant contains at least one silicon-oxygen bond. The methyl group and silicon-oxygen bond of the methacrylic acid group help to improve the ability of the foaming agent to reduce interfacial tension.
[0028] In one embodiment of the present invention, the amphoteric surfactant is 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, and its molecular structure is shown in formula (I), which contains a methacrylic acid group, a quaternary ammonium salt ion and a sulfonate ion; the nonionic surfactant is diethylaminomethyltriethoxysilane, and its molecular structure is shown in formula (II), and its molecule contains three silicon-oxygen bonds. Experiments have shown that it can significantly improve the ability of the foaming agent of the present invention to reduce interfacial tension, and is stronger than the ability of traditional ether surfactants to reduce surface tension.
[0029]
[0030] In one embodiment of the present invention, the anionic surfactant includes sodium dodecyl sulfate, which is helpful for generating bubbles of uniform size at a low dosage.
[0031] In one embodiment of the present invention, the low tension shield foaming agent comprises at least, by weight:
[0032] Amphoteric surfactant: 4.5 parts; Anionic surfactant: 3.5 parts; Nonionic surfactant: 4.5 parts; Water: 87.5 parts.
[0033] In one embodiment of the present invention, the low tension shield foaming agent is composed of the following components in parts by weight:
[0034] 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt: 4 to 5 parts; sodium dodecyl sulfate: 3 to 4 parts; diethylaminomethyltriethoxysilane: 4 to 5 parts; water: 86 to 89 parts.
[0035] Another aspect of the present invention further provides a method for preparing any of the above-mentioned low-tension shield foaming agents, comprising the following steps:
[0036] S1, add 86-89 parts of water to a reaction kettle at room temperature, introduce inert gas, add 4-5 parts of amphoteric surfactant and 3-4 parts of anionic surfactant under stirring, and stir for 15-25 minutes;
[0037] S2, continue to add 4 to 5 parts of non-ionic surfactant, stir for 10 to 15 minutes, and then perform vacuum degassing to obtain the low-tension shield foaming agent;
[0038] Wherein, the amphoteric surfactant contains at least one methacrylic acid group; and the nonionic surfactant contains at least one silicon-oxygen bond.
[0039] In one embodiment of the present invention, the inert gas is nitrogen.
[0040] In one embodiment of the present invention, the stirring speed in steps S1 and S2 is 50-100 rpm / min.
[0041] The present invention is further described in detail below in conjunction with specific embodiments and comparative examples.
[0042] Example 1
[0043] A method for preparing a low-tension shield foaming agent comprises the following steps:
[0044] S1, add 89 parts of water to the reaction kettle at room temperature, introduce nitrogen, add 4 parts of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt and 3 parts of sodium dodecyl sulfate under stirring at 50-100 rpm / min, and stir for 20 minutes;
[0045] S2, continue to add 4 parts of diethylaminomethyltriethoxysilane, stir for 10 minutes, and then perform vacuum degassing to obtain the low-tension shield foaming agent.
[0046] Example 2
[0047] A method for preparing a low-tension shield foaming agent comprises the following steps:
[0048] S1, add 87.5 parts of water to the reaction kettle at room temperature, introduce nitrogen, add 4.5 parts of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt and 3.5 parts of sodium dodecyl sulfate under stirring at 50-100 rpm / min, and stir for 20 minutes;
[0049] S2, continue to add 4.5 parts of diethylaminomethyltriethoxysilane, stir for 10 minutes, and then perform vacuum degassing to obtain the low-tension shield foaming agent.
[0050] Example 3
[0051] A method for preparing a low-tension shield foaming agent comprises the following steps:
[0052] S1, add 86 parts of water to the reaction kettle at room temperature, introduce nitrogen, add 5 parts of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt and 4 parts of sodium dodecyl sulfate under stirring at 50-100 rpm / min, and stir for 20 minutes;
[0053] S2, continue to add 5 parts of diethylaminomethyltriethoxysilane, stir for 10 minutes, and then perform vacuum degassing to obtain the low-tension shield foaming agent.
[0054] Comparative Example 1
[0055] Compared with Example 2, the difference is that sodium vinyl sulfonate is used instead of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, specifically, the following steps are included:
[0056] S1, add 87.5 parts of water to the reactor at room temperature, introduce nitrogen, add 4.5 parts of sodium vinyl sulfonate and 3.5 parts of sodium dodecyl sulfate under stirring at 50-100 rpm / min, and stir for 20 minutes;
[0057] S2, continue to add 4.5 parts of diethylaminomethyltriethoxysilane, stir for 10 minutes, and then perform vacuum degassing to obtain the foaming agent product of Comparative Example 1.
[0058] Comparative Example 2
[0059] Compared with Example 2, the difference is that 3-(N,N-dimethyldodecylammonium) is used instead of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, specifically, the following steps are included:
[0060] S1, add 87.5 parts of water to the reactor at room temperature, introduce nitrogen, add 4.5 parts of 3-(N,N-dimethyldodecylammonium) and 3.5 parts of sodium dodecyl sulfate under stirring at 50-100 rpm / min, and stir for 20 minutes;
[0061] S2, continue to add 4.5 parts of diethylaminomethyltriethoxysilane, stir for 10 minutes, and then perform vacuum degassing to obtain the foaming agent product of Comparative Example 2.
[0062] Comparative Example 3
[0063] Compared with Example 2, the difference is that trimethylsilyl diethylamine is used to replace diethylamino methyl triethoxy silane, specifically, the following steps are included:
[0064] S1, add 87.5 parts of water to the reaction kettle at room temperature, introduce nitrogen, add 4.5 parts of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt and 3.5 parts of sodium dodecyl sulfate under stirring at 50-100 rpm / min, and stir for 20 minutes;
[0065] S2, continue to add 4.5 parts of trimethylsilyl diethylamine, stir for 10 minutes, and then perform vacuum degassing to obtain the foaming agent product of Comparative Example 3.
[0066] Comparative Example 4
[0067] 87.5 parts of water were added to the reactor at room temperature, nitrogen was introduced, and 12.5 parts of sodium dodecyl sulfate were added under stirring at 50-100 rpm / min. The mixture was stirred for 30 minutes and vacuum degassed to obtain the foaming agent product of Comparative Example 4.
[0068] Comparative Examples 5 and 6 are commercially available products of BASF and CONDAT.
[0069] Performance measurement
[0070] The foaming agent products of the above three embodiments and six comparative examples were tested for the following properties.
[0071] 1. Liquid density
[0072] Wash and dry the density meter, and slowly put it into a suitable measuring cylinder containing the test liquid without touching the sides and bottom of the container. Keep the test liquid temperature at 20°C. After it has been allowed to stand, gently press it down a little, and then wait for it to rise naturally and stand until no bubbles emerge. Observe the scale at the intersection with the liquid surface from a horizontal position, which is the relative density of the sample.
[0073] 2. Foaming ratio and half-life test method
[0074] The foaming agent in the embodiment and the comparative example is diluted to a 4wt% aqueous solution, and added to the independently developed intelligent foam generator (CN202223253107.6), and the pressure of the compressed air is set to 0.2MPa; the intelligent foaming agent generator comprises: a solution barrel; an air pump (used to inject air into the solution barrel) to change the liquid foaming agent in the solution barrel into a foam state; a measuring cylinder, wherein a first and a second foam liquid level sensor are arranged inside, and the foam liquid level sensor can generate a corresponding sensing signal when it contacts the foam in the measuring cylinder; the setting positions of the first and the second foam liquid level sensors correspond to the first and the second scale values of the measuring cylinder respectively, and the second scale value is half of the first scale value; a water level sensor is arranged in the measuring cylinder to measure the liquid level height of the liquid in the measuring cylinder; a control module is configured to calculate the half-life of the foaming agent for shield based on the time when the sensing signal of the first foam liquid level sensor is initially received and the time when the sensing signal of the second foam liquid level sensor disappears; the control module is also configured to calculate the foaming multiple of the foaming agent for shield based on the measurement value of the water level sensor.
[0075] 3. Determination of surface tension
[0076] First, prepare a product solution of a certain concentration (4wt%) and measure it with a surface tension meter using the platinum sheet method. The sample solution is prepared with distilled water and the test temperature is 25±0.5℃. Pour an appropriate amount of test solution into a glass dish and place it on the platform inside the surface tension meter. Lower the platform and use the platinum sheet suspended in the air to touch the water surface. The reading on the dial at this time is the surface tension. Since the entire process is automatically operated by the system, the error caused by human factors during the measurement process can be ignored.
[0077] 4. Emulsification performance determination
[0078] Weigh 1g of sample and 99g of water to prepare a 0.1% product aqueous solution. Pour 40ml of the aqueous solution into a 100ml stoppered measuring cylinder, add 40ml of benzene, shake up and down vigorously 5 times, let stand for 1min, shake 5 times again, repeat 5 times, stop the last shake, and record the time required to separate 10ml of water. This value represents the relative emulsifying power.
[0079] The performance test results of the foaming agent products of Examples 1-3 and Comparative Examples 1-6 are shown in Table 1.
[0080] Table 1 Main performance test results of low tension shield foaming agent
[0081]
[0082] It can be seen from Examples 1-3 that as the mass concentration increases, the density in the system shows an increasing trend. Compared with Examples 1 and 3, the foaming ratio, surface tension, half-life and emulsification performance of the foaming agent prepared in Example 2 are better.
[0083] It can be seen from Example 2 and Comparative Examples 2-3 that the introduction of methacrylic acid groups and silanol bonds (Si-O bonds) can significantly reduce the surface tension in the system, improve the emulsification performance of the foaming agent, and increase the foaming rate and half-life of the foaming agent; further, it can be seen from Comparative Example 4 that by adding 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid salt and diethylaminomethyltriethoxysilane at the same time, the two can play a synergistic role, significantly reducing the surface tension of the foaming agent while improving the foaming rate, half-life and emulsification performance of the foaming agent.
[0084] Further comparison of Comparative Examples 1 and 2 shows that the presence of quaternary ammonium salt ions also helps to reduce the surface tension of the foaming agent and improve its emulsification performance.
[0085] It can be seen from Example 2 and Comparative Examples 5-6 that, compared with the commercially available foaming agent products of BASF and condat, the foaming agent prepared in the present application has lower surface tension and also has better foaming ratio, half-life and emulsification performance.
[0086] In summary, the low-tension shield foam provided by the present invention introduces methacrylic acid groups and silicon-oxygen bonds into the ingredients, which helps to reduce the interfacial tension of the foam while also having better foaming performance and stability, which is beneficial to the smooth progress of earth pressure balance shield construction. In addition, the shield foam of the present application has simple ingredients, a simple preparation method, and is pollution-free to the environment, and is suitable for market promotion and application.
[0087] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A low tension foaming agent for shield tunneling, It is characterized in that In parts by weight, the low tension shield foaming agent comprises at least: Amphoteric surfactant: 4-5 parts; Anionic surfactant: 3-4 parts; Nonionic surfactant: 4-5 parts; Water: 86-89 parts; Wherein, the amphoteric surfactant contains at least one methacrylic acid group; the nonionic surfactant contains at least one silicon-oxygen bond; The amphoteric surfactant is 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt; The nonionic surfactant is diethylaminomethyltriethoxysilane; The anionic surfactant includes sodium lauryl sulfate.
2. The low tension shield foaming agent according to claim 1, It is characterized in that In parts by weight, the low tension shield foaming agent comprises at least: Amphoteric surfactant: 4.5 parts; Anionic surfactant: 3.5 parts; Nonionic surfactant: 4.5 parts; Water: 87.5 parts.
3. A method for preparing the low tension shield foaming agent according to claim 1, It is characterized in that The following steps are involved: S1, add 86-89 parts of water to a reaction kettle at room temperature, introduce inert gas, add 4-5 parts of amphoteric surfactant and 3-4 parts of anionic surfactant under stirring, and stir for 15-25 minutes; S2, adding 4 to 5 parts of a nonionic surfactant, stirring for 10 to 15 minutes, and vacuum degassing to obtain the low-tension shield foaming agent; Wherein, the amphoteric surfactant contains at least one methacrylic acid group; and the nonionic surfactant contains at least one silicon-oxygen bond.
4. The method for preparing the low tension shield foaming agent according to claim 3, It is characterized in that The inert gas is nitrogen.
5. The method for preparing the low tension shield foaming agent according to claim 3, It is characterized in that The stirring speed of steps S1 and S2 is 50-100 rpm / min.