A yeast-derived metal phosphide electrode material and its preparation method and application
The preparation of yeast-derived nickel cobalt phosphide in yeast cell fluid through bioadsorption and hydrothermal carbonization methods, solving the high energy consumption and complex equipment problems of traditional bimetallic phosphide preparation methods, and achieving high performance and low cost production of materials.
Patent Information
- Application Number
- CN202310543207.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-05-15
AI Technical Summary
The traditional preparation method of bimetallic phosphide requires high reaction temperature and exogenous reduction gas, resulting in high production costs, complex equipment and high energy consumption. The differences in different elements in bimetallic phosphides make it difficult for compounds to react simultaneously.
Using bioadsorption and hydrothermal carbonization methods, using yeast as a biological template, cobalt acetate tetrahydrate and nickel nitrate hexahydrate were adsorbed and hydrothermal reactions in yeast cell liquid, and yeast-derived nickel cobalt phosphide was prepared by nitrogen calcination, simplifying the process and reduce energy consumption.
It realizes simple and low-energy preparation of bimetallic phosphides, improves the mechanical properties and conductivity of the materials, reduces production costs, and provides better electrochemical properties.
Smart Images

Figure CN116873886B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmental material synthesis and the category of electrochemistry, and specifically relates to a yeast-derived metal phosphide electrode material and a preparation method and application thereof. Background Art
[0002] Electrode materials are key factors in determining the performance of batteries, capacitors, and electrosorption. In recent years, transition metal phosphides have attracted extensive attention from researchers due to their outstanding physical and chemical properties. The degree of electron delocalization in transition metal phosphides is high, the oxidation state of the metal is low, and a strong MP covalent bond can be formed. Therefore, the negative electrode material made of transition metal phosphide nanoparticles has a high reversible capacity and good cycle stability. At present, single metal phosphides are more studied among transition metal phosphides, and their properties are also more comprehensively explored. In contrast, there are few research reports on bimetallic phosphides.
[0003] In the study of traditional catalysts, bimetallic catalysts have shown outstanding catalytic performance, so people expect that bimetallic phosphides can also produce better catalytic effects due to the synergistic effect between metal elements. However, due to the essential differences between the different elements in bimetallic phosphides, it is difficult to react synchronously to form bimetallic phosphides in the formation of compounds, so the synthesis method of bimetallic phosphides has great limitations. The traditional preparation method of bimetallic phosphides is the programmed temperature reduction method, which requires a high reaction temperature and programmed temperature rise, so it consumes a lot of energy and the reaction cycle is too long; in addition, this method requires the introduction of exogenous reducing gases such as H during the reaction. 2 , resulting in problems such as high production costs and complex equipment. Summary of the invention
[0004] To solve the above problems, one of the objects of the present invention is to provide a method for preparing yeast-derived metal phosphide electrode materials, which successfully synthesizes bimetallic phosphides through biosorption and hydrothermal carbonization. The process is simple, the operation is easy, and the production cost is effectively reduced.
[0005] In order to achieve the above object, the specific technical solution adopted by the present invention is as follows:
[0006] A method for preparing a yeast-derived metal phosphide electrode material comprises first adding precursor substances, cobalt acetate tetrahydrate and nickel nitrate hexahydrate, into yeast cell fluid to obtain a Co adsorbed 2+ and Ni 2+ yeast; the obtained mixed solution is subjected to a hydrothermal reaction to obtain an intermediate product; finally, the intermediate product is calcined in a nitrogen atmosphere to obtain yeast-derived nickel cobalt phosphide.
[0007] The preparation method of the yeast-derived metal phosphide electrode material specifically comprises the following steps:
[0008] S1. Add 3-5g yeast powder to 80-100mL deionized water and incubate at 35℃ for 24-48h;
[0009] S2. The culture solution is centrifuged and the precipitate is washed with deionized water to remove possible impurities to purify the yeast cells;
[0010] S3. Dissolve the precursors cobalt acetate tetrahydrate and nickel nitrate hexahydrate in the yeast cell solution and stir to make Co 2+ and Ni 2+ Adsorbed on the surface of yeast cells;
[0011] S4. The resulting solution was centrifuged and the precipitate was washed with deionized water to remove the dissociated Co 2+ and Ni 2+ , and obtain adsorbed Co 2+ and Ni 2+ of yeast cells;
[0012] S5.Co 2+ / Ni 2+ / yeast cell mixed solution is transferred to the lining of the autoclave and subjected to hydrothermal reaction at 180-200°C for 24h. During the reaction, deionized water can be added to the reactor as needed to prevent excessive viscosity;
[0013] S6. After the reaction is completed and the temperature of the reaction solution drops to room temperature, it is centrifuged and the precipitate is washed with deionized water;
[0014] S7. The centrifuged mixture is subjected to vacuum freeze drying for 24-36 hours to obtain an N and P-doped intermediate product;
[0015] S8. The freeze-dried intermediate product is calcined at 800-900° C. for 3-5 hours under nitrogen to obtain yeast-derived nickel cobalt phosphide.
[0016] Preferably, in step S1, the yeast powder used is Saccharomycete yeast powder. This yeast is different from conventional yeast, has a higher phosphorus content, and has a more uniform shape, which is beneficial to improving the size consistency of the final synthetic product.
[0017] Preferably, in step S2, the washing times with deionized water are 3-4 times. If the washing times are less than 3 times, the washing is not thorough, resulting in a large overall difference in the sample morphology. If the washing times exceed 4 times, the metal ions adsorbed by the yeast may be desorbed, affecting the product amount. In addition, the washing water must be deionized water. If other water containing impurities is used for washing, it may cause sample contamination and affect the product phase.
[0018] Preferably, in step S3, the amount of cobalt acetate tetrahydrate is 2.5-3.0 g, and the amount of nickel nitrate hexahydrate is 2.5-3.0 g. The amount should be strictly controlled, and other precursor substances or concentrations have been proven by multiple experiments to be unable to synthesize nickel cobalt phosphide.
[0019] Preferably, in step S3, the stirring method is magnetic stirring, the stirring speed is medium-low speed 120-180r / min, and the stirring time is 24-48h to ensure that Co 2+ and Ni 2+ Fully and evenly adsorbed on the surface of yeast cells.
[0020] Preferably, in steps S2, S4 and S6, the centrifugal speed is 6000-8000 r / min.
[0021] Preferably, in step S8, during calcination, the mixture is heated from room temperature to 850°C at a heating rate of 5°C / min, and then maintained at 850°C for 4 hours.
[0022] In view of the problems of the existing bimetallic phosphide preparation methods, the present invention has developed a method combining biosorption and hydrothermal carbonization. First, yeast is selected as a biosorbent. Yeast is a kind of fungus that is ubiquitous in nature and is widely used in the fermentation industry. Unlike other fungi, yeast itself contains not only rich nitrogen but also phosphorus, which can provide a phosphorus source. In addition, yeast can be used as a biological template to transfer metal ions (Ni 2+ 、Ni 3+ 、Co 2+ ) and the functional groups of biomolecules (OH - 、COOH - ) for complex assembly; at the same time, after calcination, yeast can also generate nitrogen and phosphorus-doped biochar, which can improve its ion storage performance. Therefore, it is of great significance to use yeast as a biological template to develop a relatively simple and low-energy preparation method for bimetallic phosphides.
[0023] On the basis of the above, the present invention selects Saccharomycete yeast powder as a biological template and provides a phosphorus source, selects cobalt acetate tetrahydrate and nickel nitrate hexahydrate as precursors to provide bimetallic ions, and successfully loads nickel cobalt phosphide evenly on the yeast surface through adsorption, hydrothermal reaction, and nitrogen calcination, and synthesizes yeast-derived nickel cobalt phosphide with a spherical or ellipsoidal overall morphology. The presence of yeast-derived biochar in the yeast-derived nickel cobalt phosphide of the present invention can effectively improve mechanical properties and conductivity, increase specific surface area; and can provide a buffering effect, effectively alleviate the stress and strain of metal phosphides during ion embedding and removal, and improve the stability of the electrode; compared with conventional bimetallic phosphides, the performance is more excellent. In addition, compared with the traditional programmed temperature reduction method, the preparation method of the present invention has a simple process, is easy to operate, does not require complex equipment, has low energy consumption, greatly reduces production costs, and has significant advantages.
[0024] The second object of the present invention is to provide a yeast-derived metal phosphide electrode material obtained by the above preparation method, specifically yeast-derived nickel cobalt phosphide.
[0025] The third object of the present invention is to provide an application of the yeast-derived metal phosphide electrode material obtained by the above preparation method, which can be used as an electrode material in multiple fields such as capacitor deionization, supercapacitors, sodium ion batteries, etc., and has good economic value.
[0026] The present invention has the following beneficial effects:
[0027] 1. The phosphorus in the metal phosphide electrode material prepared by the present invention comes from yeast, and the phosphorus in the yeast itself is utilized in situ during the preparation process, without the need to add other phosphorus sources.
[0028] 2. The metal phosphide electrode material prepared by the present invention contains derived biomass carbon, which has strong conductivity, can provide a large specific surface area for ion adsorption, can effectively alleviate the stress and strain of metal phosphides during ion embedding and removal, and has strong mechanical properties, so that the performance of the yeast-derived nickel cobalt phosphide as an electrode material of the present invention is significantly better than that of conventional bimetallic phosphides.
[0029] 3. Compared with the existing programmed temperature reduction method for preparing bimetallic phosphides, the preparation method of the present invention has simple process, easy operation, no need for complex equipment, low energy consumption, greatly reduced production costs, and significant advantages.
[0030] 4. The metal phosphide electrode material of the present invention can be applied in multiple fields, and the later biological template can be expanded to waste yeast for resource utilization of solid waste, which has good development prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1: SEM image of yeast culture after freeze-drying during the preparation of yeast-derived metal phosphide electrode material in Example 1.
[0032] Figure 2 : SEM image of the yeast-derived metal phosphide electrode material in Example 1.
[0033] Figure 3 : TEM image of the yeast-derived metal phosphide electrode material in Example 1.
[0034] Figure 4 : Electrochemical CV diagram of the yeast-derived metal phosphide electrode material in Example 1. DETAILED DESCRIPTION
[0035] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0036] Example 1
[0037] A method for preparing a yeast-derived metal phosphide electrode material comprises the following steps:
[0038] S1. Take 3g of Saccharomycete yeast powder purchased from Biobowei and add it to 80mL of deionized water. Incubate it in a culture dish at 35℃ for 24h.
[0039] S2. The culture solution was centrifuged at a speed of 6000 r / min, and the precipitate was washed three times with deionized water;
[0040] S3. 2.5 g of cobalt acetate tetrahydrate and 2.5 g of nickel nitrate hexahydrate were dissolved in the yeast cell solution and magnetically stirred at a stirring speed of 120 r / min for 24 h;
[0041] S4. The resulting solution was centrifuged at 6000 r / min for 5 minutes, and the precipitate was washed with deionized water to obtain adsorbed Co 2+ and Ni 2+ of yeast cells;
[0042] S5.Co 2+ / Ni 2+ / yeast cell mixed solution was transferred into a 100 mL autoclave liner and subjected to hydrothermal reaction at 180 °C for 24 h;
[0043] S6. After the reaction is completed, the reaction solution temperature is cooled to room temperature, and the reaction solution is centrifuged at 6000 r / min for 5 minutes, and the precipitate is washed with deionized water;
[0044] S7. The centrifuged mixture was subjected to vacuum freeze drying for 24 h to obtain an N- and P-doped intermediate product;
[0045] S8. The freeze-dried intermediate product is placed in the center of a quartz tube in a tube furnace, heated from room temperature to 850°C at a heating rate of 5°C / min under a nitrogen atmosphere, and then maintained at 850°C for 4 hours to obtain yeast-derived nickel cobalt phosphide.
[0046] Example 2
[0047] A method for preparing a yeast-derived metal phosphide electrode material comprises the following steps:
[0048] S1. Take 4g of Saccharomycete yeast powder purchased from Biobowei and add it to 90mL of deionized water. Incubate it in a culture dish at 35℃ for 36h.
[0049] S2. The culture solution was centrifuged at a speed of 7000 r / min, and the precipitate was washed 4 times with deionized water;
[0050] S3. 2.8 g of cobalt acetate tetrahydrate and 3.0 g of nickel nitrate hexahydrate were dissolved in the yeast cell solution and magnetically stirred at a stirring speed of 150 r / min for 30 h;
[0051] S4. The resulting solution was centrifuged at 7000 r / min for 5 minutes, and the precipitate was washed with deionized water to obtain adsorbed Co 2+ and Ni 2+ of yeast cells;
[0052] S5.Co 2+ / Ni 2+ / yeast cell mixed solution was transferred into a 100 mL autoclave liner and subjected to hydrothermal reaction at 190 °C for 24 h;
[0053] S6. After the reaction is completed, the reaction solution temperature is cooled to room temperature, and the reaction solution is centrifuged at 6000 r / min for 5 minutes, and the precipitate is washed with deionized water;
[0054] S7. The centrifuged mixture was subjected to vacuum freeze drying for 30 h to obtain an N and P-doped intermediate product;
[0055] S8. The freeze-dried intermediate product is placed in the center of a quartz tube in a tube furnace, heated from room temperature to 850°C at a heating rate of 5°C / min under a nitrogen atmosphere, and then maintained at 850°C for 4 hours to obtain yeast-derived nickel cobalt phosphide.
[0056] Example 3
[0057] A method for preparing a yeast-derived metal phosphide electrode material comprises the following steps:
[0058] S1. Take 5g of Saccharomycete yeast powder purchased from Biobowei and add it to 100mL of deionized water. Incubate it in a culture dish at 35℃ for 48h.
[0059] S2. The culture solution was centrifuged at a speed of 8000 r / min, and the precipitate was washed 4 times with deionized water;
[0060] S3. 3.0 g of cobalt acetate tetrahydrate and 2.8 g of nickel nitrate hexahydrate were dissolved in the yeast cell solution and magnetically stirred at a stirring speed of 180 r / min for 36 h;
[0061] S4. The resulting solution was centrifuged at 8000 r / min for 5 minutes, and the precipitate was washed with deionized water to obtain adsorbed Co 2+ and Ni 2+ of yeast cells;
[0062] S5.Co 2+ / Ni 2+ / yeast cell mixed solution was transferred into a 100 mL autoclave liner and subjected to hydrothermal reaction at 200 °C for 24 h;
[0063] S6. After the reaction is completed, the reaction solution temperature is cooled to room temperature, and the reaction solution is centrifuged at 6000 r / min for 5 minutes, and the precipitate is washed with deionized water;
[0064] S7. The centrifuged mixture was subjected to vacuum freeze drying for 36 h to obtain an N and P-doped intermediate product;
[0065] S8. The freeze-dried intermediate product is placed in the center of a quartz tube in a tube furnace, heated from room temperature to 850°C at a heating rate of 5°C / min under a nitrogen atmosphere, and then maintained at 850°C for 4 hours to obtain yeast-derived nickel cobalt phosphide.
[0066] Examples 1-3 all successfully prepared yeast-derived nickel cobalt phosphide with uniform loading effect and excellent electrochemical performance. Specifically, taking Example 1 as an example, the characterization and performance are as follows:
[0067] (1) The SEM image of the freeze-dried yeast after culturing in Example 1 is as follows: Figure 1 As shown in the figure, the yeast body is spherical and has a smooth surface.
[0068] (2) The SEM image of the yeast-derived metal phosphide electrode material in Example 1 is as follows Figure 2 As shown in the figure, it can be seen that nickel cobalt phosphide is loaded on the rough yeast surface in the form of white particles with relatively uniform distribution.
[0069] (3) TEM image of the yeast-derived metal phosphide electrode material in Example 1 Figure 3 As shown in the figure, it can be seen that after calcination, the surface of the yeast is rough and loaded with small particles, but the overall shape is still spherical or ellipsoidal.
[0070] (4) Cyclic voltammetry tests were performed on the yeast-derived metal phosphide electrode material in Example 1 at different scan rates within a certain potential window. The test results are as follows: Figure 4 As shown in the figure, it can be seen that at different scan rates, the CV graph is rectangular, showing a double-layer effect. In general, the yeast-derived metal phosphide electrode material exhibits excellent electrochemical performance.
[0071] The first group of comparison
[0072] Comparative Examples 1-3 used other precursor combinations to prepare yeast-derived metal phosphide electrode materials. Other than that, the preparation method was the same as Example 1. The results were as follows:
[0073]
[0074] The second group of comparison
[0075] Comparative Examples 4-7 used precursor materials exceeding the preferred dosage range of the present invention (2.5-3.0 g) to prepare yeast-derived metal phosphide electrode materials. Other than that, the preparation method was the same as Example 1. The results are as follows:
[0076]
[0077]
[0078] This specific implementation is only an explanation of the present invention, not a limitation of the present invention. Any changes made by those skilled in the art after reading the specification of the present invention will be protected by the patent law as long as they are within the scope of the claims of the present invention.
Claims
1. A method for preparing a yeast-derived metal phosphide electrode material, characterized in that: First, the precursor substances tetrahydrated cobalt acetate and hexahydrated nickel nitrate were added to the yeast cell fluid to obtain the adsorbed Co 2+ and Ni 2+ yeast; then subjecting the obtained mixed solution to a hydrothermal reaction to obtain an intermediate product; finally, calcining the intermediate product in a nitrogen atmosphere to obtain yeast-derived nickel cobalt phosphide; The specific steps include: S1. Add 3-5g yeast powder to 80-100mL deionized water and incubate at 35℃ for 24-48h; S2. The culture solution was centrifuged and the precipitate was washed 3-4 times with deionized water; S3. The precursor substances cobalt acetate tetrahydrate and nickel nitrate hexahydrate are dissolved in the yeast cell solution and stirred; the amount of cobalt acetate tetrahydrate is 2.5-3.0g, the amount of nickel nitrate hexahydrate is 2.5-3.0g; S4. The obtained solution was centrifuged and the precipitate was washed with deionized water to obtain adsorbed Co 2+ and Ni 2+ of yeast cells; S5.Co 2+ / Ni 2+ / yeast cell mixed solution was transferred to the lining of the autoclave and subjected to hydrothermal reaction at 180-200°C for 24h; S6. After the reaction is completed and the temperature of the reaction solution drops to room temperature, it is centrifuged and the precipitate is washed with deionized water; S7. The centrifuged mixture is subjected to vacuum freeze drying for 24-36 hours to obtain an N and P-doped intermediate product; S8. The freeze-dried intermediate product is calcined at 800-900° C. for 3-5 hours under nitrogen to obtain yeast-derived nickel cobalt phosphide.
2. The method for preparing a yeast-derived metal phosphide electrode material according to claim 1, characterized in that: In step S1, the yeast powder used is Saccharomycete yeast powder.
3. The method for preparing a yeast-derived metal phosphide electrode material according to claim 1, characterized in that: In step S3, the stirring method is magnetic stirring, the stirring speed is 120-180 r / min, and the stirring time is 24-48 h.
4. The method for preparing a yeast-derived metal phosphide electrode material according to claim 1, characterized in that: In steps S2, S4 and S6, the centrifugal speed is 6000-8000 r / min.
5. The method for preparing a yeast-derived metal phosphide electrode material according to claim 1, characterized in that: In step S8, during calcination, the material is heated from room temperature to 850°C at a heating rate of 5°C / min, and then maintained at 850°C for 4 hours.
6. The yeast-derived metal phosphide electrode material obtained by the preparation method according to any one of claims 1 to 5.
7. Application of the yeast-derived metal phosphide electrode material prepared by the preparation method according to any one of claims 1 to 5 in the fields of capacitor deionization, supercapacitors, and sodium ion batteries.