A sintering process method for increasing the strength of indium tin oxide target

By using a sintering base of silicon carbide beams and alumina gaskets in the ITO target sintering process, combined with gradient heating and cooling technology, the problems of easy cracking and low tensile strength of ITO targets are solved, and the tensile strength and Production efficiency and reduced costs.

CN116854485BActive Publication Date: 2024-10-11WUHU YINGRI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310510156.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-10-11
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

The ITO target material with a ratio of 97% indium oxide + 3% tin oxide is easy to crack, has low tensile strength, and is difficult to sinter, which affects the quality of glass substrate coating sputtering.

Method used

It uses a sintered base with silicon carbide beams and alumina gaskets, gradient heating and cooling, and the cooling rate is controlled at 0.4-0.6°C/min. It combines powder ball milling, spray granulation and pressure forming processes to improve the uniform heating and internalization of the target. Stress relief.

Benefits of technology

The tensile strength of the indium tin oxide target material is significantly increased to 166.89Mpa, the occurrence rate of internal cracks is reduced, and the production yield and cost-effectiveness are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116854485B_ABST
    Figure CN116854485B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of target material technology, and in particular to a sintering process for increasing the strength of an indium tin oxide target material, wherein a silicon carbide beam + an alumina gasket is used instead of a traditional alumina support plate + an alumina gasket, and gradient heating is used for sintering, and then the sintering cooling rate is 0.4-0.6°C / min, and the furnace bed is lowered after the temperature in the furnace is less than 10°C. The indium tin oxide target material prepared by the sintering process of the present invention has a tensile strength of up to 166.89Mpa, no internal abnormalities, and a production yield of more than 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of target materials, and in particular to a sintering process method for increasing the strength of an indium tin oxide target material. Background Art

[0002] ITO (Tin-doped Indium Oxide) target material is an indium tin composite oxide ceramic and an important optoelectronic functional material. It is often used as a magnetron sputtering target to prepare transparent conductive films on glass, plastic and other substrate materials. It is used in the production of flat-panel display devices such as liquid crystal displays and touch screens.

[0003] The compressive (bending) strength standard of ITO targets is ≥140Mpa (universal testing machine), and the strength of ITO targets with different ratios of indium oxide and tin oxide is different. Generally speaking, the ITO target with a ratio of 90% indium oxide + 10% tin oxide is stronger than the ITO target with a ratio of 93% indium oxide + 7% tin oxide. The ITO target with a ratio of 93% indium oxide + 7% tin oxide is even stronger than the ITO target with a ratio of 97% indium oxide + 3% tin oxide. (That is, the higher the indium oxide content + the lower the tin oxide content, the lower the strength of the target). However, the ITO target with a ratio of 97% indium oxide + 3% tin oxide is easy to crack, has low tensile strength, and is difficult to sinter. In addition, the ITO target with low tensile strength is prone to cracking and falling off during terminal use in downstream industries, which affects the sputtering of glass substrate coating. Summary of the invention

[0004] In view of this, the purpose of the present invention is to propose a sintering process method for increasing the strength of an indium tin oxide target material, so as to solve the problems of easy cracking, low tensile strength and high sintering difficulty of an ITO target material with a ratio of 97% indium oxide + 3% tin oxide.

[0005] Based on the above purpose, the present invention provides a sintering process method for increasing the strength of an indium tin oxide target. The specific steps of the sintering process method are as follows: fixing an indium tin oxide blank on a base in a high-temperature sintering furnace in a normal pressure oxygen atmosphere for sintering, the base being a silicon carbide beam and an alumina gasket, the silicon carbide beams being cross-placed on a furnace bed support, the distance between each beam being 20-30 mm, and an alumina gasket being placed on the silicon carbide beam, using a gradient heating method, and maintaining the temperature after reaching the sintering temperature, cooling after the sintering is completed, the cooling rate being 0.4-0.6°C / min, and when the temperature in the furnace is less than 10°C, the furnace bed is lowered, and the indium tin oxide target is taken out.

[0006] Preferably, the indium tin oxide target has a target tensile strength of 165.32-166.89 MPa.

[0007] Preferably, the weight ratio of indium oxide powder to tin oxide powder in the indium tin oxide element is 97:3.

[0008] Preferably, the purity of the silicon carbide crossbeam is ≥98%, the temperature resistance is ≥1700 degrees, and the compressive strength is 500-700Mpa; the purity of the alumina gasket is ≥98.7, and the modulus of rupture is ≥35Mpa.

[0009] Preferably, the gradient temperature increase is: 200-700°C, the heating rate is 0.08-0.13°C / min, 700-1580°C, the heating rate is 0.25-0.35°C / min.

[0010] Furthermore, the present invention provides a method for preparing an indium tin oxide target, wherein the method for preparing the indium tin oxide target adopts the sintering process for increasing the strength of the indium tin oxide target according to any one of claims 1 to 3, and the specific preparation method is as follows:

[0011] (1) Powder ball milling: Add indium oxide powder and tin oxide powder in a weight ratio of 97:3 into a ball mill filled with φ1-2 mm zirconium beads, then add pure water, and then ball mill for 24-48 hours to obtain ITO slurry;

[0012] (2) Spray granulation: The ITO slurry is dried and granulated using a centrifugal spray granulator to obtain ITO powder;

[0013] (3) Pressure molding: ITO powder is placed in a mold for molding to obtain an indium tin oxide embryo;

[0014] (4) High temperature sintering: The indium tin oxide target is obtained by using the sintering process method for increasing the strength of the indium tin oxide target.

[0015] Preferably, the purity of the indium oxide powder and the tin oxide powder in step (1) is ≥ 99.5%.

[0016] Preferably, in step (1), the weight of pure water, indium oxide powder and tin oxide powder is equal.

[0017] Preferably, in step (2), the air inlet temperature of the centrifugal spray granulator is 200-230°C, and the air outlet temperature is 80-110°C.

[0018] Preferably, in step (3), the molding size is: length 500-1800mm*width 200-500mm, molding pressure is: 280-350Mpa, and molding time is: 1-3h

[0019] Beneficial effects of the present invention:

[0020] The present invention uses a silicon carbide crossbeam + an alumina gasket in the sintering process instead of a traditional alumina support plate + an alumina gasket, so that the inner diameter and the outer diameter of the target material can be heated evenly, reducing the occurrence of cracks inside the target material.

[0021] The present invention adopts a gradient heating method for sintering. The target material uses different heating rates at different temperature stages, which can more effectively achieve the effects of uniform heating, crystallization, and uniform shrinkage, and further reduce the occurrence of internal cracks.

[0022] The present invention adopts a cooling rate of 0.4-0.6°C / min and a method of completely cooling and then lowering the furnace bed to replace the traditional cooling rate of 0.75-0.9°C / min and the method of starting to lower the furnace bed when the temperature in the furnace is less than 200 degrees. The stress in the target material is released more thoroughly, and the tensile strength of the target material is improved.

[0023] The tensile strength of the target material prepared by the present invention is as high as 166.89 Mpa, there is no abnormality inside the target material, and the production yield is as high as more than 90%, thereby reducing the cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 This is a schematic diagram of a silicon carbide beam and an alumina gasket in Example 1 of the present invention;

[0026] Figure 2 Schematic diagram of an alumina support plate and an alumina gasket in Comparative Example 1 of the present invention;

[0027] Figure 3 Ultrasonic flaw detection images of the indium tin oxide target material in comparative example 1 of the present invention (left) and the indium tin oxide target material in comparative example 3 (right);

[0028] Figure 4 This is an ultrasonic flaw detection image of the indium tin oxide target in Example 2 of the present invention. DETAILED DESCRIPTION

[0029] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0030] In the embodiment of the present invention, in the comparative example, the purity of indium oxide powder is 99.8%, the purity of tin oxide powder is 99.7%, the purity of silicon carbide beam is 98.5%, the temperature resistance is 1700 degrees, the compressive strength is 500Mpa, the purity of the aluminum oxide gasket is 98.7, and the modulus of rupture is 35.5Mpa.

[0031] Example 1

[0032] (1) Powder ball milling: Add 97 g of indium oxide powder and 3 g of tin oxide powder to a ball mill filled with φ1 mm zirconium beads, then add 100 g of pure water, and then ball mill for 36 h to obtain ITO slurry;

[0033] (2) Spray granulation: The ITO slurry is dried and granulated using a centrifugal spray granulator with an inlet air temperature of 210°C and an outlet air temperature of 90°C to obtain ITO powder;

[0034] (3) Pressure molding: ITO powder is placed in a mold for molding, molding size: length 1000 mm * width 400 mm, molding pressure: 320 MPa, molding time: 1 h, to obtain an indium tin oxide embryo;

[0035] (4) High temperature sintering: The indium tin oxide blank is fixed on a base in a high temperature sintering furnace in a normal pressure oxygen atmosphere for sintering. The base is a silicon carbide beam and an alumina gasket, such as Figure 1 As shown, the silicon carbide beams are placed crosswise on the furnace bed pillars, with a distance of 20 mm between each beam. Alumina gaskets are placed on the silicon carbide beams, and a gradient temperature is used, 200-700°C, the heating rate is 0.08°C / min, 700-1580°C, the heating rate is 0.25°C / min, after reaching the sintering temperature, the temperature is kept, and after sintering, the temperature is lowered, the cooling rate is 0.4°C / min, and when the temperature in the furnace is 9°C, the furnace bed is lowered to obtain an indium tin oxide target.

[0036] Example 2

[0037] (1) Powder ball milling: same as in Example 1;

[0038] (2) Spray granulation: same as in Example 1;

[0039] (3) Pressure forming: same as in Example 1;

[0040] (4) High-temperature sintering: The indium tin oxide blank is fixed on a base in a high-temperature sintering furnace in a normal pressure oxygen atmosphere for sintering. The base is a silicon carbide beam and an alumina gasket. The silicon carbide beams are placed crosswise on the furnace bed pillars. The distance between each beam is 25 mm. Alumina gaskets are placed on the silicon carbide beams. The temperature is increased by a gradient from 200 to 700°C at a heating rate of 0.1°C / min and from 700 to 1580°C at a heating rate of 0.3°C / min. After reaching the sintering temperature, the temperature is kept constant. After sintering, the temperature is lowered at a cooling rate of 0.5°C / min. When the temperature in the furnace reaches 9°C, the furnace bed is lowered to obtain the indium tin oxide target.

[0041] Example 3

[0042] (1) Powder ball milling: same as in Example 1;

[0043] (2) Spray granulation: same as in Example 1;

[0044] (3) Pressure forming: same as in Example 1;

[0045] (4) High-temperature sintering: The indium tin oxide blank is fixed on a base in a high-temperature sintering furnace in a normal pressure oxygen atmosphere for sintering. The base is a silicon carbide beam and an alumina gasket. The silicon carbide beams are placed crosswise on the furnace bed pillars. The distance between each beam is 30 mm. Alumina gaskets are placed on the silicon carbide beams. The temperature is increased by a gradient from 200 to 700°C at a heating rate of 0.13°C / min and from 700 to 1580°C at a heating rate of 0.35°C / min. After reaching the sintering temperature, the temperature is maintained. After sintering, the temperature is lowered at a cooling rate of 0.6°C / min. When the temperature in the furnace reaches 9°C, the furnace bed is lowered to obtain the indium tin oxide target.

[0046] Comparative Example 1

[0047] (1) Powder ball milling: same as in Example 1;

[0048] (2) Spray granulation: same as in Example 1;

[0049] (3) Pressure forming: same as in Example 1;

[0050] (4) High temperature sintering: The indium tin oxide blank is fixed on a base in a high temperature sintering furnace in a normal pressure oxygen atmosphere for sintering. The base is an alumina support plate and an alumina gasket, such as Figure 2 As shown, a gradient temperature increase is adopted, 200-700°C, the heating rate is 0.1°C / min, 700-1580°C, the heating rate is 0.3°C / min, after reaching the sintering temperature, the temperature is kept, and after the sintering is completed, the temperature is lowered, the cooling rate is 0.5°C / min, and when the temperature in the furnace is 9°C, the furnace bed is lowered to obtain an indium tin oxide target.

[0051] Comparative Example 2

[0052] (1) Powder ball milling: same as in Example 1;

[0053] (2) Spray granulation: same as in Example 1;

[0054] (3) Pressure forming: same as in Example 1;

[0055] (4) High-temperature sintering: The indium tin oxide blank is fixed on a base in a high-temperature sintering furnace in a normal pressure oxygen atmosphere for sintering. The base is a silicon carbide beam and an alumina gasket. The silicon carbide beams are placed crosswise on the furnace bed pillars. The distance between each beam is 25 mm. Alumina gaskets are placed on the silicon carbide beams. The temperature is increased by a gradient from 200 to 700°C at a heating rate of 0.1°C / min and from 700 to 1580°C at a heating rate of 0.3°C / min. After reaching the sintering temperature, the temperature is maintained. After sintering, the temperature is lowered at a cooling rate of 0.8°C / min. When the temperature in the furnace reaches 195°C, the furnace bed is lowered to obtain the indium tin oxide target.

[0056] Comparative Example 3

[0057] (1) Powder ball milling: same as in Example 1;

[0058] (2) Spray granulation: same as in Example 1;

[0059] (3) Pressure forming: same as in Example 1;

[0060] (4) High-temperature sintering: The indium tin oxide blank is fixed on a base in a high-temperature sintering furnace in a normal pressure oxygen atmosphere for sintering. The base is an alumina support plate and an alumina gasket. The temperature is increased in a gradient manner from 200 to 700°C at a heating rate of 0.1°C / min and from 700 to 1580°C at a heating rate of 0.3°C / min. After reaching the sintering temperature, the temperature is maintained. After sintering, the temperature is lowered at a cooling rate of 0.8°C / min. When the temperature in the furnace reaches 195°C, the furnace bed is lowered to obtain an indium tin oxide target.

[0061] Performance Testing

[0062] Internal cracks of the target material: Ultrasonic detection was used to detect Examples 1-3 and Comparative Examples 1-3 to observe whether there were cracks inside.

[0063] Tensile strength: According to the national standard GB / T 23611-2009, a target sample with the size of (length 30*width 10*thickness 8.8mm) was taken for mechanical strength test (as shown below); the name of the test equipment: compressive strength testing machine. The mechanical strength test parameters are: descending speed 0.34mm / s, span 30mm.

[0064]

[0065] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0066] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A sintering process for increasing the strength of an indium tin oxide target, characterized in that: The specific steps of the sintering process are as follows: fixing an indium tin oxide blank on a base in a high-temperature sintering furnace in an atmospheric oxygen atmosphere for sintering, the base being a silicon carbide beam and an alumina gasket, the silicon carbide beam being cross-placed on a furnace bed support, the distance between each beam being 20-30 mm, placing an alumina gasket on the silicon carbide beam, adopting a gradient heating method, maintaining the temperature after reaching the sintering temperature, cooling after the sintering is completed, the cooling rate being 0.4-0.6°C / min, and when the temperature in the furnace is less than 10°C, lowering the furnace bed and taking out the indium tin oxide target; The target tensile strength of the indium tin oxide target is 165.32-166.89Mpa; The weight ratio of indium oxide powder to tin oxide powder in the indium tin oxide element is 97:3; The gradient temperature increase is: 200-700°C, the temperature increase rate is 0.08-0.13°C / min, 700-1580°C, the temperature increase rate is 0.25-0.35°C / min.

2. The sintering process for increasing the strength of an indium tin oxide target according to claim 1, characterized in that: The purity of the silicon carbide crossbeam is ≥98%, the temperature resistance is ≥1700 degrees, and the compressive strength is 500-700Mpa. The purity of the alumina gasket is ≥98.7, and the modulus of rupture is ≥35Mpa.

3. A method for preparing an indium tin oxide target, characterized in that: The preparation method of the indium tin oxide target material adopts the sintering process method for increasing the strength of the indium tin oxide target material according to any one of claims 1-2, and the specific preparation method is as follows: (1) Powder ball milling: Add indium oxide powder and tin oxide powder in a weight ratio of 97:3 into a ball mill filled with φ1-2 mm zirconium beads, then add pure water, and then ball mill for 24-48 hours to obtain ITO slurry; (2) Spray granulation: The ITO slurry is dried and granulated using a centrifugal spray granulator to obtain ITO powder; (3) Pressure molding: ITO powder is placed in a mold for molding to obtain an indium tin oxide embryo; (4) High temperature sintering: The indium tin oxide target is obtained by using the sintering process method for increasing the strength of the indium tin oxide target.

4. The sintering process for increasing the strength of an indium tin oxide target according to claim 3, characterized in that: The purity of the indium oxide powder and the tin oxide powder in step (1) is ≥ 99.5%.

5. The sintering process for increasing the strength of an indium tin oxide target according to claim 3, characterized in that: In the step (1), the weight of pure water, indium oxide powder and tin oxide powder is equal.

6. The sintering process for increasing the strength of an indium tin oxide target according to claim 3, characterized in that: In the step (2), the air inlet temperature of the centrifugal spray granulator is 200-230°C, and the air outlet temperature is 80-110°C.

7. The sintering process for increasing the strength of an indium tin oxide target according to claim 3, characterized in that: The molding size in the step (3) is: length 500-1800mm*width 200-500mm, molding pressure: 280-350Mpa, and molding time: 1-3h.

Citation Information

Cited By

  • Pad burning mode for greatly reducing deformation of sintered bottom of ITO rotating target material

    CN120483678A