A prepreg and its application
Through the combination of maleimide compound prepolymer and epoxy resin, combined with specific reinforcing materials and siloxane compounds, a dense cross-linked network is formed, which solves the problem of planar thermal expansion coefficient and vitrification in the resin system in the existing technology. The lack of transition temperature enables the laminate to achieve low thermal expansion coefficient, high glass transition temperature and excellent heat and moisture resistance and CAF capability.
Patent Information
- Application Number
- CN202211612964.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-15
AI Technical Summary
It is difficult to simultaneously achieve extremely low planar thermal expansion coefficient, high glass transition temperature, excellent moisture and heat resistance, good resin interface bonding and excellent CAF resistance in a resin system, especially in packaging carrier materials. Traditional The technical route of reducing the plane thermal expansion coefficient can easily lead to reduced fluidity and peel strength.
Using a combination of maleimide compound prepolymer and epoxy resin, through specific reinforcing materials such as Q-glass fiber cloth and siloxane compounds, a dense spatial cross-linked network is formed, with optimal preparation conditions and composition In proportion, prepregs with low planar thermal expansion coefficient and high glass transition temperature are prepared.
It achieves the extremely low planar thermal expansion coefficient, high glass transition temperature, excellent moisture and heat resistance, good resin interface bonding and excellent CAF resistance of the laminate. It is suitable for substrate materials for high-speed and high-density packaging printed circuit boards.
Smart Images

Figure BDA0004000820440000021 
Figure BDA0004000820440000101 
Figure BDA0004000820440000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of laminated boards and relates to a prepreg and application thereof. Background Art
[0002] With the in-depth development of the information age and the intelligent age, chips are being used more and more widely, and the performance requirements for packaging substrate materials are becoming higher and higher, mainly reflected in higher glass transition temperature, lower planar thermal expansion coefficient and higher reliability.
[0003] When the resin system itself has a low in-plane thermal expansion coefficient, further optimization is very difficult and may even worsen other performance indicators: the traditional technical route to reduce the in-plane thermal expansion coefficient is mainly to improve the resin system formula, but the improvement effect is not obvious and it is easy to lead to reduced fluidity and peel strength.
[0004] Therefore, in the art, it is desired to develop a material that can make the laminate have extremely low in-plane thermal expansion coefficient, high glass transition temperature, excellent moisture and heat resistance, good resin interface bonding and excellent CAF resistance. Summary of the invention
[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a prepreg and its application. The prepreg of the present invention can make the laminate have an extremely low planar thermal expansion coefficient, a high glass transition temperature, excellent moisture and heat resistance, good resin interface bonding and excellent CAF resistance, and is suitable for making a substrate material for a high-speed, high-density packaged printed circuit board.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In one aspect, the present invention provides a prepreg, the prepreg comprising a reinforcing material and a resin composition;
[0008] The reinforcing material is selected from one of Q-fiberglass cloth, D-fiberglass cloth, L-fiberglass cloth, M-fiberglass cloth, S-fiberglass cloth or T-fiberglass cloth;
[0009] The resin composition comprises (A) a maleimide compound prepolymer and (B) an epoxy resin, wherein the raw materials for preparing the maleimide compound prepolymer (A) include a maleimide compound having a structure of formula I and a siloxane compound having at least two primary amino groups in one molecule;
[0010]
[0011] Where R 1 -R 4Each is independently selected from hydrogen or a C1-C5 (which may be a C1, C2, C3, C4 or C5 alkyl, such as methyl, ethyl, propyl, butyl or pentyl, etc.) straight chain or branched alkyl group, and X is selected from a C1-C5 (which may be a C1, C2, C3, C4 or C5 alkyl, such as methyl, ethyl, propyl, butyl or pentyl, etc.) straight chain or branched alkylene group or a single bond.
[0012] By selecting X as a straight chain or branched alkylene or single bond of a short chain structure, the segment length of the maleimide compound can be effectively compressed, and its steric hindrance can be reduced. During the prepolymerization process, the aminosilicone compound can be quickly added to the double bond of the maleimide compound to form a dense spatial cross-linked network; at the same time, the short chain structure of X is not easy to rotate, and the structure of the obtained maleimide compound prepolymer is stable, so that a low planar thermal expansion coefficient and a high glass transition temperature can be obtained. The inventors have found that the resin composition of the present invention can cooperate with a specific reinforcing material to further improve the planar thermal expansion coefficient and increase the glass transition temperature.
[0013] The maleimide compound of the formula I structure can use commercially available products, including but not limited to: bis(4-maleimidophenyl)methane (e.g., BMI of KI Chemicals, BMI-1000 of Yamato Chemicals, or BMI-01 of Hubei Honghu Shuangma Resin Factory) or bis(3-ethyl-5-methyl-4-maleimidophenyl)methane (e.g., BMI-70 of KI Chemicals, BMI-5100 of Yamato Chemicals, or D937 of Sichuan Dongcai Technology Group Co., Ltd.).
[0014] The siloxane compound containing at least two primary amino groups includes a siloxane compound containing two primary amino groups, which can obtain a resin composition having a low planar expansion coefficient. The siloxane compound containing two primary amino groups can use commercially available products, including but not limited to: PAM-E (amino functional group equivalent 130 g / mol), KF-8010 (amino functional group equivalent 430 g / mol), X-22-161A (amino functional group equivalent 800 g / mol), X-22-161B (amino functional group equivalent 1500 g / mol), KF-8012 (amino functional group equivalent 2200 g / mol), KF-8008 (amino functional group equivalent 5700 g / mol), X-22-1660B-3 (amino functional group equivalent 2200 g / mol) or X-22-9409 (amino functional group equivalent 670 g / mol) of Shin-Etsu Chemical Co., Ltd., or a combination of at least two of them.
[0015] In the present invention, the laminated board prepared by the prepreg obtained by co-curing the maleimide compound prepolymer and the epoxy resin and combining with the reinforcing material has an extremely low planar thermal expansion coefficient, a high glass transition temperature, excellent moisture and heat resistance, good resin interface bonding and excellent CAF resistance.
[0016] In the present invention, the weight average molecular weight of the maleimide compound prepolymer (A) is 1000 to 10000, for example, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000 or 10000. If the weight average molecular weight of the maleimide compound prepolymer is too small, it is difficult to obtain the effect of extremely low planar thermal expansion coefficient. If the weight average molecular weight of the maleimide compound prepolymer is too large, it may cause problems such as resin interface delamination and CAF failure, thereby reducing the reliability of the material.
[0017] The weight average molecular weight of the maleimide compound prepolymer of the present invention is obtained by GPC (gel permeation chromatography) test during the synthesis process, and the test method is GB / T 21863-2008, and the polystyrene calibration is used as the basis for determination by gel permeation chromatography. The specific operation is: during the synthesis process of the maleimide compound prepolymer, samples are taken at intervals, the samples are dissolved with tetrahydrofuran (THF), shaken, and placed in a GPC device for testing to measure the weight average molecular weight. If the weight average molecular weight reaches the range of the present invention, the synthesis reaction can be terminated. Therefore, the present invention monitors the synthesis reaction process by GPC to obtain the weight average molecular weight range of the maleimide compound prepolymer that meets the present invention.
[0018] Preferably, the temperature of the synthesis reaction is 100-150°C, for example, it can be 102°C, 105°C, 108°C, 110°C, 112°C, 115°C, 118°C, 120°C, 122°C, 125°C, 128°C, 135°C, 142°C, or 148°C.
[0019] Preferably, the synthesis reaction time is 2 to 8 h, for example, it can be 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 7 h or 8 h.
[0020] Preferably, the resin composition accounts for 45-80% of the total weight of the prepreg, for example 45%, 48%, 50%, 53%, 55%, 58%, 60%, 65%, 68%, 70%, 75%, 78% or 80%.
[0021] Preferably, based on the total weight of the resin composition as 100%, the content of the (A) maleimide compound prepolymer is 40-80% (for example, 42%, 45%, 48%, 50%, 53%, 55%, 58%, 60%, 65%, 68%, 70%, 75%, 78% or 80%), and the content of the (B) epoxy resin is 20-60% (for example, 20%, 25%, 28%, 30%, 35%, 38%, 40%, 45%, 48%, 50%, 55% or 60%).
[0022] Preferably, the content of the maleimide compound of the structure of formula I in the raw material for preparing the maleimide compound prepolymer is 50-90 weight % (for example, 50 weight %, 55 weight %, 60 weight %, 65 weight %, 70 weight %, 75 weight %, 80 weight %, 85 weight % or 90 weight %), and the content of the siloxane compound containing at least 2 primary amino groups in one molecule is 10-50 weight % (for example, 10 weight %, 15 weight %, 20 weight %, 30 weight %, 40 weight % or 50 weight %).
[0023] Preferably, the (B) epoxy resin is selected from bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, phenol formaldehyde epoxy resin, methylphenol novolac epoxy resin, bisphenol A novolac epoxy resin, dicyclopentadiene epoxy resin, biphenyl epoxy resin, dicyclopentadiene novolac epoxy resin, biphenyl novolac epoxy resin, resorcinol epoxy resin, naphthalene epoxy resin, phosphorus-containing epoxy resin, silicon-containing epoxy resin, glycidylamine epoxy resin, alicyclic epoxy resin, polyethylene glycol epoxy resin, tetraphenol ethane tetraglycidyl ether, trisphenol methane epoxy resin, condensation product of cyanate ester and epoxy resin or condensation product of difunctional isocyanate and epoxy resin, any one or a combination of at least two thereof.
[0024] Preferably, the resin composition further comprises other curing agents, and the other curing agents are selected from any one or a combination of at least two of amine curing agents, phenolic curing agents, benzoxazine curing agents, cyanate curing agents, active ester curing agents, anhydride curing agents or other modified maleimide curing agents.
[0025] Preferably, the resin composition further comprises an inorganic filler.
[0026] Preferably, the inorganic filler is selected from any one or a combination of at least two of non-metallic oxides, metal nitrides, non-metallic nitrides, inorganic hydrates, inorganic salts, metal hydrates or inorganic phosphorus; further preferably, it is any one or a combination of at least two of fused silica, crystalline silica, spherical silica, hollow silica, aluminum hydroxide, aluminum oxide, talc, aluminum nitride, boron nitride, silicon carbide, barium sulfate, barium titanate, strontium titanate, calcium carbonate, calcium silicate or mica.
[0027] In another aspect, the present invention provides a laminate comprising at least one prepreg as described above.
[0028] In another aspect, the present invention provides a metal foil-clad laminate, comprising at least one prepreg as described above and a metal foil coated on one side or both sides of the prepreg.
[0029] The material of the metal foil is not particularly limited; preferably, the metal foil includes copper foil, nickel foil, aluminum foil or SUS foil.
[0030] In another aspect, the present invention provides a printed wiring board, comprising at least one prepreg as described above.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The laminated board prepared by the prepreg obtained by co-curing the maleimide compound prepolymer and the epoxy resin and combining them with the reinforcing material has extremely low planar thermal expansion coefficient, high glass transition temperature, excellent moisture and heat resistance, good resin interface bonding and excellent CAF resistance. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0034] Synthesis example 1:
[0035] A maleimide compound prepolymer A-1, prepared by the following method:
[0036] Into a 2-liter reaction container capable of heating and cooling and equipped with a thermometer, a stirring device, and a moisture meter with a reflux condenser, were added 100 g of a two-terminal diamine-modified siloxane (X-22-161B manufactured by Shin-Etsu Chemical Co., Ltd., with an amino functional group equivalent of 1500 g / mol), 50 g of 4-aminophenol (Guangtuo Chemical Co., Ltd.), 350 g of bis(3-ethyl-5-methyl-4-maleimidophenyl)methane (BMI-5100 manufactured by Yamato Chemical Co., Ltd.) and 500 g of propylene glycol monomethyl ether, and the mixture was reacted at 110°C for 3 hours to obtain a solution of maleimide compound prepolymer A-1, whose weight average molecular weight Mw was measured by GPC to be 4000±500.
[0037] Synthesis example 2:
[0038] A maleimide compound prepolymer A-2, prepared by the following method:
[0039] Into a 2-liter reaction container capable of heating and cooling and equipped with a thermometer, a stirring device, and a moisture meter with a reflux condenser, were added 100 g of a two-terminal diamine-modified siloxane (X-22-161A manufactured by Shin-Etsu Chemical Co., Ltd., with an amino functional group equivalent of 800 g / mol), 10 g of 4-aminophenol (Guangtuo Chemical Co., Ltd.), 390 g of bis(4-maleimidephenyl)methane (BMI-1000 manufactured by Yamato Chemical Co., Ltd.) and 500 g of propylene glycol monomethyl ether, and the mixture was reacted at 120°C for 3.5 hours to obtain a solution of maleimide compound prepolymer A-2, whose weight average molecular weight Mw was measured by GPC to be 5300±700.
[0040] Synthesis example 3
[0041] A maleimide compound prepolymer A-3, prepared by the following method:
[0042] Into a 2-liter reaction container capable of heating and cooling and equipped with a thermometer, a stirring device, and a moisture meter with a reflux condenser, were added 35 g of a two-terminal diamine-modified siloxane (X-22-161A manufactured by Shin-Etsu Chemical Co., Ltd., with an amino functional group equivalent of 800 g / mol), 85 g of 4-aminophenol (Guangtuo Chemical Co., Ltd.), 380 g of bis(4-maleimidephenyl)methane (BMI-1000 manufactured by Yamato Chemical Co., Ltd.) and 500 g of propylene glycol monomethyl ether, and the mixture was reacted at 110°C for 2 hours to obtain a solution of maleimide compound prepolymer A-3, whose weight average molecular weight Mw was measured by GPC to be 1300±100.
[0043] Synthesis example 4
[0044] A maleimide compound prepolymer A-4, prepared by the following method:
[0045] Into a 2-liter reaction container capable of heating and cooling and equipped with a thermometer, a stirring device, and a moisture meter with a reflux condenser, were added 130 g of a two-terminal diamine-modified siloxane (X-22-161A manufactured by Shin-Etsu Chemical Co., Ltd., with an amino functional group equivalent of 800 g / mol), 370 g of bis(4-maleimidephenyl)methane (BMI-1000 manufactured by Yamato Chemical Co., Ltd.) and 500 g of propylene glycol monomethyl ether, and the mixture was reacted at 120°C for 3 hours to obtain a solution of maleimide compound prepolymer A-4, whose weight average molecular weight Mw was measured by GPC to be 9000±900.
[0046] Synthesis example 5:
[0047] A maleimide compound prepolymer A-5, prepared by the following method:
[0048] Into a 2-liter reaction container capable of heating and cooling and equipped with a thermometer, a stirring device, and a moisture meter with a reflux condenser, were added 140 g of a two-terminal diamine-modified siloxane (X-22-161A manufactured by Shin-Etsu Chemical Co., Ltd., with an amino functional group equivalent of 800 g / mol), 10 g of 4-aminophenol (Guangtuo Chemical Co., Ltd.), 350 g of bis(4-maleimidephenyl)methane (BMI-1000 manufactured by Yamato Chemical Co., Ltd.) and 500 g of propylene glycol monomethyl ether, and the mixture was reacted at 110°C for 3 hours to obtain a solution of maleimide compound prepolymer A-5, whose weight average molecular weight Mw was measured by GPC to be 11000±900.
[0049] Synthesis example 6:
[0050] A maleimide compound prepolymer A-6, prepared by the following method:
[0051] Into a 2-liter reaction container capable of heating and cooling and equipped with a thermometer, a stirring device, and a moisture meter with a reflux condenser, were added 30 g of a two-terminal diamine-modified siloxane (X-22-161A manufactured by Shin-Etsu Chemical Co., Ltd., with an amino functional group equivalent of 800 g / mol), 80 g of 4-aminophenol (Guangtuo Chemical Co., Ltd.), 390 g of bis(4-maleimidephenyl)methane (BMI-1000 manufactured by Yamato Chemical Co., Ltd.) and 500 g of propylene glycol monomethyl ether, and the mixture was reacted at 110°C for 3 hours to obtain a solution of maleimide compound prepolymer A-6, whose weight average molecular weight Mw was measured by GPC to be 860±100.
[0052] Synthesis example 7:
[0053] A maleimide compound prepolymer A-7, prepared by the following method:
[0054] Into a 2-liter reaction container capable of heating and cooling and equipped with a thermometer, a stirring device, and a moisture meter with a reflux condenser, were added 70 g of a two-terminal diamine-modified siloxane (X-22-161A manufactured by Shin-Etsu Chemical Co., Ltd., with an amino functional group equivalent of 800 g / mol), 40 g of 4-aminophenol (Guangtuo Chemical Co., Ltd.), 390 g of bis(4-maleimide phenyl ether) methane (BMI-4000 manufactured by Yamato Chemical Co., Ltd.) and 500 g of propylene glycol monomethyl ether, and the mixture was reacted at 110°C for 3 hours to obtain a solution of maleimide compound prepolymer A-7, whose weight average molecular weight Mw was measured by GPC to be 4500±800.
[0055] Synthesis example 8:
[0056] A maleimide compound prepolymer A-8, prepared by the following method:
[0057] Into a 2-liter reaction container capable of heating and cooling and equipped with a thermometer, a stirring device, and a moisture meter with a reflux condenser, were added 70 g of a two-terminal diamine-modified siloxane (X-22-161A manufactured by Shin-Etsu Chemical Co., Ltd., with an amino functional group equivalent of 800 g / mol), 40 g of 4-aminophenol (Guangtuo Chemical Co., Ltd.), 390 g of polybis(4-maleimidephenyl)methane (BMI-2300 manufactured by Yamato Chemical Co., Ltd.) and 500 g of propylene glycol monomethyl ether, and the mixture was reacted at 110°C for 3 hours to obtain a solution of maleimide compound prepolymer A-8, whose weight average molecular weight Mw was measured by GPC to be 6500±1100.
[0058] Examples 1-12, Comparative Examples 1-5
[0059] The components shown below were mixed in the proportions shown in Tables 1 and 2 (the units of the values in the tables are parts by mass, and in the case of solutions, the amounts are calculated based on the solid content). Methyl ethyl ketone was used as the solvent to prepare a uniform varnish having a solid content concentration of 65% by mass. The varnish was then applied to Q-glass cloth 2116, E-glass cloth 2116, T-glass cloth 2116 or E-glass cloth 2118 by impregnation, and dried at 150°C for 4 minutes to obtain a prepreg, the thickness of which was controlled to be 0.10 mm.
[0060] Two (or eight or fifteen) prepregs were stacked, and electrolytic copper foils with a thickness of 18 μm were pressed on the upper and lower sides. 2 After curing for 2 hours, a copper-clad laminate with a core board thickness of 0.20 mm (or 0.80 mm, or 1.50 mm) was obtained.
[0061] The copper foil of the copper-clad laminate is etched to obtain a laminate having a thickness of 0.20 mm (or 0.80 mm, or 1.50 mm).
[0062] The obtained copper clad laminate and laminate were subjected to performance tests, and the test methods were as follows:
[0063] < Planar thermal expansion coefficient (XY-CTE) >
[0064] Take a laminate with a length of 60mm, a width of 4mm, and a thickness of 0.20mm as a sample, with the warp direction of the glass fiber in the Y direction and the weft direction of the glass fiber in the X direction. The sample is dried in an oven at 105℃ for 1h and then cooled to room temperature in a dryer. Use thermal analysis mechanical method (TMA) for measurement, with a heating rate of 10℃ / min, from room temperature to 300℃, and two heatings. After the first heating is completed and cooled to room temperature, the sample is re-set for the second heating. The result is the thermal expansion coefficient in the plane direction at the second heating of 50℃ to 130℃, and the unit is ppm / ℃.
[0065] <Glass transition temperature (Tg)>
[0066] A laminate with a length of 60 mm, a width of 10 mm, and a thickness of 0.80 mm was taken as a sample and measured using a dynamic mechanical thermal analyzer (DMA) with a heating rate of 10°C / min. The result was taken as the transition peak temperature of tanδ in °C.
[0067] <High Pressure Thermal Cooking (PCT)>
[0068] Take 3 laminates with a length of 100mm, a width of 100mm and a thickness of 0.80mm as samples. Cover the lid of the pressure cooker with enough water but do not seal it. Heat the water to boiling without pressure. Open the lid and quickly place the formed sheet vertically on the sample rack in the pressure cooker. Suspend the sample vertically above the boiling water. After the pressure (gauge pressure) reaches 103.4±3KPa, keep it for 300 minutes. After the cooking is completed, cool it and exhaust the gas from the pressure cooker. Take out the formed sheet and wipe it with a dry cloth, immerse it in a 288℃ tin furnace, and take the average time without delamination and explosion.
[0069] <Laminate resin interface bonding>
[0070] A laminate with a length of 10 mm, a width of 10 mm, and a thickness of 0.80 mm was taken as a sample, and after being cut into slices, the interface between the two adjacent prepreg sections was observed to see if there was separation, and the degree of separation.
[0071] <Rapid CAF pass rate>
[0072] A copper-clad laminate with a warp of 400 mm, a weft of 380 mm, and a thickness of 1.50 mm was taken as a sample and processed into test circuit modules with hole wall spacing of 125 μm (weft) × 1, 175 μm (warp and weft) × 2, and 250 μm (warp and weft) × 2, 5 each, for a total of 25 CAF test channels. The module was placed under 85°C / 85% RH for 15 hours, and the sample was taken out and placed in a CAF test box. The channel was connected and 100 V DC was applied. It was placed under 85°C / 85% RH for 66 hours. Failure was judged as resistance less than 2×10 7 If the passing rate is less than 80% (less than 20 of the 25 test channels pass), it is considered unqualified.
[0073] The evaluation results obtained by the above-mentioned measuring method are shown in Table 1-3.
[0074] Table 1
[0075]
[0076]
[0077] Table 2
[0078]
[0079] Table 3
[0080]
[0081] From the data in Table 1-3, it can be seen that the laminates prepared by the resin composition of maleimide compound prepolymer and epoxy resin co-cured in Examples 1-8 with specific reinforcing materials have extremely low in-plane thermal expansion coefficient (XY-CTE below 4.5ppm / ℃), high glass transition temperature (above 256℃), excellent moisture and heat resistance (PCT>300s), excellent resin interface bonding (no or only slight laminate resin interface separation) and excellent CAF resistance (fast CAF pass rate above 80%). In the system of the present invention, the resin composition with Q-glass cloth (Example 2) performs better in in-plane thermal expansion coefficient and glass transition temperature than T-glass cloth (Example 8).
[0082] If the weight average molecular weight of the maleimide compound prepolymer is too low (Example 10), the planar thermal expansion coefficient of the resulting laminate increases to 5.2 ppm / °C; if the weight average molecular weight of the maleimide compound prepolymer is too high (Example 9), the glass transition temperature of the resulting laminate decreases, and obvious separation occurs at the resin interface of the laminate, and the fast CAF pass rate is unqualified.
[0083] If the amount of maleimide compound prepolymer used is too much (Example 11), the resin interface of the resulting laminate will show obvious separation, the fast CAF pass rate will be unqualified, and the moisture and heat resistance will be reduced; if the amount of maleimide compound prepolymer used is too little (Example 12), the glass transition temperature of the resulting laminate will be reduced and the moisture and heat resistance will be reduced.
[0084] Compared with Example 2, in Comparative Example 1, the reinforcing material of the present invention was not used but E-glass cloth 2116 was used instead, and the planar thermal expansion coefficient of the obtained laminate was increased to 6.1 ppm / °C; in Comparative Example 2, although the planar thermal expansion coefficient of E-glass cloth 2118 was improved compared with E-glass cloth 2116, the glass transition temperature of the obtained laminate was reduced, and the resin interface of the laminate showed obvious separation, and the fast CAF pass rate was unqualified.
[0085] Compared with Example 2, Comparative Examples 3 and 4 do not use the maleimide compound of the formula I structure of the present invention. The raw material monomer for preparing the maleimide compound prepolymer in Comparative Example 3 contains -O- with large steric hindrance, and the glass transition temperature of the prepared laminate is sharply reduced; the raw material monomer for preparing the maleimide compound prepolymer in Comparative Example 4 is a poly-maleimide structure, the chain segment of the maleimide compound is relatively long, and the planar thermal expansion coefficient of the prepared laminate is increased to 5.1ppm / °C, and the glass transition temperature is only 276°C.
[0086] If the traditional BT resin formula is used in combination with Q-glass cloth, it is difficult for the resulting laminate to obtain an extremely low planar thermal expansion coefficient and a high glass transition temperature (Comparative Example 5); if the traditional BT resin formula is used in combination with Q-glass cloth and the amount of filler is increased, although the planar thermal expansion coefficient can reach 3.6ppm / °C, the glass transition temperature is only 227°C, and the resin interface of the laminate shows obvious separation, and the fast CAF pass rate is unqualified (Comparative Example 6).
[0087] The applicant declares that the present invention illustrates the prepreg and its application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A prepreg, characterized in that: The prepreg comprises a reinforcing material and a resin composition; The reinforcing material is selected from one of Q-fiberglass cloth and T-fiberglass cloth; The resin composition comprises (A) a maleimide compound prepolymer and (B) an epoxy resin, wherein the raw materials for preparing the maleimide compound prepolymer (A) include a maleimide compound having a structure of formula I and a siloxane compound having at least two primary amino groups in one molecule; wherein R1-R4 are each independently selected from hydrogen or a C1-C5 straight or branched alkyl group, and X is selected from a C1 alkylene group; The weight average molecular weight of the (A) maleimide compound prepolymer is 2000-8000; Based on the total weight of the resin composition as 100%, the content of the (A) maleimide compound prepolymer is 60-80%, and the content of the (B) epoxy resin is 20-40%; The content of the maleimide compound of the structure of formula I in the raw material for preparing the maleimide compound prepolymer is 50-90% by weight, and the content of the siloxane compound containing at least 2 primary amino groups in one molecule is 10-50% by weight.
2. The prepreg according to claim 1, characterized in that The resin composition accounts for 45-80% of the total weight of the prepreg.
3. The prepreg according to claim 1, characterized in that The (B) epoxy resin is selected from any one or a combination of at least two of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, phenol formaldehyde epoxy resin, methylphenol novolac epoxy resin, biphenyl epoxy resin, resorcinol epoxy resin, naphthalene epoxy resin, phosphorus-containing epoxy resin, silicon-containing epoxy resin, glycidylamine epoxy resin, alicyclic epoxy resin, polyethylene glycol epoxy resin, tetraphenol ethane tetraglycidyl ether, trisphenol methane epoxy resin or a condensate of cyanate ester and epoxy resin.
4. The prepreg according to claim 1, characterized in that The (B) epoxy resin is bisphenol A novolac epoxy resin.
5. The prepreg according to claim 1, characterized in that The (B) epoxy resin is dicyclopentadiene epoxy resin.
6. The prepreg according to claim 1, characterized in that The (B) epoxy resin is a dicyclopentadiene phenolic epoxy resin.
7. The prepreg according to claim 1, characterized in that The (B) epoxy resin is biphenyl phenolic epoxy resin.
8. The prepreg according to claim 1, characterized in that The (B) epoxy resin is a condensate of a difunctional isocyanate and an epoxy resin.
9. The prepreg according to claim 1, characterized in that The resin composition further comprises other curing agents, which are selected from any one of amine curing agents, phenolic curing agents, benzoxazine curing agents, cyanate curing agents, active ester curing agents or anhydride curing agents, or a combination of at least two thereof.
10. The prepreg according to claim 1, characterized in that The resin composition further includes an inorganic filler.
11. The prepreg according to claim 10, characterized in that The inorganic filler includes any one of non-metallic oxides, metal nitrides, non-metallic nitrides, inorganic hydrates, inorganic salts, metal hydrates or inorganic phosphorus, or a combination of at least two thereof.
12. The prepreg according to claim 10, characterized in that The inorganic filler is selected from any one or a combination of at least two of fused silica, crystalline silica, spherical silica, hollow silica, aluminum hydroxide, aluminum oxide, talc, aluminum nitride, boron nitride, silicon carbide, barium sulfate, barium titanate, strontium titanate, calcium carbonate, calcium silicate or mica.
13. A laminate comprising at least one prepreg according to any one of claims 1 to 12.
14. A metal foil-clad laminate, comprising at least one prepreg according to any one of claims 1 to 12 and a metal foil covering one side or both sides of the prepreg.