A high-efficiency dephosphorization electric furnace smelting method

The two-stage electric furnace smelting method with controlled slag retention and removal enhances dephosphorization efficiency, shortening the cycle and reducing costs by stabilizing thermodynamic and kinetic conditions, achieving efficient dephosphorization and environmental benefits.

CN116814900BActive Publication Date: 2024-12-03МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310789833.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-30
Publication Date
2024-12-03
Estimated Expiration
2043-06-30

AI Technical Summary

Technical Problem

Existing electric furnace smelting methods face low dephosphorization efficiency and long smelting cycles, particularly due to poor kinetic conditions in the molten steel pool without bottom-blowing systems, leading to increased production costs and reduced efficiency.

Method used

A two-stage electric furnace smelting method with controlled slag retention and removal, utilizing specific slag compositions and oxygen and power supply intensities to enhance thermodynamic and kinetic conditions, including the use of CaO as the main active component for dephosphorization, while controlling the basicity and oxidizability, while controlling the basicity and oxidizability, while ensuring the thermodynamic and kinetic conditions for dephosphorization, while ensuring the thermodynamic and kinetic conditions for dephosphorization, and the second stage: the technical solution is the use of CaO as the main active component for dephosphorization, and the second stage: the technical solution is the use of MgO and Al2O3, the melting point of the slag is lowered and the slag-forming performance is improved by adding MgO and Al2O3, the melting point of the slag is lowered and the slag is fully melted and reacted under the stirring of oxygen.

Benefits of technology

The method significantly enhances dephosphorization efficiency in the early and middle stages, shortening the smelting cycle to 36 minutes with a final P content below 0.005%, reducing lime consumption, and improving production efficiency and environmental sustainability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004313289780000051
    Figure BDA0004313289780000051
Patent Text Reader

Abstract

The invention discloses an electric furnace smelting method with high efficiency dephosphorization, and belongs to the field of electric furnace steelmaking. The electric furnace smelting method with high efficiency dephosphorization of the invention designs a reasonable slag retention and deslagging process according to the loading system, stabilizes the slag retention conditions of each furnace, formulates a reasonable deslagging process, improves the matching between the power supply, oxygen supply, and slag making system during the electric furnace blowing process, establishes good dephosphorization thermodynamic and kinetic conditions, strengthens the dephosphorization reaction in the early and middle stages, shortens the smelting cycle to within 36 minutes under the premise of ensuring that the final P content does not exceed 0.005%, reduces lime consumption and metallurgical slag emissions, and saves energy and reduces emissions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electric furnace steelmaking, and more specifically, relates to an electric furnace smelting method with high efficiency dephosphorization. Background Art

[0002] Compared with converters, electric furnace steelmaking has a higher control ability over the terminal temperature, carbon and phosphorus of molten steel, but the current proportion of electric furnace steelmaking in the country is not high. The main reasons are the cost of scrap steel and the long smelting cycle of electric furnaces. Among them, the long smelting cycle has the greatest impact on the subsequent efficient continuous casting, which greatly restricts the number of continuous casting furnaces and the casting speed, reduces production efficiency and increases production costs. In order to shorten the smelting cycle of electric furnaces, the metallurgical industry has developed and applied electric furnace smelting technologies such as ultra-high power power supply, strong oxygen supply, scrap steel preheating and smelting with molten iron to increase chemical heat and physical heat, which can effectively shorten the smelting cycle of electric furnaces. At present, a cycle of 40 minutes can basically be achieved. However, as the smelting cycle is further shortened, the bottleneck problem encountered is the rapid dephosphorization during the smelting process.

[0003] In the prior art, the bottom-blowing electric furnace is used. Through process control, the bottom-blowing gas strengthens the stirring of the molten pool, which can effectively achieve rapid dephosphorization, which is beneficial to dephosphorization and shortening the smelting cycle. However, the maintenance of the bottom-blowing components of the electric furnace is much more difficult than that of the converter, because there is no slag splashing to protect the furnace. The life of the bottom-blowing electric furnace is much shorter than that of the converter, and it has many unfavorable factors such as cost and safety. Therefore, the dephosphorization method without the bottom-blowing system is more widely used.

[0004] Most domestic electric furnaces do not have bottom blowing systems, and the dephosphorization process requires good kinetic conditions. Therefore, in order to avoid the problem of extended electric furnace cycle caused by enhanced dephosphorization, it is necessary to ensure good dephosphorization thermodynamic and kinetic conditions when there is a certain decarburization reaction rate in the furnace, that is, to strengthen the dephosphorization in the early and middle stages of the electric furnace. At present, for this problem, for electric furnaces, the main method to achieve efficient dephosphorization in the early and middle stages is the slag retention and slag discharge method, which ensures a relatively large amount of slag and appropriate slag basicity and oxidizability. However, if the slag discharge process is not properly controlled, it is easy to produce lime consumption, high steel consumption and low dephosphorization effect, which has a great impact on production efficiency and cost.

[0005] At present, for the dephosphorization problem in the electric furnace smelting process, the existing technologies such as a dephosphorization method for electric furnace steelmaking (CN102251072 A) and a method for dephosphorization by slag removal in an electric furnace (CN101619377A) are mainly used to solve the dephosphorization problem, such as slag retention and slag removal operations, which mainly provide good thermodynamic conditions for dephosphorization, but will result in high lime consumption, extended smelting cycle or no obvious improvement.

[0006] A method for dephosphorization by spraying lime powder in an electric furnace (CN 112301184 A), "Research and application of carbon retention control technology in 60t electric furnace", "Composition control analysis of spring steel produced by EAF", "Carbon retention operation technology for hot-charged hot metal smelting in electric furnace", "70t electric furnace production 82B process practice". Although the slag blowing process can dephosphorize, from a kinetic point of view, under the condition of an electric furnace without bottom blowing, only the slag blowing operation is used, and the molten steel in the middle and lower parts of the electric furnace molten pool basically does not undergo decarburization reaction. The dephosphorization kinetic conditions of the molten steel in the middle and lower parts of the electric furnace molten pool are poor. This operation will increase the electric furnace smelting cycle and reduce production efficiency.

[0007] Therefore, the dephosphorization in the electric furnace smelting process of the prior art still has the problem of low dephosphorization efficiency and long smelting cycle. Summary of the invention

[0008] 1. Problem to be solved

[0009] In view of the problem that the existing electric furnace smelting has low dephosphorization efficiency and leads to a long smelting cycle, the present invention provides an electric furnace smelting method with high efficiency dephosphorization. The electric furnace smelting method of the present invention can enhance the dephosphorization rate in the early and middle stages of the electric furnace, and shorten the smelting cycle to within 36 minutes while ensuring that the final P content does not exceed 0.005%.

[0010] 2. Technical solution

[0011] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0012] The technical problem to be solved by the present invention is to remove phosphorus from molten iron. By controlling the matching of the three, phosphorus can be removed stably and efficiently, and the content of key phosphorus can be reduced. The composition of molten iron meets the following requirements: C content is 3.90% to 4.80%, Si content is 0.1% to 0.9%, P content does not exceed 0.150%, iron-to-water ratio is 45% to 60%, and molten iron temperature is 1250 to 1400°C.

[0013] The present invention provides an electric furnace smelting method for efficient dephosphorization, which specifically comprises the following steps:

[0014] Step S1, slag retention: the ratio of molten iron charged into the electric furnace accounts for 40-60% of the total charging mass, and the amount of slag retained in the electric furnace is 65-85 kg per ton of steel.

[0015] Step S2, slag making and smelting: according to the composition of molten iron, scrap steel and slag left in the furnace, the first batch of materials added into the furnace are: 13-18 kg of lime per ton of steel, 1.8-2.4 kg of magnesium balls per ton of steel, and 1.2-1.7 kg of bauxite per ton of steel;

[0016] The oxygen supply intensity from the start of smelting to slag discharge is: 1.0~1.3m 3 / (min·t);

[0017] From the beginning of smelting to slag discharge, the power supply intensity after arcing is: 740~810kVA / t.

[0018] Step S3, slag removal: when the temperature of the molten steel rises to 1480°C, the slag removal operation begins, the slag removal amount is 55-65 kg per ton of steel, and the slag removal end temperature is not higher than 1500°C.

[0019] The slag composition requirements during slag discharge are: basicity (CaO / SiO2) 2.4-2.9, MgO 4%-5%, Al2O3 3.5%-4.5%, TFe 23%-29%.

[0020] Step S4, secondary slag making: After the slag is discharged, the second batch of slag making materials is added, with 15-22 kg of lime per ton of steel and 3.2-3.8 kg of magnesium balls per ton of steel. No bauxite is needed in this step, as the temperature has risen in the later stage and the slag can be fully melted, so there is no need to add bauxite to promote slag melting.

[0021] Step S5, slag discharge: oxygen supply intensity after slag discharge is: 1.1-1.2m 3 / (min·t), power supply intensity is: 770~835kVA / t. Among them, oxygen supply intensity and power supply intensity are greater than those in step S2. The function of this step is to quickly decarburize and heat up, in order to quickly reach the terminal temperature and carbon content requirements and shorten the smelting cycle.

[0022] Step S6, steel tapping: The steel tapping adopts the operation of leaving slag and steel, and the specific amount of steel left is based on the molten steel level during stable blowing.

[0023] The mass ratio of effective CaO in lime is not less than 85%, the mass ratio of MgO in magnesium balls is not less than 70%, and the mass ratio of bauxite Al2O3 is not less than 80%.

[0024] The present invention constructs a two-stage matching, the first stage: from the beginning of smelting to slag discharge, the matching of oxygen supply intensity, power supply intensity after arcing and slag production; the second stage: the matching of oxygen supply intensity, power supply intensity and slag production from secondary slag production to slag discharge.

[0025] Consider both thermodynamics and kinetics. In terms of thermodynamics, by adding slag-forming materials and utilizing CaO as the main active component for dephosphorization, while controlling the basicity and TFe of the components of the slag, efficient dephosphorization can be achieved during smelting. In terms of kinetics, by adding MgO and Al2O3, the melting point of the slag is lowered and the slag-forming performance is improved. Through appropriate oxygen supply intensity, the slag can be quickly and fully melted and reacted under the stirring of oxygen.

[0026] Among them, if the power supply intensity is too high, the phosphorus removal rate will decrease, if it is too low, the slag cannot be melted, and the slag-making materials cannot be melted to remove the phosphorus in the molten iron; if the oxygen supply intensity is too high, although the temperature rises quickly, the slag has poor oxidizability, if it is too low, the temperature is low, the slag oxidizability is too high, and dephosphorization is not utilized. The present invention establishes good thermodynamic and kinetic conditions for dephosphorization by matching the slag-making reaction, temperature system and oxygen supply system.

[0027] The present invention provides an electric furnace smelting method with high efficiency in dephosphorization, designs a reasonable loading system, adopts a slag-retaining and slag-removing process, stabilizes the slag-retaining conditions of each furnace, improves the matching between the power supply, oxygen supply, and slag-making systems during the electric furnace blowing process, establishes good thermodynamic and kinetic conditions for dephosphorization, strengthens the dephosphorization reaction in the early and middle stages, formulates a reasonable slag-removing process, determines the appropriate slag-removing time and slag-removing amount, etc., reduces the phosphorus content in the slag, avoids phosphorus reversion during the smelting process, and improves the effect of slag-retaining and dephosphorization in the early and middle stages of the next furnace. In order to further shorten the electric furnace smelting cycle, match the continuous casting casting speed, and improve the production capacity of the continuous casting process in the electric furnace-continuous casting steelmaking process, this solution adopts a slag-retaining and slag-removing process.

[0028] The electric furnace smelting method of the present invention can significantly improve the dephosphorization rate of the electric furnace in the early and middle stages. Under the premise of ensuring that the final P content does not exceed 0.005%, the smelting cycle is shortened to about 35 minutes, and the lime consumption per ton of steel is less than 36 kg, which can further release the production capacity of the continuous casting process, effectively reduce the consumption of steel materials and the cost per ton of steel, and at the same time reduce the emission of solid waste such as metallurgical slag, which is green and environmentally friendly and meets the national development requirements of energy conservation and emission reduction.

[0029] 3. Beneficial effects

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The present invention provides an electric furnace smelting method with high efficiency in dephosphorization. According to the charging system, a reasonable slag retention and deslagging process is designed, the slag retention conditions of each furnace are stabilized, and a reasonable deslagging process is formulated. During the electric furnace blowing process, the matching between the power supply, oxygen supply, and slag making system is improved, good dephosphorization thermodynamic and kinetic conditions are established, the dephosphorization reaction in the early and middle stages is strengthened, and the electric furnace smelting cycle is shortened under the condition of ensuring the final P content;

[0032] (2) This scheme adopts the slag retention and slag removal process, which establishes good thermodynamic and kinetic conditions for dephosphorization. The lime consumption per ton of steel is less than 36 kg, which can further release the production capacity of the continuous casting process, effectively reduce the steel material consumption and the cost per ton of steel, and at the same time reduce the emission of solid waste such as metallurgical slag. It is green and environmentally friendly, and has well coordinated the solutions to the problems of dephosphorization, cycle, cost, etc. in electric furnace smelting. DETAILED DESCRIPTION

[0033] The following is an example of an exemplary embodiment of the present invention. Although these exemplary embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention, it should be understood that other embodiments can be implemented and various changes can be made to the present invention without departing from the spirit and scope of the present invention. The more detailed description of the embodiments of the present invention below is not intended to limit the scope of the present invention as required, but is merely for illustration and does not limit the description of the characteristics and features of the present invention, so as to propose the best mode for performing the present invention, and is sufficient to enable those skilled in the art to implement the present invention. Therefore, the scope of the present invention is limited only by the appended claims.

[0034] The present invention is further described by taking a 120-ton electric furnace in a certain factory to produce 42CrMo as an example. During the production process, 8 furnace tests were carried out respectively, of which the first 6 furnaces were examples and the last 2 furnaces were comparative examples. The main process control process of the example is: the ratio of molten iron into the electric furnace accounts for 40-60% of the total charging mass, and the electric furnace adopts slag retention and slag removal operation.

[0035] Step S1, slag retention: the amount of slag retention is about 65-85 kg per ton of steel.

[0036] Step S2, slag making and smelting: the first batch of materials added into the furnace is: 13-18 kg of lime per ton of steel, 1.8-2.4 kg of magnesium balls per ton of steel, and 1.2-1.7 kg of bauxite per ton of steel; wherein the mass ratio of effective CaO in the lime is not less than 85%, the mass ratio of MgO in the magnesium balls is not less than 70%, and the mass ratio of bauxite Al2O3 is not less than 80%;

[0037] The oxygen supply intensity from the start of smelting to slag discharge is: 1.0~1.3m 3 / (min·t); from the beginning of smelting to slag discharge, the power supply intensity after arcing is: 740~810kVA / t.

[0038] Step S3, slag discharge: when the temperature of the molten steel rises to 1480°C, the slag discharge operation begins, the slag discharge amount is 55-65 kg per ton of steel, the slag discharge end temperature is not higher than 1500°C, and the slag composition requirements during slag discharge are: basicity of 2.4-2.9, MgO of 4%-5%, Al2O3 of 3.5%-4.5%, and TFe of 23%-29%.

[0039] Step S4, secondary slag making: after the slag discharge is completed, the second batch of slag making materials is added, 15-22 kg of lime per ton of steel, and 3.2-3.8 kg of magnesium balls per ton of steel.

[0040] Step S5, slag discharge: oxygen supply intensity after slag discharge is: 1.1-1.2m 3 / (min·t), power supply intensity is: 770~835kVA / t.

[0041] Step S6, steel tapping: The steel tapping adopts the operation of leaving slag and steel, and the specific amount of steel left is based on the stable blowing molten steel level.

[0042] The main process and endpoint control conditions are shown in the following table, wherein Table 1 is the composition parameters in molten iron; Table 2 is the process parameters of the electric furnace smelting process; Table 3 is the specific conditions of the electric furnace carbon retention and dephosphorization embodiment and the comparative example process.

[0043] Table 1 Parameters of hot metal entering the furnace

[0044] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Temperature / ℃ 1265 1381 1314 1367 1344 1292 1342 1339 C / wt% 4.24 3.98 4.15 4.68 4.36 4.51 4.45 4.39 Si / wt% 0.81 0.60 0.42 0.15 0.32 0.27 0.35 0.61 P / wt% 0.115 0.140 0.123 0.113 0.130 0.104 0.119 0.134 Hot metal ratio / % 45% 48% 49% 54% 55% 57% 48% 54%

[0045] Table 2 Process parameters of electric furnace smelting process

[0046]

[0047] Table 3 Electric furnace carbon removal and dephosphorization embodiment and comparative example process smelting specific conditions

[0048] Lime consumption per ton of steel / kg Steel material consumption / kg Smelting cycle / min End point P / % Residue amount / ton Example 1 29 1077 36 0.004 8.3 Example 2 34 1076 35 0.005 10.1 Example 3 36 1075 34 0.004 9.7 Example 4 30 1077 36 0.005 8.5 Example 5 33 1078 35 0.005 9.0 Example 6 36 1076 35 0.005 9.4 Comparative Example 1 42 1081 41 0.006 2.4 Comparative Example 2 40 1080 42 0.006 5.8

[0049] It can be seen from the results of the embodiment that the method can significantly improve the dephosphorization rate of the electric furnace in the early and middle stages, shorten the smelting cycle to within 36 minutes while ensuring that the final P content does not exceed 0.005%, and the lime consumption per ton of steel is less than 36 kg, which can further release the production capacity of the continuous casting process, effectively reduce the consumption of steel materials and the cost per ton of steel, and at the same time reduce the emission of solid waste such as metallurgical slag, which is green and environmentally friendly and meets the national development requirements of energy conservation and emission reduction.

Claims

1. An electric furnace smelting method for efficient dephosphorization, characterized in that: The following steps are involved: Step S1, slag retention, the amount of slag retained in the electric furnace is 65-85 kg per ton of steel; Step S2, slag making and smelting: molten iron is put into the furnace, and primary slag making materials are added, including 13-18 kg of lime per ton of steel, 1.8-2.4 kg of magnesium balls per ton of steel, and 1.2-1.7 kg of bauxite per ton of steel; The oxygen supply intensity from the start of smelting to slag discharge is 1.0~1.3m 3 / (min·t); after arcing, the power supply intensity is: 740~810kVA / t; Step S3, slag removal; in step S3, the starting temperature of the slag removal operation is 1480°C, and the ending temperature of the slag removal is not higher than 1500°C; The slag composition requirements during slag discharge in step S3 are as follows: basicity of 2.4-2.9, MgO of 4%-5%, Al2O3 of 3.5%-4.5%, and TFe of 23%-29%; Step S4, secondary slag making: after the slag discharge is completed, secondary slag making materials are added, including 15-22 kg of lime per ton of steel and 3.2-3.8 kg of magnesium balls per ton of steel; Step S5, slag discharge: oxygen supply intensity after slag discharge is: 1.1-1.2m 3 / (min·t), power supply intensity: 770~835kVA / t; Step S6, steel tapping: the steel tapping adopts the operation of leaving slag and steel.

2. The electric furnace smelting method for efficient dephosphorization according to claim 1, characterized in that: The proportion of molten iron charged into the electric furnace accounts for 40-60% of the total charging mass.

3. The electric furnace smelting method for efficient dephosphorization according to claim 2, characterized in that: In step S2, the molten iron meets the following conditions: C content is 3.90% to 4.80%, Si content is 0.1% to 0.9%, P content does not exceed 0.150%, and the iron-to-metal ratio is 45% to 60%.

4. The electric furnace smelting method for efficient dephosphorization according to claim 3 is characterized in that: The temperature of molten iron entering the furnace is 1250~1400℃.

5. The electric furnace smelting method for efficient dephosphorization according to claim 4 is characterized in that: The slag discharge amount in step S3 is 55-65 kg per ton of steel.

6. The electric furnace smelting method for efficient dephosphorization according to claim 5, characterized in that: The mass ratio of effective CaO in lime shall not be less than 85%; the mass ratio of MgO in magnesium balls shall not be less than 70%; the mass ratio of bauxite Al2O3 shall not be less than 80%.

Citation Information

Cited By

  • Phosphorus-enriching agent based on multiphase solvent dephosphorization theory, preparation method of phosphorus-enriching agent and application of phosphorus-enriching agent in dephosphorization of iron and molten steel

    CN122235414A