A phosphorylated chitin composite material and its preparation and application

Fe3O4@PCT, a composite material formed by phosphorylated chitin and ferrotetraoxide microspheres, solved the problem of poor adsorption effect of bentonite and low polyphenol retention rate in the prevention and control of turbidity after fruit wine, and achieved chitinase The high-efficiency adsorption and significant retention of polyphenols have improved the quality of fruit wine.

CN116809033BActive Publication Date: 2024-12-06XIHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310900140.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-21
Publication Date
2024-12-06
Estimated Expiration
2043-07-21

AI Technical Summary

Technical Problem

In the prior art, when preventing turbidity after fruit wine, the use of bentonite leads to protein removal and also loses physiological active ingredients, such as polyphenols, resulting in a decrease in the quality of fruit wine, and the adsorption effect of bentonite on chitinase is not good.

Method used

Using the phosphorylated chitin composite material Fe3O4@PCT, by combining chitin powder with phosphorylated agent and ferrous tetraoxide microspheres, a composite material with magnetic effect is formed, and chitin enzymes are specifically adsorbed, and polyphenols are improved. retention rate.

Benefits of technology

It significantly improves the retention rate of polyphenols in fruit wine, improves the quality of fruit wine, and provides an efficient and low-cost solution, overcoming the problems of poor adsorption effect of bentonite and low polyphenol retention rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116809033B_ABST
    Figure CN116809033B_ABST
Patent Text Reader

Abstract

The present invention discloses a phosphorylated chitin composite material and its preparation and application. The present invention phosphorylates chitin and then composites phosphorylated chitin with ferroferric oxide microspheres to obtain a composite material Fe3O4@PCT, which can specifically adsorb chitinase. Compared with bentonite and unmodified chitin, the composite material has better adsorption of chitinase, and at the same time improves the retention rate of polyphenols in fruit wine, which is beneficial to improving the quality of fruit wine, and has significant economic value and application value in the application of post-turbidity prevention and control of fruit wine or in the adsorption of chitinase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of prevention and control of post-haze turbidity in fruit wine, and in particular to a phosphorylated chitin composite material and a preparation method and application thereof. Background Art

[0002] The post-haze phenomenon in fruit wine is a sensory quality defect that occurs during transportation or storage. Although post-haze may have little effect on taste and flavor, it will bring an unpleasant experience to consumers. At present, studies have shown that proteins that cause post-haze formation in fruit wine and beverages are commonly found in plant raw materials. As reported in the literature (Roles of Grape Thaumatin-like Protein and Chitinase in White Wine Haze Formation. JOURNAL OF AGRICULTURAL AND FOOD CHEMISTRY, 2021, 59 (2): 733-740), grape chitinase is the main protein causing heat-induced haze in unrefined wine, and the final stage of chitinase aggregation has been shown to be irreversible and closely related to visible haze. In order to prevent the formation of post-haze, bentonite is usually added in the commercial industry to remove proteins. However, bentonite treatment not only removes turbidity-causing proteins, but also removes physiologically active ingredients, such as polyphenols, resulting in quality loss. Therefore, a protein selective removal technology is needed to control the post-haze of fruit wine while retaining physiologically active ingredients as much as possible to improve the quality of fruit wine. Summary of the invention

[0003] The purpose of the present invention is to provide a phosphorylated chitin composite material and its preparation and application. The phosphorylated chitin composite material provided by the present invention can specifically adsorb chitinase, significantly improves the retention rate of polyphenols compared with bentonite, and has significant application value in preventing and controlling post-haze of fruit wine.

[0004] In order to achieve the above object, the present invention provides a method for preparing a phosphorylated chitin composite material Fe3O4@PCT, comprising the following steps:

[0005] 1) mixing chitin powder with P2O5, H3PO4, triethyl phosphate and hexanol for reaction;

[0006] 2) precipitating the reaction mixture in methanol, filtering the precipitate and drying it to obtain phosphorylated chitin;

[0007] 3) dispersing the phosphorylated chitin in a mixed solution of sodium hydroxide, urea and water, and obtaining a phosphorylated chitin solution through a freeze-thaw process;

[0008] 4) dispersing the ferrosoferric oxide microspheres into water, mixing with the phosphated chitin solution obtained in step 3), adding a mixed solution of Span 85 and isooctane, stirring the obtained mixed system, and then adding Span 85 and isooctane and continuing to stir;

[0009] 5) heating the product in step 4) to form phosphorylated chitin composite ferroferric oxide microspheres;

[0010] 6) Using a magnet to separate and wash the product obtained in step 5), and drying the obtained product to obtain the phosphorylated chitin composite material Fe3O4@PCT.

[0011] Preferably, the usage ratio of the chitin powder to P2O5, H3PO4, triethyl phosphate and hexanol is 1 g:2 g:10 mL:5 mL:5 mL.

[0012] Preferably, the reaction is carried out at 35° C. for 3 days.

[0013] Preferably, in the mixed solution of step 3), the mass ratio of sodium hydroxide, urea and ultrapure water is 2:1:22; and the weight ratio of the phosphorylated chitin to the mixed solution is 1:20.

[0014] Preferably, in the above step 4), the ratio of ferrosoferric oxide microspheres to ultrapure water is 1 g:12.5 mL.

[0015] Preferably, the stirring in the above step 4) is stirring for 60 min in an ice bath.

[0016] Preferably, the heating condition in the above step 5) is heating at 60°C.

[0017] Preferably, the washing in the above step 6) is performed using water and ethanol.

[0018] The present invention also provides a composite material Fe3O4@PCT prepared by the above preparation method.

[0019] The composite material Fe3O4@PCT provided by the present invention can be applied to the prevention and control of post-turbidity of fruit wine or in the adsorption of chitinase.

[0020] Preferably, the above application comprises the removal of turbidity-causing proteins in fruit wine and / or the retention of biologically active components.

[0021] The phosphorylated chitin composite material of the present invention and its preparation and application solve the problems of poor chitinase adsorption effect and low polyphenol retention rate of bentonite commonly used in the prevention and control of post-turbidity of fruit wine, and has the following advantages:

[0022] (1) The phosphorylated chitin composite material provided by the present invention has simple preparation steps, is easy to operate, and is green and pollution-free.

[0023] (2) The present invention connects phosphorylated chitin with ferroferric oxide magnetic beads, and the connection product has a magnetic effect and better immobilization performance. It is an efficient and low-cost adsorption material with more significant application potential.

[0024] (3) Compared with bentonite and unmodified chitin, the phosphorylated chitin composite material provided by the present invention is used in the prevention and control of post-harvest turbidity of fruit wine. The composite material can significantly improve the adsorption effect of chitinase and increase the retention rate of polyphenols in wine samples. It plays a certain role in the prevention and control of post-harvest turbidity of fruit wine and has significant economic value and application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the SEM image of Fe3O4@PCT and Fe3O4 in the present invention.

[0026] Figure 2 is the EDS spectrum of Fe3O4@PCT in the present invention, where Figure 2 A, B, C, and D in the figure are the EDS spectra of Fe, C, O, and P in Fe3O4@PCT, respectively.

[0027] Figure 3 FT-IR graph of chitin and PCT in the present invention.

[0028] Figure 4 Zeta potential diagram of Fe3O4, PCT, Fe3O4@PCT (pH=6.5), and Fe3O4@PCT (pH=4.1) in the present invention.

[0029] Figure 5 This is the result of determining the optimum adsorption temperature of Fe3O4@PCT in the present invention.

[0030] Figure 6 This is the result of determining the optimum adsorption dosage of Fe3O4@PCT in the present invention.

[0031] Figure 7 This is the result of determining the optimum adsorption time of Fe3O4@PCT in the present invention.

[0032] Figure 8 This is the SDS-PAGE analysis result of Fe3O4@PCT adsorbed protein in the present invention.

[0033] Fig. 9 This is the mass spectrometry analysis result of the protein band sample adsorbed by Fe3O4@PCT in the present invention.

[0034] Fig.10 These are the results of the adsorption of protein, polyphenols and anthocyanins by Fe3O4@PCT in the present invention.

[0035] Fig.11 These are the results of measuring the thermal stability of the wine sample after the wine sample was treated with Fe3O4@PCT in the present invention. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] In order to further improve the affinity adsorption of chitin to chitinase, the present invention uses molecular docking software to retrieve chemically modified compounds based on chitin on the website www.pubchem.com, and screens phosphorylated chitin as an adsorption substrate based on the docking score. The surface morphology research results also show that phosphorylated chitin exhibits a very porous and rough structure due to phosphorylation, which further enhances the adsorption capacity of chitin. After being connected to ferroferric oxide magnetic beads, phosphorylated chitin has a magnetic effect and better immobilization performance, and has more significant application potential.

[0038] Example 1 Preparation and characterization of composite material Fe3O4@PCT

[0039] A method for preparing a composite material for specifically selectively adsorbing chitinase comprises the following steps:

[0040] Chitin powder (Chitin, 5g) was added to a round-bottom flask, and P2O5 (10g), H3PO4 (50mL), triethyl phosphate (25mL) and hexanol (25mL) were added. The reaction was continued at 35°C for 3 days. After the reaction was completed, the reaction mixture was poured into excess methanol for precipitation. The precipitate was filtered and washed with methanol, and then dried in a vacuum oven at 37°C for 1 day to obtain the desired phosphorylated chitin (PCT);

[0041] 5 g of PCT was dispersed in a mixed solution containing sodium hydroxide (8 g), urea (4 g) and ultrapure water (88 g) to obtain a transparent phosphorylated chitin solution using a freeze-thaw process;

[0042] 0.4 g of ferrosoferric oxide microspheres (Fe3O4) were dispersed in 5 mL of ultrapure water, ultrasonically treated for 10 min, and then mixed with the above-obtained phosphated chitin solution under ice bath conditions, and a mixed solution of 1.1 g of Span 85 and 50 g of isooctane was added. The mixed solution system was stirred under ice bath conditions for 60 min, and then 0.6 g of Span85 and 3.5 g of isooctane were added, and the stirring was continued under ice bath conditions for 60 min;

[0043] After stirring, the mixture was placed in a 60°C water bath to form phosphorylated chitin composite ferroferric oxide microspheres. The product was separated using a magnet, and washed three times with water and ethanol, respectively. The product was dried to obtain a composite material phosphorylated chitin composite ferroferric oxide microspheres - Fe3O4@PCT. The prepared powdered composite material was collected for later use.

[0044] The characterization results of Fe3O4@PCT prepared above were obtained as follows: Figure 1-Figure 4 As shown, Figure 1 A in the figure is the SEM image of Fe3O4; Figure 1 B is the SEM image of Fe3O4@PCT; Figure 2 is the EDS spectrum of Fe3O4@PCT (where Figure 2 A, B, C, and D are the EDS spectra of Fe, C, O, and P in Fe3O4@PCT respectively); Figure 3 FT-IR images of chitin and PCT; Figure 4 Zeta potential diagrams of Fe3O4, PCT, Fe3O4@PCT (pH=6.5), and Fe3O4@PCT (pH=4.1).

[0045] Example 2 Determination of the optimal adsorption conditions of the composite material Fe3O4@PCT

[0046] 1. Determination of the optimal adsorption temperature

[0047] Take 5mL of fruit wine in a sample bottle, add 3mg of Fe3O4@PCT adsorption material, and place it in a constant temperature oscillator at different temperatures (25, 30, 35, 40, 45℃) for 8h. After the adsorption, separate it with a magnet and keep the supernatant to determine its protein concentration and calculate the adsorption amount. The adsorption amount calculation formula is as follows:

[0048]

[0049] Where:

[0050] Q e —Adsorption capacity (mg / g)

[0051] C0—Initial protein concentration in fruit wine (mg / mL)

[0052] C1—Protein concentration in wine after adsorption (mg / mL)

[0053] V—volume of solution (mL)

[0054] m—Mass of Fe3O4@PCT (mg)

[0055] The adsorption temperature results are as follows Figure 5 It can be seen that the protein adsorption amount is the largest when the adsorption temperature is 35℃, and 35℃ is determined to be the optimal temperature.

[0056] 2. Determination of the most suitable amount

[0057] Take 5 mL of wine in a sample bottle, add different amounts of Fe3O4@PCT adsorption material, place it in a constant temperature oscillator at 35°C for adsorption for 24 hours, separate the material with a magnet and keep the supernatant, determine the protein concentration of the supernatant, and calculate the adsorption amount in the same way as above.

[0058] The most suitable amount results are as follows Figure 6 As shown, it can be seen that when the wine sample is 5mL and the amount of the composite material is 3mg, the unit adsorption amount of the composite material is the largest, and it is determined that the amount of composite material added in 0.6g / mL wine sample is the most suitable amount.

[0059] 3. Determination of the optimal adsorption time

[0060] Take 5 mL of fruit wine in a sample bottle, add the most suitable amount of Fe3O4@PCT adsorption material, place it in a constant temperature oscillator at 35°C, adsorb for different times, separate it with a magnet after adsorption and retain the supernatant to determine its protein concentration. The method for calculating the adsorption amount is the same as above.

[0061] The adsorption time results are as follows Figure 7 It can be seen that the amount of protein tends to be saturated after 8 hours of adsorption, and 8 hours is determined to be the optimal adsorption time.

[0062] Example 3 Specific adsorption study of Fe3O4@PCT

[0063] 1. SDS-PAGE Analysis

[0064] Referring to the optimal optimization conditions obtained in Experimental Example 1, Fe3O4@PCT was added to mulberry wine, Fe3O4@PCT was collected after separation and adsorption by magnet, H2O was added and vortexed, the supernatant was collected, and then SDS (0.2%) and NaCl solution were added and vortexed to collect the supernatant. The collected supernatant was then analyzed by SDS-PAGE.

[0065] SDS-PAGE results are as follows Figure 8As shown, lane 1 is a protein molecular weight standard, lanes 2 and 3 are original samples of mulberry wine (two replicates), lanes 4 and 5 are supernatants recovered from water elution materials (two replicates), and lanes 6 and 7 are recovered supernatants eluted with 0.1% SDS and NaCl solutions (two replicates). It can be seen that in the original sample of mulberry wine (lanes 2 and 3), obvious bands in the range of 27-35 kDa were clearly observed. According to existing literature reports, the molecular weight of chitinase from plant sources is between 25 and 35 kDa, but after elution with H2O (lanes 4 and 5), almost no protein was detected in the supernatant; after elution with SDS and NaCl solutions (lanes 6 and 7), two bands in the range of 27-35 kDa appeared clearly; because SDS and NaCl destroyed the hydrophobic force and hydrogen bonds of specific adsorption, the specifically adsorbed protein was eluted, and the results showed that Fe3O4@PCT has specific adsorption for protein adsorption.

[0066] 2. Analysis of protein band samples based on nano LC-Q-Exactive-MS / MS technology

[0067] The total ion current of the protein band sample collected by high-resolution nano LC-Q-Exactive-MS / MS is shown in Fig. 9 . The collected mass spectrometry data were processed using MaxQuant 1.6.14 software, and the Andromeda and Uniprot databases were used to identify the peptide sequences and attribute the protein sources. Finally, 136 peptides were identified from the protein band trypsin hydrolyzed peptide samples, originating from 68 proteins. The top 20 proteins in terms of protein expression intensity scores are shown in Table 1 below. The molecular weight of the hydrolyzed peptide sequence is 1411.6368, and the score of this peptide relative to the entire protein is 133.71, which is equal to or greater than 35. The empirical value is credible, and the protein coverage is 46.4% (20%-50% coverage is the successful matching interval). The analysis results show that the polypeptide sequence has a high similarity with chitinase Class I (relative molecular mass: 34.943kDa). In addition, the protein coverage of this polypeptide sequence with chitinase Class I b (relative molecular mass: 33.791kDa) is 47.2%, indicating a high similarity with chitinase Class I b, which is consistent with SDS-PAGE analysis ( Figure 8 The results of the two bands in Figure 3 are shown in Figure 3. The combined SDS-PAGE analysis and nano LC-Q-Exactive-MS / MS analysis showed that Fe3O4@PCT had a good specific adsorption effect on chitinase.

[0068] Table 1 The top 20 proteins in the protein strips

[0069]

[0070]

[0071] Example 4 Effect Comparison Verification

[0072] Referring to the optimal conditions obtained in Experimental Example 1, take an appropriate amount of fruit wine in a sample bottle, add the same amount of Fe3O4@PCT, chitin and bentonite, and place it in a constant temperature oscillator for adsorption treatment. After the end, the supernatant was collected and the contents of protein, polyphenols and anthocyanin in the supernatant were determined.

[0073] The results of the test are as follows Fig.10 As shown in the figure, the adsorption rates of Fe3O4@PCT on protein, polyphenols and anthocyanins were 3.221%, 5.09% and 3.019%, respectively, which were significantly lower than those of Bentonite and Chitin treatments (the adsorption rates of Bentonite on protein, polyphenols and anthocyanins were 21.24%, 14.4% and 17.15%, respectively; the adsorption rates of Chitin on protein, polyphenols and anthocyanins were 27.21%, 18.98% and 25.32%, respectively), indicating that Fe3O4@PCT has a selective adsorption effect on protein and can significantly retain the physiologically active substances in fruit wine.

[0074] Example 5 Thermal Stability Determination

[0075] The fruit wine treated with Fe3O4@PCT, chitin and bentonite was placed in a sample bottle, first placed in an environment of 80℃ for 2h, then placed in an environment of -20℃ for 2h, and finally placed at room temperature. The change in absorbance before and after treatment was measured at 540nm. When the difference in absorbance between the heated and unheated wine sample (ΔA 540nm )>0.02, the protein is considered unstable.

[0076] The results of the test are as follows Fig.11 As shown, after treatment with bentonite, chitin and Fe3O4@PCT, ΔA 540nm They are all less than 0.02, indicating that the wine is still thermally stable after Fe3O4@PCT adsorption treatment.

[0077] In summary, the present invention phosphorylates chitin and then composites the phosphorylated chitin with ferroferric oxide microspheres to obtain a composite material Fe3O4@PCT, which can specifically adsorb chitinase. Compared with bentonite and unmodified chitin, the composite material has better adsorption of chitinase and improves the retention rate of polyphenols in fruit wine, which is beneficial to improving the quality of fruit wine and has significant economic value and application value in the application of post-turbidity prevention and control of fruit wine.

[0078] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing a phosphorylated chitin composite material Fe3O4@PCT, characterized in that: The following steps are included: 1) mixing chitin powder with P2O5, H3PO4, triethyl phosphate and hexanol for reaction, wherein the amount ratio of chitin powder to P2O5, H3PO4, triethyl phosphate and hexanol is 1g:2g:10mL:5mL:5mL, and the reaction condition is 35°C for 3 days; 2) precipitating the reaction mixture in methanol, filtering the precipitate and drying it to obtain phosphorylated chitin; 3) dispersing the phosphorylated chitin in a mixed solution of sodium hydroxide, urea and ultrapure water, and obtaining a phosphorylated chitin solution through a freeze-thaw process, wherein the mass ratio of sodium hydroxide, urea and ultrapure water in the mixed solution is 2:1:22; and the weight ratio of the phosphorylated chitin to the mixed solution is 1:20; 4) dispersing the ferroferric oxide microspheres into water, mixing with the phosphated chitin solution obtained in step 3), adding a mixed solution of Span 85 and isooctane, stirring the obtained mixed system, and then adding Span 85 and isooctane and continuing to stir, wherein the ratio of the ferroferric oxide microspheres to ultrapure water is 1 g: 12.5 mL, and the stirring is stirring for 60 min in an ice bath; 5) heating the product of step 4) at 60° C. to form phosphorylated chitin composite ferroferric oxide microspheres; 6) Using a magnet to separate and wash the product obtained in step 5), and drying the obtained product to obtain the phosphorylated chitin composite material Fe3O4@PCT.

2. The composite material Fe3O4@PCT prepared by the preparation method described in claim 1.

3. Application of the composite material Fe3O4@PCT as claimed in claim 2 in the prevention and control of post-production turbidity of fruit wine or in the adsorption of chitinase.

4. The use according to claim 3, characterized in that: The application includes removing turbidity-causing proteins in fruit wine and / or retaining biologically active components.