A heat treatment process for GH4706 alloy and its obtained forgings and applications
Through the heat treatment process of GH4706 alloy, including solid solution heat treatment and graded cooling, the precipitation state of the alloy is controlled, which solves the difficulty of structural control and residual stress problems of turbine disk forgings, improves its room temperature impact, tensile and high temperature durability properties, and extends the service life of the alloy. Service life.
Patent Information
- Application Number
- CN202310607896.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-05-26
AI Technical Summary
GH4706 alloy large-size turbine disk forgings have problems such as difficulty in microstructure control and excessive residual stress in high-temperature and high-stress environments, which affects its long-term service performance and machining accuracy.
The heat treatment process of GH4706 alloy is adopted, including solid solution heat treatment, graded cooling and double-stage aging treatment. By adjusting the cooling rate and temperature, the precipitation state of γ' phase, γ" phase and eta phase is controlled, reducing residual stress and improving the strength of forgings. Room temperature impact, room temperature tensile and high temperature durability properties.
It effectively improves the comprehensive performance of GH4706 alloy large-size turbine disk forgings, extends its long-term service life, reduces micro-deformation and notch sensitivity, enhances the ability to hinder crack expansion, and meets the performance requirements of heavy-duty gas turbines and other components.
Smart Images

Figure CN116804260B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of high-temperature alloy structure and performance control, and specifically to a heat treatment process for a GH4706 alloy and the obtained forgings and applications. Background Art
[0002] Large-sized high-temperature alloy components are widely used in turbine discs for heavy-duty gas turbines, nuclear reactor pressure vessels, ship-mounted gas turbine discs, and aerospace components. Among them, large-sized turbine discs are used in heavy-duty gas turbines and need to serve for more than 100,000 hours in high temperature, high stress, high speed, and corrosive gas environments. Therefore, the requirements for the uniformity of the organization and the stability of the performance of large-sized turbine discs are stringent. With the continuous improvement of the thermal efficiency and power of heavy-duty gas turbines, the blank diameter of large-sized turbine discs has reached more than 2,200 mm, the weight exceeds 10 tons, and the service environment is close to 600°C.
[0003] According to the structural design characteristics of heavy-duty gas turbines, large-size turbine disks are non-maintainable and have unique components, and the integrated regulation of their organization, performance and residual stress plays a very prominent role.
[0004] GH4706 alloy is a precipitation-strengthened high-temperature alloy. The main strengthening phases are γ' phase, γ" phase and η phase precipitated in a suitable state at the grain boundary. The recrystallization temperature of the alloy is about 975℃, and the thermal deformation is in the single-phase region. Therefore, heat treatment (solution + aging) is the last way to regulate the microstructure and properties of GH4706 alloy. Solution heat treatment includes variables such as solution temperature, solution time, and cooling rate after solution, which affect the evolution behavior of the alloy's grains and strengthening phases.
[0005] In recent years, improving alloy performance by adjusting the organization through solution heat treatment has been one of the main research hotspots. In order to improve the core performance of large-sized turbine disks, rapid cooling after solution treatment is usually adopted to suppress the reduction of endurance performance due to the increase in the size of the η phase at the grain boundary. However, this method greatly increases the residual stress of the alloy, increases the notch sensitivity, and reduces the ability of the alloy to hinder crack propagation, which is not conducive to the long-term service of large-sized turbine disks. At the same time, it is easy to cause micro-deformation during machining and affect the dimensional accuracy of the workpiece. Another way to improve the performance of the alloy is to add a high-temperature aging treatment (stabilization treatment) after solution cooling. By changing the precipitation state of the η phase at the grain boundary, it presents a cellular precipitation that is alternately arranged with the matrix, thereby improving the alloy's endurance and room temperature tensile properties. At the same time, adding an aging treatment can reduce the residual stress of the wheel to a certain extent. However, the η phase of the GH4706 alloy (the main component element is Ni 3 Ti) precipitates in large quantities, reducing the intragranular strengthening phase γ' phase (Ni 3At the same time, the η phase is a brittle phase at room temperature, which is not conducive to the room temperature impact performance of large-size turbine disks of GH4706 alloy. Summary of the invention
[0006] In view of the problems of difficult microstructure control and excessive residual stress in large-size turbine disk forgings made of GH4706 alloy, the present application provides a heat treatment process for GH4706 alloy and the forgings obtained therefrom and their applications.
[0007] In a first aspect, the present application provides a heat treatment process for a GH4706 alloy, specifically comprising the following steps: solution heat treatment, furnace-out graded cooling, and two-stage aging treatment;
[0008] The specific steps of the furnace-out graded cooling are as follows: firstly slowly cooling the GH4706 alloy after the solution heat treatment to the graded cooling temperature and then rapidly cooling to room temperature;
[0009] The cooling classification temperature is 10-50°C higher than the peak precipitation temperature of the grain boundary strengthening phase of the GH4706 alloy, the cooling rate of the slow cooling is 0.5-10°C / min, and the cooling rate of the fast cooling is 4-22°C / min.
[0010] Based on the precipitation characteristics of η phase of GH4706 alloy calculated by JMatpro, this application adopts the system of graded cooling after solid solutionization, combining the advantages of rapid cooling and stabilization treatment after solid solutionization, to achieve the goal of regulating the precipitation phase and reducing the residual stress of the alloy. At the same time, in order to obtain more consistent organizational characteristics at the core and edge positions of large-sized turbine disk forgings of GH4706 alloy, this application adopts a system of slow cooling first and then rapid cooling in the graded cooling step, which can avoid the core of the large-sized turbine disk forgings from growing the γ' phase, γ" phase and η phase due to too slow cooling rate, thereby reducing the strengthening effect, and can also reduce the increase of residual stress in large-sized turbine disk forgings due to too fast cooling rate.
[0011] By adopting the above technical scheme, the present application performs step-cooling after solution heat treatment of the GH4706 alloy, and selects appropriate cooling step temperature and cooling rate, thereby reasonably regulating the precipitation state of the γ' phase, γ" phase and η phase of the GH4706 alloy, effectively improving the room temperature impact, room temperature tensile and high temperature endurance properties of the GH4706 alloy large-size turbine disk forgings to meet the performance requirements of the turbine disk; at the same time, the residual stress generated in the alloy preparation process can be reduced, thereby reducing the micro-deformation and notch sensitivity of the GH4706 high-temperature alloy large-size turbine disk forgings caused by stress during subsequent machining and service, and improving the ability of the alloy to hinder crack propagation, thereby improving the long-term service life of the GH4706 alloy large-size turbine disk forgings, and ensuring the comprehensive performance of the GH4706 alloy large-size turbine disk.
[0012] Preferably, the cooling rate of the slow cooling is lower than the cooling rate of the fast cooling.
[0013] According to experimental analysis, in the furnace-out graded cooling step, when the slow cooling rate is greater than the fast cooling rate, the room temperature tensile and endurance properties of the large-sized turbine disk forgings of the GH4706 alloy are poor. Therefore, the technical solution of the present application controls the slow cooling rate to be less than the fast cooling rate.
[0014] Preferably, the cooling classification temperature is 810-850°C.
[0015] In a specific embodiment, the cooling classification temperature may be 810°C, 825°C, 840°C, or 850°C.
[0016] In some specific embodiments, the cooling and classification temperature may also be 810-825°C, 810-840°C, 825-840°C, 825-850°C, 840-850°C.
[0017] Preferably, the slow cooling rate is 5-10°C / min.
[0018] In a specific embodiment, the cooling rate of the slow cooling can be 0.5°C / min, 0.55°C / min, 4.28°C / min, 5°C / min, 5.18°C / min, 8.54°C / min, or 10°C / min.
[0019] Preferably, the cooling rate of the rapid cooling is 10-22°C / min.
[0020] In a specific embodiment, the cooling rate of the rapid cooling can be 4°C / min, 5.57°C / min, 10°C / min, 15°C / min, or 22°C / min.
[0021] Through experimental analysis, it can be known that when the GH4706 alloy large-size turbine disk forging is a full-size turbine disk (GH4706 alloy full-size disk with a diameter greater than 2000mm and a thickness of 175-425mm), in order to obtain more consistent organizational characteristics at the core and edge positions of the GH4706 alloy large-size turbine disk forging, the present application controls the cooling rate of slow cooling and the cooling rate of fast cooling to the above-mentioned range.
[0022] Preferably, during the solution heat treatment, the temperature is 940-980°C.
[0023] Furthermore, in the solution heat treatment, the temperature is 965-980°C.
[0024] In a specific embodiment, the solution heat treatment temperature may be 940°C, 965°C, or 980°C.
[0025] In the heat treatment process of the GH4706 alloy provided in the present application, the solution heat treatment temperature is 10-50°C higher than the precipitation temperature of the γ′ phase of the intragranular strengthening phase of the GH4706 alloy (910-930°C), that is, 940-980°C; solution heat treatment of the GH4706 alloy within this temperature range can reduce the atomic migration speed of the intragranular strengthening phase during the solution process, ensure the uniformity of the structure of large-sized turbine disk forgings under long-term heat preservation, and promote the precipitation of the grain boundary strengthening phase (the initial precipitation temperature of the grain boundary strengthening phase η phase is 940-960°C, and the peak precipitation temperature is 800°C). The grain boundary strengthening phase after the solution heat treatment can hinder the expansion of the grain boundaries and can refine the grains, thereby improving the room temperature impact, room temperature tensile and high temperature endurance properties of the large-sized turbine disk forgings of the GH4706 alloy.
[0026] Furthermore, the material to be heat-treated in the present application is a large-sized turbine disk forging of GH4706 alloy. Compared with the rod material, its initial thermal deformation grain size is larger and needs to be regulated in the solid solution heat treatment stage. Therefore, the temperature in the solid solution heat treatment is optimized to 965-980°C in the present application, which can further regulate the precipitation state of the γ′ phase, γ" phase and η phase of the GH4706 alloy, thereby improving the room temperature impact, room temperature tensile and high temperature endurance properties of the large-sized turbine disk forging of GH4706 alloy.
[0027] Preferably, in the solution heat treatment, the holding time is 2-8 hours.
[0028] The present invention controls the treatment temperature and holding time of the solution heat treatment, and can adjust the size and quantity of the intragranular strengthening phases γ′ phase, γ" phase and the grain boundary strengthening phase η phase, thereby improving the impact, tensile and durability properties of the large-size turbine disk forgings of the GH4706 alloy.
[0029] Preferably, in the double-stage aging treatment, the treatment temperature of the primary aging treatment is 720-740° C., and the treatment time is 8-18 h; the treatment temperature of the secondary aging treatment is 610-630° C., and the treatment time is 8-36 h.
[0030] By adopting the above technical solution, the present application adopts the method of high temperature aging first and low temperature aging later to ensure that the alloy strengthening phases γ' and γ" phases can be fully precipitated, so that the GH4706 alloy large-size turbine disk forgings have good impact toughness and can further improve the tensile strength and durability of the forgings.
[0031] In a second aspect, the present application provides a large-size turbine disk forging of GH4706 high-temperature alloy prepared using the above-mentioned heat treatment process.
[0032] The room temperature impact energy of the GH4706 high-temperature alloy large-size turbine disk forging provided in the present application is ≥52J, the tensile strength is ≥1228MPa, the yield strength is ≥1029MPa, the elongation is ≥19%, the cross-sectional shrinkage is ≥28%, the endurance time under the test conditions of 650℃ / 690MPa is ≥38h, and the elongation is ≥4%.
[0033] In a third aspect, the present application provides the use of the above-mentioned GH4706 high-temperature alloy large-size turbine disk forgings in the preparation of heavy-duty gas turbine disk forgings and large-size ring parts and rotating shafts.
[0034] The GH4706 high-temperature alloy large-size turbine disk forgings prepared using the technical solution provided in the present application have excellent room temperature impact, room temperature tensile and high temperature endurance properties, while meeting the long-term service performance requirements of the forgings, ensuring the comprehensive performance of the GH4706 alloy large-size turbine disk, and can be widely used in turbine disks for heavy-duty gas turbines, large-size ring parts, rotating shafts and other components.
[0035] In summary, the technical solution of this application has the following effects:
[0036] The present invention performs graded cooling after solution heat treatment of GH4706 alloy, and selects appropriate graded cooling temperature and cooling rate according to the precipitation characteristics of η phase of GH4706 alloy, so as to realize reasonable regulation of precipitation states of γ' phase, γ" phase and η phase of GH4706 alloy, and effectively improve room temperature impact, room temperature tensile and high temperature endurance properties of forgings after treatment; at the same time, the residual stress generated in the alloy preparation process can be reduced, thereby reducing the micro deformation and notch sensitivity caused by the residual stress in the subsequent machining and service process of the forging, and improving the ability of the alloy to hinder crack propagation, thereby improving the long-term service life of GH4706 alloy large-size turbine disk forgings, and ensuring the comprehensive performance of GH4706 alloy large-size turbine disks. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a schematic diagram of the graded cooling system after solutionizing in the embodiment of the present application.
[0038] Figure 2 These are the precipitation phase morphologies of the forgings after treatment in Example 1 and Comparative Examples 4-7 of the present application; wherein A1 represents Example 1, A2 represents Comparative Example 4, A3 represents Comparative Example 5, A4 represents Comparative Example 6, and A5 represents Comparative Example 7.
[0039] Figure 3 These are the precipitation phase morphologies of the forgings after treatment in Examples 16 and 18 of the present application; wherein B1 represents Example 16, and B2 represents Example 18. DETAILED DESCRIPTION
[0040] GH4706 alloy is one of the most advanced materials for manufacturing super-large wheel forgings. The main chemical composition of GH4706 alloy is: 0.2wt% Al, 1.8wt% Ti, 3wt% Nb, 0.03wt% Co, 16wt% Cr, 38wt% Fe, Ni balance. The initial precipitation temperature of the γ' phase of the intragranular strengthening phase of GH4706 alloy calculated by JMatpro software is 910-930℃, the initial precipitation temperature of the η phase of the alloy grain boundary strengthening phase is 940-960℃, and the peak precipitation temperature T η峰 It is 800℃.
[0041] According to the precipitation characteristics of η phase in GH4706 alloy calculated by JMatpro, combined with the advantages of rapid cooling and stabilization treatment after solutionizing, a cooling rate grading system after solutionizing was adopted to achieve the goals of regulating the precipitation phase and reducing the residual stress of the alloy.
[0042] In order to obtain relatively consistent precipitation phase characteristics at the center and edge of a large-sized turbine disk, in a first aspect, the present application provides a heat treatment process for a GH4706 alloy, specifically comprising the following steps:
[0043] Solution heat treatment, graded cooling after furnace exit, and two-stage aging treatment;
[0044] Among them, the specific steps of furnace-out graded cooling are: first slowly cooling the GH4706 alloy after solution heat treatment to the cooling graded temperature and then quickly cooling to room temperature; the cooling graded temperature is 10-50°C (i.e. 810-850°C) higher than the peak precipitation temperature of the grain boundary strengthening phase of the GH4706 alloy, the cooling rate of slow cooling is 0.5-10°C / min, preferably 5-10°C / min, and the cooling rate of fast cooling is 4-22°C / min, preferably 10-22°C / min; preferably, the cooling rate of slow cooling is less than the cooling rate of fast cooling.
[0045] In a specific implementation scheme, the cooling rate of slow cooling and the cooling rate of fast cooling can be determined in combination with the size of the produced forgings in actual production.
[0046] Specifically, in the solution heat treatment, the temperature is 940-980°C and the holding time is 2-8h; in the double-stage aging treatment, the treatment temperature of the primary aging treatment is 720-740°C and the treatment time is 8-18h, and the treatment temperature of the secondary aging treatment is 610-630°C and the treatment time is 8-36h.
[0047] In a second aspect, the present application provides a large-size turbine disk forging of GH4706 high-temperature alloy prepared using the above-mentioned heat treatment process.
[0048] In a third aspect, the present application provides the use of the above-mentioned GH4706 high-temperature alloy large-size turbine disk forgings in the preparation of heavy-duty gas turbine disk forgings and large-size ring parts and rotating shafts.
[0049] The present application is further described in detail below in conjunction with examples, comparative examples and performance testing experiments. These examples should not be construed as limiting the scope of protection claimed in the present application.
[0050] Example
[0051] Examples 1-5
[0052] Examples 1-5 provide a heat treatment process for a GH4706 alloy.
[0053] The schematic diagram of the post-solutionizing step cooling system in Examples 1-5 is as follows: Figure 1 As shown, the specific steps include: the GH4706 alloy in the above embodiment is a sub-sized disk with a diameter of 1500 mm and a thickness of 160 mm after forging; since the service temperature of the large-sized turbine disk of the GH4706 alloy is 600°C, the evolution behavior of the alloy precipitation phase is very slow at this temperature, and it is of no practical significance to count the cooling rate to room temperature; therefore, in the test process, only the cooling rate of the GH4706 alloy when it is quickly cooled to 600°C is counted; at the same time, the cooling classification temperature is set to 825°C (that is, the peak precipitation temperature T η峰 +25℃).
[0054] (1) Solution heat treatment: The GH4706 alloy was solution heat treated at 980 °C for 4 h.
[0055] (2) Step cooling: The GH4706 alloy after solution heat treatment is first slowly cooled to the cooling step temperature and then quickly cooled to room temperature. The temperature change is monitored by inserting a temperature measuring couple at the center. The different step cooling systems in Examples 1-5 are shown in Table 1.
[0056] (3) Two-stage aging treatment: keep at 720℃ for 8h, then cool to 620℃ at a cooling rate of 55℃ / h and keep at 8h to obtain the forging.
[0057] Table 1 Graded cooling system after solution treatment of GH4706 alloy sub-sized disks in Examples 1-5
[0058]
[0059] Example 6
[0060] This embodiment provides a heat treatment process for GH4706 alloy.
[0061] The difference between this embodiment and embodiment 1 is that the classification temperature of the classification cooling after being discharged from the furnace in step (2) is different. The specific steps are as follows:
[0062] (2) Step cooling after exiting the furnace: The step cooling temperature is set to 810°C (i.e., the peak precipitation temperature T η峰+ 10°C), the GH4706 alloy after solution heat treatment was slowly cooled to 810°C at a cooling rate of 0.55°C / min, and then quickly cooled to room temperature at a cooling rate of 5.57°C / min.
[0063] Example 7
[0064] This embodiment provides a heat treatment process for GH4706 alloy.
[0065] The difference between this embodiment and embodiment 1 is that the classification temperature of the classification cooling after being discharged from the furnace in step (2) is different. The specific steps are as follows:
[0066] (2) Step cooling after exiting the furnace: The step cooling temperature is set to 850°C (i.e., the peak precipitation temperature T η峰 +50℃), the GH4706 alloy after solution heat treatment was slowly cooled to 850℃ at a cooling rate of 0.55℃ / min, and then quickly cooled to room temperature at a cooling rate of 5.57℃ / min.
[0067] Example 8
[0068] This embodiment provides a heat treatment process for GH4706 alloy.
[0069] The difference between this embodiment and embodiment 1 is that the solution heat treatment in step (1) is: subjecting the GH4706 alloy to solution heat treatment at 965° C. for 4 hours.
[0070] Example 9
[0071] This embodiment provides a heat treatment process for GH4706 alloy.
[0072] The difference between this embodiment and embodiment 1 is that the solution heat treatment in step (1) is: subjecting the GH4706 alloy to solution heat treatment at 940° C. for 4 hours.
[0073] Comparative Example
[0074] Comparative Example 1
[0075] This comparative example provides a heat treatment process for GH4706 alloy.
[0076] The difference between this comparative example and Example 1 is that: in step (2), the cooling out of the furnace does not adopt a graded cooling system, and the specific steps are:
[0077] (2) Cooling after solution heat treatment: The GH4706 alloy was slowly cooled to room temperature at a cooling rate of 3°C / min.
[0078] Comparative Example 2
[0079] This comparative example provides a heat treatment process for GH4706 alloy.
[0080] The difference between this comparative example and Example 1 is that the classification temperature of the classification cooling after being discharged from the furnace in step (2) is different. The specific steps are as follows:
[0081] (2) Step cooling after exiting the furnace: The step cooling temperature is set to 800°C (i.e., the peak precipitation temperature T η峰 ), the GH4706 alloy after solution heat treatment was slowly cooled to 800°C at a cooling rate of 0.55°C / min, and then quickly cooled to room temperature at a cooling rate of 5.57°C / min.
[0082] Comparative Example 3
[0083] This comparative example provides a heat treatment process for GH4706 alloy.
[0084] The difference between this comparative example and Example 1 is that the classification temperature of the classification cooling after being discharged from the furnace in step (2) is different. The specific steps are as follows:
[0085] (2) Step cooling after exiting the furnace: The step cooling temperature is set to 860°C (i.e., the peak precipitation temperature T η峰 +60℃), the GH4706 alloy after solution heat treatment was slowly cooled to 860℃ at a cooling rate of 0.55℃ / min, and then quickly cooled to room temperature at a cooling rate of 5.57℃ / min.
[0086] Comparative Examples 4-7
[0087] Comparative Examples 4-7 respectively provide a heat treatment process for a GH4706 alloy.
[0088] The difference between the comparative example and the embodiment 1 is that the graded cooling system of the graded cooling out of the furnace in step (2) is different, as follows:
[0089] (2) Step cooling after exiting the furnace: The step cooling temperature is set to 825°C (i.e., the peak precipitation temperature T η峰 +25℃), and the temperature change is monitored by inserting a thermocouple in the center.
[0090] The temperature change was monitored by inserting a temperature measuring couple at the center. The different graded cooling systems in Comparative Examples 4-7 are shown in Table 2.
[0091] Table 2 Graded cooling system of GH4706 alloy after solution treatment in Comparative Examples 4-7
[0092]
[0093] Performance test 1
[0094] The forgings treated in Examples 1-9 and Comparative Examples 1-7 were used as test objects, and their mechanical properties and microstructures of precipitated phases were tested.
[0095] The mechanical properties of the forgings after treatment in Examples 1-9 and Comparative Examples 1-7 are shown in Table 3.
[0096] The morphology of the precipitation phase of the forgings after treatment in Example 1 and Comparative Examples 4-7 is as follows: Figure 2 As shown; wherein A1 represents Example 1, A2 represents Comparative Example 4, A3 represents Comparative Example 5, A4 represents Comparative Example 6, and A5 represents Comparative Example 7.
[0097] Table 3 Mechanical properties of forgings in Examples 1-9 and Comparative Examples 1-7
[0098]
[0099]
[0100] Combined with Table 3, according to the test results of Comparative Examples 1-9 and Comparative Examples 1-7, it can be known that in the heat treatment process of GH4706 alloy, the present application performs graded cooling of the alloy after solution heat treatment, and selects appropriate cooling graded temperature and cooling rate, thereby reasonably regulating the precipitation state of γ' phase and η phase of GH4706 alloy, effectively improving the room temperature impact, room temperature tensile and high temperature endurance properties of GH4706 alloy large-size wheel disk forgings, and at the same time reducing the residual stress generated in the preparation process, improving the long-term service reliability of GH4706 alloy large-size turbine disk forgings, and ensuring the comprehensive performance of GH4706 alloy large-size turbine disks.
[0101] In Comparative Example 1, no graded cooling system was used for the cooling out of the furnace. When the GH4706 alloy after solution heat treatment was cooled at a rate of 3°C / min, the room temperature impact energy of the forging after treatment was 49J, the tensile strength was 1227MPa, the yield strength was 995MPa, the elongation was 22%, the cross-sectional shrinkage was 35%, the endurance time under the test conditions of 650°C / 690MPa was 40h, and the elongation was 5%.
[0102] When the cooling and grading temperature of the furnace-out graded cooling in Comparative Example 2 is 800°C, the room temperature impact energy of the forging after treatment is 53J, the tensile strength is 1225MPa, the yield strength is 1005MPa, the elongation is 24%, the cross-sectional shrinkage is 36%, the endurance time under the test conditions of 650°C / 690MPa is 38h, and the elongation is 3%. When the cooling and grading temperature of the furnace-out graded cooling in Comparative Example 3 is 860°C, the room temperature impact energy of the forging after treatment is 58J, the tensile strength is 1219MPa, the yield strength is 1012MPa, the elongation is 23%, the cross-sectional shrinkage is 37%, the endurance time under the test conditions of 650°C / 690MPa is 33h, and the elongation is 3%.
[0103] Combination Figure 2 The morphology of the precipitated phase of the forging after the medium treatment, although the cooling graded temperature in Examples 4-6 is set to 825°C, Example 4 is first furnace cooled to 825°C and then cotton cooled (the cooling rate of fast cooling is too slow), Example 5 is air cooled throughout the process (the cooling rate of slow cooling is too fast), and Example 6 is water cooled throughout the process (the cooling rate of the whole process is too fast). The room temperature impact properties of the forgings treated with the above three schemes can meet the requirements, but the room temperature tensile strength of Example 4 and the endurance properties of the forgings treated with the three schemes under 650°C / 690MPa conditions are all poor.
[0104] Although the cooling stage temperature in Comparative Example 7 is set to 825°C, during the cooling process, the scheme first furnace cools to 825°C and then keeps it warm for 3.5 hours, and then air cools it. Although the forgings treated by this scheme have excellent durability, after the insulation treatment, a large amount of η phase of the GH4706 alloy is precipitated, which reduces the precipitation amount of the intragranular strengthening phase γ' phase. The η phase is a brittle phase at room temperature, which greatly reduces the impact performance, which is not conducive to the actual service of large-size turbine disks for heavy-duty gas engines.
[0105] Compared with Comparative Examples 1-7, and combined with Figure 2 The morphology of the precipitated phase of the forging after treatment in Example 1, the cooling out of the furnace in Examples 1-9 of the present application adopts a graded cooling system, and is first slowly cooled to the cooling graded temperature (810-850°C) at a cooling rate of 0.5-10°C / min and then quickly cooled at a cooling rate of 4-22°C / min. The room temperature impact energy of the forging after treatment reaches more than 52J, the tensile strength is ≥1228MPa, the yield strength is ≥1029MPa, the elongation is ≥19%, the cross-sectional shrinkage is ≥28%, the endurance time under the test conditions of 650°C / 690MPa is ≥38h, and the elongation is ≥4%. The results show that the forgings treated by the treatment process of the present application have good comprehensive mechanical properties.
[0106] By comparing the test results of Examples 1, 8-9, when the temperature of the solution heat treatment is lower than 965°C, the η phase of the grain boundary strengthening phase of the GH4706 alloy is not completely dissolved (the initial precipitation temperature is 940-960°C, and the peak precipitation temperature is 800°C), and it is easy to grow into a needle shape and precipitate inside the crystal in the subsequent slow cooling stage, so that the room temperature impact, room temperature tensile and high temperature rupture properties of the forgings after treatment are inferior to those of the forgings treated when the solution heat treatment temperature is higher than 965°C. Therefore, the present application optimizes the temperature of the solution heat treatment to 965-980°C.
[0107] From the above, it can be seen that the goal of regulating the precipitation phase and reducing the residual stress of the alloy can be achieved by reasonably controlling the graded cooling system after the solution heat treatment of the GH4706 alloy for super-large wheel forgings, so that the center and edge positions of the large-size turbine disk of the GH4706 alloy can obtain more consistent precipitation phase characteristics, and improve the room temperature impact, room temperature tensile and high temperature endurance properties of the forgings after treatment.
[0108] Examples 10-18
[0109] Examples 10-18 respectively provide a heat treatment process for a GH4706 alloy.
[0110] The GH4706 alloy in the above embodiment is a full-size disk of GH4706 alloy having a diameter greater than 2000 mm and a thickness of 175-425 mm after forging.
[0111] The heat treatment process of the GH4706 alloy in the above embodiment specifically includes the following steps:
[0112] (1) Solution heat treatment: The GH4706 alloy was solution heat treated at 980 °C for 4 h.
[0113] (2) Step cooling: The GH4706 alloy after solution heat treatment is first slowly cooled to the cooling step temperature and then quickly cooled to room temperature. The temperature change is monitored by inserting a temperature measuring couple at the center. The different step cooling systems in Examples 10-18 are shown in Table 4.
[0114] (3) Two-stage aging treatment: keep at 720℃ for 8h, then cool to 620℃ at a cooling rate of 55℃ / h and keep at 8h to obtain the forging.
[0115] Table 4 Graded cooling system after solution treatment of full-size disk of GH4706 alloy in Examples 10-18
[0116]
[0117] Performance test 2
[0118] The forgings treated in Examples 10-18 were used as test objects to test their respective mechanical properties and microstructures of the precipitated phases.
[0119] The mechanical properties of the forgings after treatment in Examples 10-18 are shown in Table 5.
[0120] The morphology of the precipitated phase of the forgings after treatment in Example 16 and Example 18 is as follows: Figure 3 As shown; wherein, B1 represents Example 16 and B2 represents Example 18.
[0121] Table 5 Mechanical properties of forgings in Examples 10-18
[0122]
[0123] Combined with the mechanical properties test results of the large-size turbine disk forgings of GH4706 alloy in actual production in Table 5 and Figure 3 From the morphology of the precipitated phase of the forging, it can be seen that when the GH4706 alloy in actual production is a GH4706 alloy full-size disk with a diameter greater than 2000mm and a thickness of 175-425mm after forging, Examples 10-12 use slow cooling with a cooling rate that is too slow, and Examples 13 and 16 use fast cooling with a cooling rate that is too slow, so that the core position of the full-size wheel forging reduces the performance due to the slow cooling rate; while the schemes in Examples 14-15 and Examples 17-18 control the cooling rate in the slow cooling process to 5-10℃ / min, and the cooling rate in the fast cooling process to 10-22℃ / min. After treatment, the forgings have significantly improved room temperature tensile and endurance properties while maintaining comparable impact properties. Therefore, in order to obtain relatively consistent organizational characteristics at the core and edge of the GH4706 alloy large-size turbine disk forging, in the preferred scheme of the GH4706 alloy large-size turbine disk forging in actual production of the present application, it is necessary to control the cooling rate in the graded cooling within the above range.
[0124] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A heat treatment process for GH4706 alloy, characterized in that: The specific steps include: Solution heat treatment, graded cooling after furnace exit, and two-stage aging treatment; The specific steps of the furnace-out graded cooling are as follows: firstly slowly cooling the GH4706 alloy after the solution heat treatment to the graded cooling temperature and then directly fast cooling to room temperature; The cooling classification temperature is 10-50°C higher than the peak precipitation temperature of the grain boundary strengthening phase of the GH4706 alloy, the cooling rate of the slow cooling is 0.5-10°C / min, and the cooling rate of the fast cooling is 4-22°C / min; the cooling rate of the slow cooling is lower than the cooling rate of the fast cooling; The GH4706 alloy grain boundary strengthening phase is η phase, the GH4706 alloy grain boundary strengthening phase peak precipitation temperature is 800° C., and the cooling classification temperature is 810-850° C.; In the solution heat treatment, the temperature is 965-980° C. and the holding time is 2-8 hours.
2. The heat treatment process of GH4706 alloy according to claim 1, characterized in that: The cooling rate of the rapid cooling is 10-22°C / min.
3. The heat treatment process of GH4706 alloy according to claim 1, characterized in that: In the double-stage aging treatment, the treatment temperature of the first-stage aging treatment is 720-740° C., and the treatment time is 8-18 hours; the treatment temperature of the second-stage aging treatment is 610-630° C., and the treatment time is 8-36 hours.
4. A GH4706 high-temperature alloy large-size turbine disk forging prepared by the heat treatment process described in any one of claims 1 to 3.
5. The GH4706 high temperature alloy large-size turbine disk forging according to claim 4 is characterized in that: The room temperature impact energy of the GH4706 high-temperature alloy large-size turbine disk forging is ≥52J, the tensile strength is ≥1228MPa, the yield strength is ≥1029MPa, the elongation is ≥19%, the cross-sectional shrinkage is ≥28%, the endurance time under the test conditions of 650°C / 690MPa is ≥38h, and the elongation is ≥4%.
6. Use of the GH4706 high-temperature alloy large-size turbine disk forging according to any one of claims 4 to 5 in the preparation of heavy-duty gas turbine disk forgings, large-size ring parts and rotating shafts.