Polysiloxane dispersants

By using a polysiloxane dispersant with multiple siloxane groups and covalently linked cyclic carboxylic anhydride groups, the shortcomings of existing dispersants in reducing viscosity and improving compatibility are overcome, achieving efficient dispersion and curing in non-aqueous compositions, suitable for thermal interface materials of electronic devices.

CN116888192BActive Publication Date: 2026-11-17BYK CHEMIE GMBH
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
CN202280016294.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-02-23
Filing Date
2022-02-21
Publication Date
2026-11-17
Estimated Expiration
2042-02-21

AI Technical Summary

Technical Problem

Existing dispersants, when dispersing pigments and fillers, are difficult to simultaneously reduce viscosity, maintain color fastness, and improve compatibility with different compositions, especially in non-polar compositions such as oil-based and silicone-based compositions. Furthermore, high filler loading leads to increased viscosity of conductive materials, affecting application performance.

Method used

Polysiloxanes with multiple siloxane groups and covalently linked cyclic carboxylic anhydride groups or their hydrolysis products are used as dispersants and prepared by a hydrosilylation reaction. They are used to disperse solid particles in non-aqueous compositions and are then cured in combination with a crosslinking agent.

Benefits of technology

It effectively reduces the viscosity of the composition, improves the color fastness of the pigment dispersion, and enhances compatibility with different compositions. In particular, when used as a thermal interface material in electronic devices, it achieves high thermal conductivity and good application performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004406272520000081
    Figure BDA0004406272520000081
  • Figure BDA0004406272520000251
    Figure BDA0004406272520000251
  • Figure BDA0004406272520000261
    Figure BDA0004406272520000261
Patent Text Reader

Abstract

This invention relates to the use of polysiloxanes as dispersants for solid particles in non-aqueous compositions, the polysiloxanes having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or its hydrolysis product covalently linked to the polysiloxane.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention relates to the use of polysiloxanes having a plurality of siloxane groups as dispersants for solid particles in non-aqueous compositions, and to non-aqueous compositions comprising polysiloxanes having a plurality of siloxane groups, a dispersion medium, and solid particles. The invention further relates to a method for dispersing solid particles in a non-aqueous composition.

[0002] A wide variety of substances can be used as dispersants in pigments and fillers. In addition to simple compounds with low molecular weights such as fatty acids and their salts, or various silanes such as alkyl or vinyl silanes, complex structures are also used.

[0003] EP 0931537 B1 describes the dispersion of organic and inorganic powders in an oil-containing composition using a compound containing a polysiloxane. The polymer is prepared by free radical copolymerization of a vinyl polysiloxane macromonomer with other vinyl monomers containing nitrogen-containing groups, polyoxyalkylene groups, anionic groups, or polylactone groups.

[0004] US 9217083 B2 describes copolymers containing at least one polysiloxane alkyl group and a backbone structure, said backbone structure being an addition compound of at least one amine and at least one epoxide. The invention further relates to the use of said product as a dispersant in organic and inorganic pigments and fillers in oil-based compositions, particularly in compositions containing organosilicon.

[0005] US 7329706 B2 describes a thermally conductive organosilicon composition comprising an organopolysiloxane, a thermally conductive filler, and a specific polysiloxane macromonomer with an alkoxysilyl group as a dispersant.

[0006] EP 2107078 A1 describes the reaction of Si-H functionalized polysiloxanes with allyl succinic anhydride to prepare anhydride-functionalized polysiloxanes. The anhydride-functionalized polysiloxanes are then hydrolyzed to form dicarboxylic acid-functionalized polysiloxanes. This material is used to treat titanium dioxide powder and zinc oxide.

[0007] JP 2020 / 059771A describes a dispersant having an organosilicon structure and a dicarboxylic anhydride structure located at one end of the organosilicon structure. This dispersant is used to treat zirconium oxide, which is then dispersed in silicone oil.

[0008] While existing dispersants provide acceptable stability for dispersed pigments and / or fillers, there is still a need for improved systems that reduce pigment settling, improve the color fastness of pigment dispersions, reduce viscosity, and ensure wider compatibility of dispersants with different compositions, such as compatibility with highly nonpolar compositions, for example, oil-based compositions and silicone-based compositions.

[0009] Compositions containing silicone can be non-curable or curable, such as condensation- or addition-curing compositions. In the case of addition curing, the composition consists of two parts: a SiH- and a vinyl-functionalized organopolysiloxane component, and typically uses a platinum-based catalyst. If the composition also contains one or more functional fillers or pigments, a dispersant is typically used to compatibilize the filler or pigment and the silicone. It has been found that known dispersants are insufficient to adequately disperse fillers or pigments. In particular, it is impossible to achieve a sufficiently low composition viscosity without adversely affecting the curing process.

[0010] In the field of modern electronics, thermal management plays an increasingly important role. Without thermally conductive materials, the development of microelectronics would not have enabled the creation of electronic devices capable of processing signals and data at unprecedented speeds. Electronic and / or integrated circuit (“IC”) devices, such as microprocessors, memory devices, printed circuits, and so on, are becoming smaller, but at the same time, their heat dissipation requirements are becoming greater.

[0011] To achieve high thermal conductivity in potting materials, gaskets, solder pastes, underfills, thermal interface materials (e.g., thermal gap fillers, thermal gap pads, silicone pads, phase change materials, thermal pastes, thermal gels, thermal encapsulants, thermal coatings), adhesives, sealants, and coatings, it is necessary to load highly thermally conductive particles. A significant drawback of highly filled systems is that the high filler load causes the viscosity of the conductive material to increase to undesirably high levels, significantly impairing application performance.

[0012] This invention seeks to address or mitigate the aforementioned drawbacks by combining effective dispersion and curing speed.

[0013] This invention relates to the use of polysiloxanes as dispersants in solid filler particles in non-aqueous compositions containing a dispersion medium, the polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or its hydrolysis product covalently linked to the polysiloxane, wherein the filler particle content is 500 to 2500 parts by weight per 100 parts by weight of dispersion medium.

[0014] The above-described use can also be described as a method for dispersing pigments / fillers in a non-aqueous composition, comprising the steps of: adding a polysiloxane to a non-aqueous composition containing solid particles, said polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or its hydrolysis product covalently linked to said polysiloxane; and then dispersing the solid particles in the non-aqueous composition. The liquid composition can be used as is or further reacted with a crosslinking agent to obtain a cured composition. In this case, there is no limitation on the curing mechanism of the liquid composition; curing can be based, for example, on a hydrosilylation reaction, condensation reaction, addition reaction, or free radical reaction induced by an organic peroxide.

[0015] A non-aqueous composition is one in which the water content, calculated based on the weight of the composition, is less than 10% by weight, preferably less than 5% by weight. In some embodiments, the non-aqueous composition is water-free or substantially water-free.

[0016] Polysiloxanes having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or its hydrolysis product covalently linked to the polysiloxane have been found to provide improved dispersion properties when used as dispersants in compositions containing solid particles. When used in potting materials, gaskets, solder pastes, underfills, thermal interface materials such as thermal gap fillers, thermal gap pads, silicone pads, phase change materials, thermal conductive pastes, thermal gels, thermal coating materials, thermal encapsulants, adhesives, sealants, and coating compositions, they can reduce viscosity.

[0017] The use of non-aqueous compositions as thermal interface materials is preferred, especially as thermal interface materials in electronic components.

[0018] As described above, the polysiloxane has at least one cyclic carboxylic anhydride group or its hydrolysis product covalently linked to the polysiloxane. The hydrolysis product of the cyclic carboxylic anhydride is the corresponding dicarboxylic acid or its salt. Suitable examples of the cyclic carboxylic anhydride group are those derived from: bicyclic [2.2.1]hept-5-ene-2,3-dicarboxylic anhydride, 5-norbornene-2,3-carboxylic anhydride, 1-cyclopentene-1,2-dicarboxylic anhydride, maleic anhydride, tetrahydrophthalic anhydride, citraconic anhydride, itaconic anhydride, allyl succinic anhydride. In some embodiments, the cyclic carboxylic anhydride group is in the form of a 5-membered ring. In a further embodiment, at least one cyclic carboxylic anhydride group is derived from allyl succinic anhydride. In another embodiment, the cyclic carboxylic anhydride group is present as a 6-membered ring. If the polysiloxane has two or more cyclic carboxylic anhydride groups covalently linked to it, these anhydride groups can be of the same or different types. In some embodiments, the polysiloxane has more than two cyclic carboxylic anhydride groups or their hydrolysis products covalently linked thereto. In other embodiments, the polysiloxane has two cyclic carboxylic anhydride groups linked thereto. In further embodiments, the polysiloxane has one cyclic carboxylic anhydride group or its hydrolysis product linked thereto. However, mixtures of polysiloxanes may also be used, such as a first polysiloxane having one or more cyclic carboxylic anhydride groups or their hydrolysis products linked thereto, and a second different mixture of polysiloxanes having one or more cyclic carboxylic anhydride groups or their hydrolysis products linked thereto.

[0019] Cyclic carboxylic anhydride groups or their hydrolysis products can be located at various positions along the polysiloxane chain. In some embodiments, at least one anhydride group is covalently attached to the polysiloxane as an end group located at both ends of the polysiloxane chain. This polymer form with two anhydride groups located at both ends of the polysiloxane chain can also be called an ABA polymer. In other embodiments, at least one anhydride group is covalently attached to the polysiloxane as an end group located at only one end of the polysiloxane chain. This polymer form with an anhydride group located at only one end of the polysiloxane chain can also be called a macromonomer. Alternatively or additionally, at least one anhydride group is covalently attached to the polysiloxane at a non-terminal position. When several anhydride groups are attached from different positions along the polysiloxane chain, this polymer form can also be called a comb polymer.

[0020] Polysiloxanes having multiple siloxane groups typically have 1 to 15 cyclic carboxylic anhydride groups or their hydrolysis products covalently linked thereto. In a preferred embodiment, 1 to 10, more preferably 1 to 2 cyclic carboxylic anhydride groups or their hydrolysis products are covalently linked to the polysiloxane. In some embodiments, mixtures of polysiloxanes with different numbers of cyclic carboxylic anhydride groups or their hydrolysis products can be used. If such a mixture is used, the number of cyclic carboxylic anhydride groups or their hydrolysis products relates to the average number of cyclic carboxylic anhydride groups or their hydrolysis products. In a preferred embodiment, an average of 0.7 to 3.0 cyclic carboxylic anhydride groups or their hydrolysis products are covalently linked to the polysiloxane molecule.

[0021] Polysiloxanes having multiple siloxane groups and at least one cyclic carboxylic anhydride group or its hydrolysis product covalently linked to the polysiloxane can be prepared according to known methods. In a preferred embodiment, the cyclic carboxylic anhydride group or its hydrolysis product is linked to the polysiloxane via a Si-C bond.

[0022] In one embodiment, the compound is prepared by a hydrosilylation reaction, wherein a polysiloxane having a plurality of siloxane groups and at least one Si-H group reacts with an acid anhydride compound having olefinically unsaturated groups. This reaction is typically catalyzed by a metal-based catalyst. Details of this hydrosilylation reaction and suitable conditions are generally known.

[0023] The hydrosilylation catalyst used is preferably a noble metal or its compound, such as platinum, rhodium, and palladium or their compounds, more preferably a platinum compound. Particularly preferred platinum compounds are hexachloroplatinic acid, alcoholic solutions of hexachloroplatinic acid, complexes of platinum and aliphatic unsaturated hydrocarbon compounds, and platinum-vinylsiloxane complexes. However, platinum black and platinum on activated carbon can also be used. For example, if a platinum compound is used, 1 to 50 ppm of platinum metal is preferred.

[0024] The progress of the hydride alkylation reaction can be determined by measuring the gas volume of the remaining SiH groups or by infrared spectroscopy (hydride at 2150 cm⁻¹). -1 The absorption band at the location is used for monitoring. The polysiloxane of the present invention preferably does not contain residual Si-H groups.

[0025] When a polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or its hydrolysis product covalently linked to the polysiloxane is prepared by a hydrogenation silylation reaction of an olefinic unsaturated anhydride, a covalent bond is formed between the polysiloxane and at least one anhydride group. A specific example of an olefinic unsaturated anhydride suitable for preparing the polysiloxane of the present invention is allyl succinic anhydride.

[0026] The above synthetic route requires a polysiloxane having multiple siloxane groups and at least one Si-H group as a starting material. A suitable polysiloxane having at least one Si-H group can be represented by the following general formula (I):

[0027] M a M′ b D c D′ d T e Q f (I)

[0028] in

[0029] M represents [R3SiO] 1 / 2 ]

[0030] ·M′ represents [R2SiHO 1 / 2 ]

[0031] ·D represents [R2SiO] 2 / 2 ]

[0032] ·D′ represents [RSiHO] 2 / 2 ]

[0033] ·T represents [RSiO] 3 / 2 ]

[0034] Q represents SiO 4 / 2 ]

[0035] •a is an integer from 0 to 10, preferably an integer from 0 to 1, and more preferably 1.

[0036] • b is an integer from 0 to 10, preferably an integer from 1 to 2, and more preferably 1.

[0037] c is an integer from 0 to 500, preferably an integer from 2 to 300, and more particularly an integer from 5 to 250.

[0038] ·d is an integer from 0 to 100, preferably an integer from 0 to 50, and more particularly an integer from 0 to 30.

[0039] ·e is an integer from 0 to 10, preferably an integer from 0 to 5, and more specifically 0.

[0040] f is an integer from 0 to 10, preferably an integer from 0 to 5, and more specifically 0, provided that a+b≧2 and b+d≧1.

[0041] ·R represents C1-C independently 30 Hydrocarbon group, preferably methyl, octyl or phenyl, (α-methyl)styryl, more preferably methyl.

[0042] It is generally known in the art to describe polysiloxanes using M, D, T, and Q units.

[0043] Typically, classical equilibrium reactions known in the art are used to synthesize polysiloxanes with SiH groups.

[0044] Typically, polysiloxanes have 1 to 15 SiH groups, preferably 1 to 10 SiH groups, and more preferably 1 to 2 SiH groups. Typically, polysiloxanes have 4 to 70 silicon atoms, preferably 10 to 50 silicon atoms.

[0045] If desired, polysiloxanes having multiple siloxane groups and two anhydride groups covalently linked to the polysiloxane can be prepared by other suitable synthetic routes, such as the equilibrium reaction of anhydride-functionalized polysiloxanes with ABA structures, see, for example, EP 0 112 845 B1, particularly Example 4 in that document.

[0046] Polysiloxanes having a plurality of siloxane groups and at least one anhydride group covalently linked to the polysiloxane typically have a number average molecular weight of 300 to 15,000 g / mol, preferably 500 to 10,000 g / mol, and even more preferably 800 to 8,000 g / mol.

[0047] Number-average molecular weight was determined by gel permeation chromatography at 22°C using a Waters 2695 separation module and a Waters 2414 refractive index detector. Toluene was a suitable eluent, and calibration was performed using polydimethylsiloxane standards.

[0048] Optionally, a polysiloxane having multiple siloxane groups and at least one anhydride group covalently linked to the polysiloxane may have additional structural segments. These optional segments may be included to adjust and fine-tune compatibility with systems using them and other properties of the polysiloxane. Examples of such optional segments are polyether segments, such as those based on polyethylene oxide and / or polypropylene oxide; polyester segments, hydrocarbon segments, fluorinated hydrocarbon segments, and polyurethane segments. These optional segments may be attached to the polysiloxane backbone via hydrosilylation or dehydrogenation condensation reactions. Such dehydrogenation condensation reactions are suitably catalyzed by metal complexes. This type of reaction is described in German patent application DE 102005051939A. These optional segments are preferentially attached to the polysiloxane backbone via hydrosilylation reactions.

[0049] In many embodiments, the polysiloxane having a plurality of siloxane groups and at least one anhydride group covalently linked to the polysiloxane is liquid at room temperature. The polysiloxane can be used and included in liquid compositions according to the invention, for example as a 100% active substance. If desired, the polysiloxane may also be diluted with an organic solvent or oil or organosilicon before being included in the liquid composition. In other embodiments, the polysiloxane may be included in the liquid composition as an emulsion or dispersion. The amount of polysiloxane contained in the liquid composition is preferably used to achieve effective dispersion performance. The specific amount depends on the content of solid particles in the composition and the desired degree of dispersion; the solid particles are, for example, pigments and / or fillers. Typically, the polysiloxane content in the liquid composition is 0.001 to 10.000% by weight, preferably 0.010 to 8.000% by weight, more preferably 0.050 to 7.000% by weight, or 0.060 to 6.000% by weight, or 0.080 to 5.000% by weight, particularly 0.100 to 2.000% by weight, in each case based on the total weight of the composition.

[0050] The pigment and / or filler dispersions according to the invention can be used in a wide range of formulations, including resins, oils, greases, lubricants, rubber materials, potting materials, gaskets, solder pastes, underfills, thermal interface materials (e.g., thermal gap fillers, thermal gap pads, silicone pads, phase change materials, thermal conductive pastes, thermal gels, thermal coating materials, thermal encapsulants), adhesives, sealants, coatings, waxes, or material compositions. The dispersions can also be used in formulations produced in the personal care industry, or for electronic applications in the electronics industry, marine industry, medical applications, construction industry, or in the electronics, battery, and automotive industries. Examples include cosmetics, electronic paper (e.g., displays in e-books), encapsulation of microelectronic chips, underwater skin coatings (e.g., antifouling coatings), silicone tubing, or lubricating additives for brake components.

[0051] The dispersions described are particularly suitable for use in thermal interface materials (TIM) products. These materials serve as interfaces between devices or their components to dissipate heat from these devices (e.g., microprocessors). A typical TIM typically comprises a polymer matrix and one or more thermally conductive fillers. TIM technologies for electronic devices encompass a wide range of materials, such as epoxides, greases, sheets, pads, phase change materials, filled polymer matrices such as elastomers, gels, carbon-based materials, and adhesives. U.S. Patent No. 6,469,379 describes a silicone-based TIM comprising a vinyl-terminated silicone polymer; a silicone crosslinker having terminal silicon-hydride units; a chain extender; and thermally conductive fillers, such as metals (e.g., aluminum, silver, etc.) and / or ceramics (e.g., aluminum nitride, alumina, zinc oxide, etc.).

[0052] The use of non-aqueous compositions as thermal interface materials is preferred, especially as thermal interface materials in electronic components.

[0053] One aspect of the invention relates to a method for preparing dispersions, the method comprising mixing at least one pigment and / or filler in a medium selected from at least one silicone oil and silicone rubber material, with the aid of at least one anhydride-modified polysiloxane of the invention. These dispersions preferably represent pigment formulations and / or filler formulations, which are preferably used in various compositions.

[0054] In a further embodiment, the surface of the dry filler is modified by treating the polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or a hydrolysis product thereof covalently linked to the polysiloxane, and then the treated filler is mixed with a dispersion medium.

[0055] In a preferred embodiment, the non-aqueous composition contains a dispersion medium that is different from the polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or its hydrolysis product.

[0056] In a further preferred embodiment, the dispersion medium comprises organosilicon.

[0057] In some implementations, the silicone is silicone oil or silicone rubber.

[0058] Examples of silicone oils include those with the following structures:

[0059]

[0060] R 3 4-z Si(OSi(CH3)3) z (IV)

[0061] Where R 2Selected from the following group: hydrogen, hydroxyl, alkyl or fluorinated alkyl having 2 to 20 carbon atoms, aryl, aminoalkyl, C 6-22 Alkyl groups, and those having the formula (CH3)3SiO[(CH3)2SiO] y The group is Si(CH3)2CH2CH2-, where y is an integer from 0 to 500. R 3 It is C 1-20 Alkyl groups. In formula (II), h is an integer from 0 to 1000, i is an integer from 0 to 1000, provided that h+i is in the range of 1 to 2000, and each j and k is independently 0, 1, 2, or 3. In formula (III), l and m are integers from 0 to 8, where l+m is in the range of 3 to 8; and in formula (IV), z is an integer from 1 to 4. R 2 Examples of the groups include methyl, ethyl, propyl, butyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, trifluoropropyl, nonafluorohexyl, heptadecanylfluorodecyl, phenyl, aminopropyl, dimethylaminopropyl, aminoethylaminopropyl, stearyloxy, butoxy, ethoxy, propoxy, hexadecyloxy, myristyloxy, styryl, and α-methylstyryl, with hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, trifluoropropyl, phenyl, aminopropyl, and aminoethylaminopropyl. Examples of silicone oils include: organopolysiloxanes with low or high viscosity, such as dimethylpolysiloxane, methylphenylpolysiloxane, methyl-hydropolysiloxane, and dimethylsiloxane-methyl-phenylsiloxane copolymers; cyclosiloxanes, such as octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), dodecylcyclohexasiloxane (D6), tetramethyltetrahydrocyclotetrasiloxane (H4), and tetramethyltetraphenylcyclotetrasiloxane; tri-trimethylsiloxysilane (M3T), tetra-trimethylsiloxysilane (M4Q); branched siloxanes, such as tri-trimethylsiloxypropylsilane, tri-trimethylsiloxy-butylsilane, tri-trimethylsiloxyhexylsilane, and tri-trimethylsiloxyphenylsilane; and organosilicones modified with higher alcohols, such as stearyloxysilanes, alkyl-modified organosilicones, amino-modified organosilicones, and fluorine-modified organosilicones.

[0062] In some embodiments, the silicone dispersion medium is a crosslinkable silicone. Crosslinkable silicones can exist in various compound forms, such as silicone oils, high-solids silicones, waterborne silicones, silicone alkyd resins, silicone-treated polyesters, or silicone-treated acrylic resins. Crosslinking can be achieved through moisture curing, hydrosilylation curing, irradiation curing, free radical-induced curing, or a combination of irradiation and heat curing (dual curing). Crosslinkable silicones are also known as silicone rubbers or liquid silicone rubbers.

[0063] As silicon-linked groups in organopolysiloxanes, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecanyl, octadecyl, nonadecanyl, eicosyl, and other straight-chain alkyl groups are suggested; isopropyl, tert-butyl, isobutyl, 2-methylundecyl, 1-hexylheptyl, and other branched alkyl groups; cyclopentyl, cyclohexyl, cyclododecyl, and other cycloalkyl groups; vinyl, allyl, butenyl, pentenyl, hexenyl, and other alkenyl groups; phenyl, tolyl, xylyl, and other aryl groups; benzyl, phenethyl, 2-(2,4,6-trimethylphenyl)propyl, and other aralkyl groups; 3,3,3-trifluoropropyl, 3-chloropropyl, and other haloalkyl groups. Preferably, these groups are alkyl, alkenyl, or aryl, with methyl, vinyl, or phenyl groups being particularly preferred. Furthermore, there is no limitation on the viscosity of the organopolysiloxane at 25°C. However, the viscosity is preferably in the range of 20 to 100,000 mPa·s, more preferably 50 to 100,000 mPa·s, even more preferably 50 to 50,000 mPa·s, and particularly preferably 100 to 50,000 mPa·s. This is because when the viscosity at 25°C is less than the lower limit of the above range, the physical properties of the resulting organosilicon composition tend to decrease; on the other hand, when the viscosity exceeds the upper limit of the above range, the processability of the resulting organosilicon composition tends to decrease. There is no limitation on the molecular structure of these organopolysiloxanes, which can be, for example, linear, branched, partially branched linear, or dendritic (dendritic) structures, and preferably linear or partially branched linear structures. Examples of such organopolysiloxanes include, for example, homopolymers having the above molecular structure, copolymers having the above molecular structure, or mixtures of the above polymers. Examples of such organopolysiloxanes may include: dimethylpolysiloxanes whose molecular chains are both ends capped with dimethylvinylsiloxy groups; dimethylpolysiloxanes whose molecular chains are both ends capped with methylphenylvinylsiloxy groups; dimethylsiloxane-methylphenylsiloxane copolymers whose molecular chains are both ends capped with dimethylvinylsiloxy groups; dimethylsiloxane-methylvinylsiloxane copolymers whose molecular chains are both ends capped with dimethylvinylsiloxy groups; dimethylsiloxane-methylvinylsiloxane copolymers whose molecular chains are both ends capped with trimethylsiloxy groups; methyl(3,3,3-trifluoropropyl)-polysiloxanes whose molecular chains are both ends capped with dimethyl-vinylsiloxy groups; dimethylsiloxane-methylvinylsiloxane copolymers whose molecular chains are both ends capped with silanol groups; and dimethylsiloxane-methylvinyl-siloxane-methylphenylsiloxane copolymers whose molecular chains are both ends capped with silanol groups. 1 / 2The siloxane unit shown, formula (CH3)2(CH2=CH)SiO 1 / 2 The siloxane unit shown, with the formula CH3SiO 3 / 2 The siloxane unit shown and the formula (CH3)2SiO 2 / 2 The organosiloxane copolymers composed of siloxane units shown; dimethyl polysiloxanes whose molecular chains are both ends capped with silanol groups; dimethylsiloxane-methylphenylsiloxane copolymers whose molecular chains are both ends capped with silanol groups; dimethyl polysiloxanes whose molecular chains are both ends capped with trimethoxysiloxy groups; dimethylsiloxane-methylphenylsiloxane copolymers whose molecular chains are both ends capped with trimethoxysilyl groups; dimethyl polysiloxanes whose molecular chains are both ends capped with methyldimethoxysiloxy groups; dimethyl polysiloxanes whose molecular chains are both ends capped with triethoxysiloxy groups; dimethyl polysiloxanes whose molecular chains are both ends capped with trimethoxysilylethyl groups; and mixtures of two or more of the above compounds.

[0064] When the composition is cured by a hydrosilylation reaction, the dispersion medium is preferably an organopolysiloxane having an average of not less than 0.1 silicon-linked alkenyl groups per molecule. More preferably, the dispersion medium is an organopolysiloxane having an average of not less than 0.5 silicon-linked alkenyl groups per molecule, and particularly preferably, it is an organopolysiloxane having an average of not less than 0.8 silicon-linked alkenyl groups per molecule. This is because when the average number of silicon-linked alkenyl groups per molecule is less than the lower limit of the above range, the resulting composition tends not to cure sufficiently. The silicon-linked alkenyl groups in the organopolysiloxane are, for example, the same alkenyl groups as those described above, preferably vinyl groups. In addition, other silicon-linked groups that are not alkenyl groups in the organopolysiloxane are, for example, the same straight-chain alkyl, branched alkyl, cycloalkyl, aryl, aralkyl, and haloalkyl groups as those described above. They are preferably alkyl and aryl, and particularly preferably methyl and phenyl. There are no restrictions on the molecular structure of such organopolysiloxanes, which may have, for example, the same structures as those described above, preferably linear structures or partially branched linear structures. Such organopolysiloxanes may be, for example, homopolymers having the above-described molecular structures, copolymers having the above-described molecular structures, or mixtures of these polymers. Such organopolysiloxanes may be, for example, organopolysiloxanes having the same alkenyl groups as those described above.

[0065] When the composition is cured by a condensation reaction, the dispersion medium is an organopolysiloxane having at least two silanol groups or hydrolyzable groups attached to silicon per molecule. Examples of hydrolyzable groups attached to silicon in organopolysiloxanes include, for example: methoxy, ethoxy, propoxy, and other alkoxy groups; vinyloxy, propenyloxy, isopropenyloxy, 1-ethyl-2-methylvinyloxy, and other alkenyloxy groups; methoxyethoxy, ethoxyethoxy, methoxypropoxy, and other alkoxyalkoxy groups; acetoxy, octanoyloxy, and other acyloxy groups; dimethyl ketoxime, methyl ethyl ketoxime, and other ketoxime groups; dimethylamino, diethylamino, butylamino, and other amino groups; dimethylaminooxy, diethylaminooxy, and other aminooxy groups; N-methylacetamido, N-ethylacetamido, and other acylamino groups. Furthermore, the silanol groups and the hydrolyzable groups attached to silicon in the organopolysiloxane are, for example, the same straight-chain alkyl, branched alkyl, cycloalkyl, alkenyl, aryl, aralkyl, and haloalkyl groups as described above. There are no restrictions on the molecular structure of such organopolysiloxanes; they may have, for example, the same structures as those described above, preferably linear or partially branched linear structures. Such organopolysiloxanes are, for example, organopolysiloxanes having at least two silanol groups or hydrolyzable groups attached to silicon per molecule, said groups being the same as those described above.

[0066] When the composition is cured via an organic peroxide-induced free radical reaction, there are no limitations on the organopolysiloxane of the dispersion medium. However, organopolysiloxanes having at least one alkenyl group linked to silicon are preferred. In such organopolysiloxanes, the silicon-linked group is, for example, the same linear alkyl, branched alkyl, cycloalkyl, alkenyl, aryl, aralkyl, and haloalkyl groups as described above, and preferably alkyl, alkenyl, or aryl, particularly methyl, vinyl, and phenyl. There are no limitations on the molecular structure of the organopolysiloxane, which may be, for example, the same structures described above, preferably linear or partially branched linear structures. Such organopolysiloxanes are, for example, homopolymers having the above molecular structures, copolymers having the above molecular structures, or mixtures of the above polymers. Such organopolysiloxanes are, for example, the same organopolysiloxanes as those described above.

[0067] Silicone rubber can be classified as room temperature vulcanizing (RTV) silicone rubber or high temperature vulcanizing (HTV) silicone rubber. They are commonly known, for example, see US 6172150 B1, WO 2018051158 A1, WO 2003078527A1, US 6194508B1 and WO 2003057782A1.

[0068] Liquid silicone rubber is further described in WO 2015003978 A1, WO 2018051158 A1 and WO 2020223864A1.

[0069] Suitable crosslinkable silicones are commercially available, for example, from Wacker Chemie AG. and

[0070] As described above, polysiloxanes having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or its hydrolysis product covalently linked to the polysiloxane are used as dispersants for solid particles in non-aqueous compositions. Examples of solid particles include pigments and fillers.

[0071] Solid particles can be surface-modified, wherein the surface can, for example, have hydrophilic, amphiphilic, or hydrophobic compounds or groups. Surface treatment can include providing pigments with a thin hydrophilic and / or hydrophobic inorganic or organic layer by methods known to those skilled in the art.

[0072] In a preferred embodiment, the average particle size of the solid particles is in the range of 0.1 to 500.0 μm, preferably 0.1 to 100 μm.

[0073] Average particle size involves D 50 The average particle size was determined by laser diffraction analysis according to ISO 13320:2009-10.

[0074] In a further preferred embodiment, the solid particles comprise alumina particles. Particularly preferred is that the alumina particles comprise at least one of spherical alumina particles with an average particle size of 1.0 to 50.0 μm and alumina particles with an irregular shape and an average particle size of 0.1 to 50.0 μm.

[0075] Pigments include inorganic and organic pigments, pigment black, effect pigments such as pearlescent and / or metallic effect pigments, glitter pigments, and mixtures thereof.

[0076] Suitable organic pigments include, for example, nitroso compounds, nitro compounds, azo compounds, xanthones, quinoline, anthraquinones, phthalocyanines, metal complexes, isoindolineones, dihydroisoindolines, quinacridones, perinones, perylene, diketopyrrolopyrroles, thioindole, and dioxindoline. Azides, triphenylmethane, and quinacridone compounds. In addition, organic pigments may be selected, for example, from: carmine, carbon black, aniline black, azo yellow, quinacridone, and phthalocyanine blue. Examples of D&C red (CI 45), D&C orange (CI 45), D&C red 3 (CI 45530), D&C red 7 (CI 15850), D&C red 4 (CI 15510), D&C red 33 (CI 17200), D&C red 34 (CI 15880), D&C yellow 5 (CI 19140), D&C yellow 6 (CI 15985), D&C green (CI 61570), D&C yellow 10 (CI 77002), D&C green 3 (CI 42053) and / or D&C blue 1 (CI 42090).

[0077] Suitable inorganic pigments include, for example, metal oxides, or other metal compounds that are sparingly soluble in water or at least substantially insoluble in water, particularly oxides of titanium, such as titanium dioxide (CI 77891), zinc, iron, such as iron oxide red and iron oxide black (CI 77491 (red), 77499 (black)), or iron oxide hydrate (CI 77492, yellow), zirconium, silicon, manganese, aluminum, cerium, chromium, and mixed oxides of the above elements, and mixtures thereof. Other suitable pigments are barium sulfate, zinc sulfide, manganese violet, ultramarine blue, and Berlin blue pigments.

[0078] Regarding pearlescent pigments, one or more of the following types of pearlescent pigments can be used:

[0079] • Natural pearlescent pigments, such as "fish scale silver" (a mixture of guanidine / hypoxanthine crystals derived from fish scales) and "mother-of-pearl" (ground mussel shells).

[0080] • Single-crystal pearlescent pigments, such as bismuth oxychloride (BiOCl) or small flakes of titanium dioxide, and

[0081] • Pearl pigments in a layered substrate.

[0082] Suitable flake-shaped transparent substrates for coating with layered substrate pearlescent pigments are non-metallic, natural, or synthetic flake-shaped substrates. These substrates are preferably substantially transparent, and more preferably transparent, i.e., at least partially transparent to visible light.

[0083] Small, transparent flake substrates may be selected from the group consisting of: natural mica, synthetic mica, glass flakes, SiO2 flakes, Al2O3, kaolin, graphite, talc, polymer flakes, small flakes of bismuth oxychloride, small flake substrates containing an inorganic-organic mixed layer, and mixtures thereof.

[0084] In addition to pearlescent pigments, metallic effect pigments can also be used in this invention.

[0085] The small, sheet-like metal substrate may, in this case, specifically comprise pure metals and / or their metal alloys. In particular, the metal substrate may preferably be selected from silver, aluminum, iron, chromium, nickel, molybdenum, gold, copper, zinc, tin, stainless steel, magnesium, steel, bronze, brass, titanium, and their alloys.

[0086] In a further embodiment, the solid particles comprise fillers. All kinds of fillers known in the art can be used. In particular, functional fillers are used in the composition. Thermally conductive materials help remove heat from the components and contain one or more thermally conductive fillers as functional fillers. The filler material comprises a solid material having a higher thermal conductivity than the matrix material. Suitable filler materials for use in embodiments of the invention include, for example, aluminum powder, copper powder, nickel powder, or other metal powders; alumina powder, magnesium oxide powder, barium oxide powder, chromium oxide powder, precipitated silica, pyrolytic silica, titanium dioxide powder, or other metal oxide powders; boron nitride powder, aluminum nitride powder, or other metal nitride powders; boron carbide powder, titanium carbide powder, silicon carbide powder, or other metal carbide powders; Fe-Si alloys, Fe-Al alloys, Fe-Si-Al alloys, Fe-Si- Powders of Cr alloys, Fe-Ni alloys, Fe-Ni-Co alloys, Fe-Ni-Mo alloys, Fe-Co alloys, Fe-Si-Al-Cr alloys, Fe-Si-B alloys, and Fe-Si-Co-B alloys; and other soft magnetic alloy powders; Mn-Zn ferrite, Mn-Mg-Zn ferrite, Mg-Cu-Zn ferrite, Ni-Zn ferrite, Ni-Cu-Zn ferrite, Cu-Zn ferrite, or other ferrites, and mixtures of two or more of the above materials. Furthermore, the filler shape can be, for example, spherical, needle-like, disc-like, rod-like, elliptical, or irregular. When the composition of the present invention or the cured organosilicon product obtained by curing the composition of the present invention is required to have electrical insulating properties, the filler is preferably a metal oxide powder, a metal nitride powder, or a metal carbide powder, and particularly preferably alumina powder. There is no limitation on the average particle size of the filler, but the average particle size is preferably in the range of 0.1 to 500 μm, and particularly preferably 0.1 to 100 μm. When alumina particles are used as a thermally conductive filler, it is preferably a mixture of the following particles: (B1) spherical alumina particles with an average particle size of 1 to 50 μm, and (B2) spherical or irregularly shaped alumina particles with an average particle size of 0.1 to 50 μm. Furthermore, in this mixture, the content of component (B1) is preferably in the range of 30-90% by weight, and the content of component (B2) is preferably in the range of 10-70% by weight, based on the total amount of components (B1) and (B2). There is no limitation on the filler content in this composition. However, in order to form an organosilicon composition with excellent thermal conductivity, the filler content in the composition, by volume%, is preferably at least 30% by volume, more preferably in the range of 30-90% by volume, even more preferably 60-90% by volume, and particularly preferably 80-90% by volume%. In order to form an organosilicon composition with excellent thermal conductivity, the filler content in the composition is preferably at least 50% by weight, more preferably in the range of 70-98% by weight, and especially preferably in the range of 90-97% by weight.Fillers can have different particle sizes and can exist not only alone, but also as mixtures, and can also be coated with each other.

[0087] Specifically, the filler content is 500 to 2500 parts by weight, more preferably 500 to 2000 parts by weight, and particularly preferably 800 to 2000 parts by weight per 100 parts by weight of the dispersion medium. This is because when the filler content is less than the lower limit of the above range, the thermal conductivity of the resulting silicone composition tends to decrease; while on the other hand, when the filler content exceeds the upper limit of the above range, the viscosity of the resulting silicone composition increases, and its processability tends to deteriorate.

[0088] The composition may also contain a curing agent, which allows for the production of a curable composition. When the composition is cured by a hydrosilylation reaction, the curing agent is made from a platinum catalyst and an organopolysiloxane having an average of at least two hydrogen atoms bonded to silicon per molecule. The groups bonded to silicon atoms in the organopolysiloxane are, for example, the same straight-chain alkyl, branched alkyl, cycloalkyl, aryl, aralkyl, and haloalkyl groups described above, preferably, for example, alkyl or aryl, and particularly preferably, for example, methyl or phenyl.

[0089] The proposed organopolysiloxanes include, for example, dimethylpolysiloxanes whose molecular chains are both ends capped with dimethylhydrosiloxy groups, dimethylsiloxane-methylhydrosiloxane copolymers whose molecular chains are both ends capped with trimethylsiloxy groups, and dimethylsiloxane-methylhydrosiloxane copolymers whose molecular chains are both ends capped with dimethylhydrosiloxy groups, formed from a polymer having the formula (CH3)3SiO 1 / 2 The siloxane unit, having the formula (CH3)2HSiO 1 / 2 Siloxane units and having the formula SiO 4 / 2 Organosiloxane copolymers composed of siloxane units, and mixtures of two or more of the above compounds.

[0090] In the composition, the amount of organopolysiloxane having an average of at least two silicon-bonded hydrogen atoms per molecule is necessary for curing the composition. Specifically, this amount is preferably sufficient to provide 0.1-10.0 mol, more preferably 0.1-5.0 mol, and particularly preferably 0.1-3.0 mol of silicon-bonded hydrogen atoms from the component, based on 1 mol of silicon-bonded alkenyl groups in the dispersion medium. This is because when the content of the component is less than the lower limit of the above range, the resulting organosilicon composition tends not to cure completely; on the other hand, when the content exceeds the upper limit of the above range, the resulting cured organosilicon product is very hard and tends to have many cracks on the surface. Additionally, a platinum catalyst is used to promote the curing of the composition of the present invention. Examples of such catalysts include, for example, chloroplatinic acid, alcoholic solutions of chloroplatinic acid, platinum olefin complexes, platinum alkenylsiloxane complexes, and platinum carbonyl complexes. In this composition, the amount of platinum catalyst is necessary for curing the composition of the present invention. Specifically, this content is sufficient to provide, by weight, preferably 0.01 ppm to 1,000 ppm, particularly preferably 0.1 ppm to 500 ppm of platinum metal from this component, relative to the amount of the dispersion medium. This is due to the fact that when the content of this component is less than the lower limit of the above range, the resulting silicone composition tends not to cure completely; while on the other hand, when the amount added exceeds the upper limit of the above range, it does not significantly improve the curing rate of the resulting silicone composition.

[0091] When the composition is cured by a condensation reaction, the curing agent is characterized by comprising a silane or a partially hydrolyzed product thereof having at least two hydrolyzable groups attached to silicon per molecule, and, if necessary, a condensation reaction catalyst. The hydrolyzable groups attached to silicon in the silane are, for example, the same alkoxy, alkoxyalkoxy, acyloxy, ketoxime, alkenyl, amino, aminooxy, and amide groups described above. Examples of other groups that can be incorporated into the silicon atoms of the silane, besides the aforementioned hydrolyzable groups, include, for example, the same straight-chain alkyl, branched alkyl, cycloalkyl, alkenyl, aryl, aralkyl, and haloalkyl groups described above. Suggested silanes or partially hydrolyzed products thereof include, for example, methyltriethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, and ethyl orthosilicate.

[0092] In the composition, the content of silane or its partially hydrolyzed derivative is necessary for curing the composition of the present invention. Specifically, this content is preferably 0.01 to 20 parts by weight, and particularly preferably 0.1 to 10 parts by weight per 100 parts by weight of the dispersion medium. This is because when the content of silane or its partially hydrolyzed derivative is less than the lower limit of the above range, the storage stability of the resulting composition deteriorates; in addition, its adhesive properties tend to decrease. On the other hand, when the content exceeds the upper limit of the above range, the curing of the resulting composition tends to be slower. Furthermore, the condensation reaction catalyst is an optional component and is not necessary when using silanes having, for example, amino, amino, ketoxime, and other hydrolyzable groups as curing agents. Suggested condensation catalysts include, for example, tetrabutyl titanate, tetraisopropyl titanate, and other organotitanates; diisopropoxydi(acetylacetate)titanium, diisopropoxydi(ethylacetylacetonate)titanium, and other chelating organotitanate compounds; tri(acetylacetonate)aluminum, tri(ethylacetylacetonate)aluminum, and other organoaluminum compounds; tetra(acetylacetonate)zirconium, tetrazirconium butyrate, and other organozirconium compounds; dibutyltin dioctanoate, dibutyltin dilaurate, butyltin-2-ethylhexanoate, and other organotin compounds; tin naphthenate, tin oleate, tin butyrate, cobalt naphthenate, zinc stearate, and other metal salts of organocarboxylic acids; hexylamine, dodecylamine phosphate, and other amine compounds or their salts; benzyltriethylammonium acetate, and other quaternary ammonium salts; potassium acetate, lithium nitrate, and other alkali metal salts of lower fatty acids; dimethylhydroxylamine, diethylhydroxylamine, and other dialkylhydroxylamines; and organosilicon compounds containing guanidine groups. The content of the condensation reaction catalyst in the composition is variable and should be sufficient to cure the composition of the invention. Specifically, the content is preferably 0.01 to 20.00 parts by weight, and particularly preferably 0.1 to 10.0 parts by weight per 100 parts by weight of the dispersion medium. This is because if a catalyst is necessary, when the catalyst content is less than the lower limit of the above range, it tends to be difficult to completely cure the resulting composition; on the other hand, when the content exceeds the upper limit of the above range, the storage stability of the resulting composition tends to decrease.

[0093] When the composition is cured via a free radical reaction induced by an organic peroxide, the curing agent is suitably an organic peroxide. Suggested organic peroxides include, for example, benzoyl peroxide, dicumyl peroxide, 2,5-dimethyl-di(2,5-tert-butylperoxy)hexane, di-tert-butyl peroxide, and tert-butyl perbenzoate. The content of the organic peroxide is the amount necessary for curing the composition. Specifically, this content is preferably 0.1 to 5.0 parts by weight per 100 parts by weight of the above-described dispersion medium of an organopolysiloxane.

[0094] In particular, when the compositions of the present invention are cured by a hydrosilylation reaction, in order to adjust the curing rate of the compositions and improve their processability, it is preferable to combine the compositions with the following substances: 2-methyl-3-butyn-2-ol, 2-phenyl-3-butyn-2-ol, 1-ethynyl-1-cyclohexanol, and other acetylene compounds; 3-methyl-3-penten-1-yne, 3,5-dimethyl-3-hexen-1-yne, and other ene-yne ​​compounds; and additionally, hydrazine compounds, phosphine compounds, thiols, and other curing reaction inhibitors. There is no limitation on the content of the curing reaction inhibitors, however, the content is preferably 0.0001 to 1.0% by weight relative to the amount of the composition of the present invention. When the compositions of the present invention are curable, there is no limitation on the curing method. This method may, for example, involve molding the compositions of the present invention and then allowing them to stand at room temperature, or molding the compositions of the present invention and then heating them to 50-200°C. Furthermore, there are no restrictions on the physical properties of the resulting organosilicon, but suggested forms include, for example, gels, low-hardness rubbers, or high-hardness rubbers.

[0095] The present invention also relates to a non-aqueous composition comprising:

[0096] a) A polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or its hydrolysis product covalently linked to the polysiloxane.

[0097] b) Dispersion medium, and

[0098] c) Solid filler particles

[0099] The content of the filler particles is 500 to 2500 parts by weight per 100 parts by weight of dispersion medium.

[0100] In a preferred embodiment, the dispersion medium b) comprises an organosilicon that is different from the polysiloxane a).

[0101] Particularly preferred is that the dispersion medium b) is a crosslinkable organosilicon.

[0102] The solid particles in the composition preferably include at least one of fillers and pigments, as described above.

[0103] In a preferred embodiment of the composition, the amount of component a) is 0.010 to 10.000 by weight based on the total weight of the composition.

[0104] In this composition, there is no limitation on the content of polysiloxane a). The content should be sufficient to treat the filler with polysiloxane a) to improve its dispersibility in the resulting thermally conductive silicone composition; specifically, the content is preferably 0.001 to 10.000 parts by weight per 100 parts by weight of filler, and particularly preferably 0.001 to 5 parts by weight per 100 parts by weight of filler. This is because when the content of polysiloxane a) is less than the lower limit of the above range, the addition of a large amount of filler leads to a decrease in the moldability of the resulting silicone composition, and causes the filler to precipitate and separate during storage of the resulting silicone composition, resulting in a significant decrease in consistency. On the other hand, when the content exceeds the upper limit of the above range, the physical properties of the resulting silicone composition tend to deteriorate.

[0105] In some embodiments, the composition is used as a paint or coating composition, as a molding composition, or as a paste or potting material, gasket, solder paste, underfill, thermal interface material, such as thermal gap filler, thermal gap pad, silicone pad, phase change material, thermal grease, thermal gel, thermal coating material, thermal encapsulant, adhesive, or sealant material.

[0106] If desired, the composition may contain other components, such as binders or polymeric resins, reactive or non-reactive diluents, solvents, and conventional auxiliary additives. Examples of such additives include adhesion promoters, such as 3-glycidoxypropyltrimethoxysilane or 3-methacryloyloxypropyltrimethoxysilane, defoamers, heat stabilizers or UV stabilizers, rheology modifiers, and flow and leveling additives, crosslinking agents, chain extenders, reinforcing fillers, non-reinforcing fillers, plasticizers, flame retardants and heat-resistant agents, such as triazole compounds, dehydrating agents, biocides, curing accelerators, (fluorescent) dyes, inhibitors, antistatic agents, waxes, catalysts, and additives well known to those skilled in the art.

[0107] The present invention also relates to a method for dispersing solid filler particles in a non-aqueous composition, the method comprising:

[0108] a) Providing a polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group or a hydrolysis product thereof covalently linked to the polysiloxane.

[0109] b) Provide solid filler particles, and

[0110] c) Incorporate the components provided in steps a) and b) into a non-aqueous composition containing a dispersion medium to form a dispersion base, and

[0111] d) subject the dispersion base material to shear force,

[0112] The content of the filler particles is 500 to 2500 parts by weight per 100 parts by weight of dispersion medium. Example

[0113] Contrast dispersants

[0114] Synthesis of ethoxy / amine adduct copolymers containing polysiloxane groups:

[0115] A monoamino-functionalized polysiloxane (376.3 g) and 1,6-hexanediol diglycidyl ether (22.8 g) as described in Example 1 of US9217083B2 were added to a four-necked flask equipped with a stirrer, thermometer, dropping funnel, reflux condenser, and nitrogen inlet, and the mixture was heated to 140 °C under nitrogen. The conversion of the epoxide was monitored by 1H NMR. After complete conversion of the epoxide groups, the reaction mixture was cooled to room temperature. GPC data: Mn = 5500 g / mol, and PDI = 2.0.

[0116] Preparation of Si-H functional intermediates

[0117] Butyl-D, a SiH-functional organosilicon macromonomer, was synthesized according to the method described in Example 1 of US8304077B2. 25 M H Mw 2000. Butyl-D was synthesized by adjusting the ratio between butyllithium and hexamethylcyclotrisiloxane monomer. 38, 5M H and butyl-D 65,5 M H .

[0118] Dispersant 1

[0119] Butyl-D 25 M H Reaction with 30% molar excess allyl succinic anhydride

[0120] Add 181.15 g of butyl-D to a flask equipped with a stirrer, thermometer, reflux condenser and nitrogen inlet. 25 M H The mixture was heated to 75°C. Then, 0.60 g of a 0.6% H₂PtCl₆ solution in xylene was added. Subsequently, 18.85 g of allyl succinic anhydride was added via a dropping funnel. The reaction mixture was maintained at 100°C for 3 hours. After this time, the conversion rate of the SiH groups was found to be above 98%. Volatile substances were removed by rotary evaporation at 130°C and 15 mbar.

[0121] GPC data of the obtained product: Mn 1759 g / mol, Mw 2232 g / mol, DPI 1.27.

[0122] Dispersant 2

[0123] Butyl-D 65,5 M H Reaction with 30% molar excess allyl succinic anhydride

[0124] Add 143.91 g of butyl-D to a flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet. 65.5 M H The mixture was heated to 75°C. Then, 0.53 g of a 0.6% H₂PtCl₆ solution in xylene was added. Subsequently, 6.09 g of allyl succinic anhydride was added via a dropping funnel. The reaction mixture was maintained at 100°C for 3 hours. After this time, the conversion rate of the SiH groups was found to be above 98%. Volatile substances were removed by rotary evaporation at 130°C and 15 mbar.

[0125] GPC data of the obtained product: Mn 5630 g / mol, Mw 9153 g / mol, DPI 1.62.

[0126] Dispersant 3

[0127] Butyl-D 38,5 M H Reaction with 30% molar excess allyl succinic anhydride

[0128] Add 140.98 g of butyl-D to a flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet. 38.5 M H The mixture was heated to 75°C. Then, 0.53 g of a 0.6% solution of H₂PtCl₆ in xylene was added. Subsequently, 9.02 g of allyl succinic anhydride was added via a dropping funnel. The reaction mixture was kept at 100°C for 3 hours. After this time, the conversion rate of SiH groups was found to be above 98%. Volatile substances were removed by rotary evaporation at 130°C and 15 mbar.

[0129] GPC data of the obtained product: Mn 2745 g / mol, Mw 3399 g / mol, DPI 1.21.

[0130] Dispersant 4

[0131] Step 1:

[0132] Preparation of MD with an average of 1 SiH group 38,5 M H siloxane

[0133] Add 9.46 g of HMDSO (hexamethyldisiloxane), 302.93 g of D5, and 37.61 g of M to a flask equipped with a stirrer, thermometer, and reflux condenser. H 2D6. The mixture was heated to 75°C. At this temperature, 3.5 g of catalyst K20 (calcium montmorillonite treated with hydrochloric acid) from Clariant was added to the mixture. The mixture was stirred at 80°C for 3 hours, then cooled to 50°C and stirred again at this temperature for 3 hours. 1.75 g of Harbolite 900 (amorphous alumina silicate) filter aid was added, the mixture was stirred, and filtered through a pressure filter. The content of SiH groups was determined by iodine value and found to be 8.14.

[0134] Step 2

[0135] The reaction of siloxane from step 1 with allyl succinic anhydride

[0136] In a flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet, 141.72 g of the siloxane from step 1 was added, and the mixture was heated to 75 °C. Then, 0.53 g of a 0.6% solution of H₂PtCl₆ in xylene was added. Subsequently, 8.28 g of allyl succinic anhydride was added via a dropping funnel. The reaction mixture was maintained at 100 °C for 3 hours. After this time, the conversion of SiH groups was found to be above 98%. Volatile substances were removed by rotary evaporation at 130 °C and 15 mbar.

[0137] GPC data of the obtained product: Mn 1813 g / mol, Mw 5272 g / mol, DPI 2.91.

[0138] Dispersant 5

[0139] Step 1

[0140] Preparation of MD with an average of 1 SiH group 65,5 M H siloxane

[0141] Add 5.68 g of HMDSO, 321.76 g of D5, and 22.57 g of M to a flask equipped with a stirrer, thermometer, and reflux condenser. H 2D6. The mixture was heated to 75°C. At this temperature, 3.5 g of catalyst K20 was added to the mixture. The mixture was stirred at 80°C for 3 hours, then cooled to 50°C and stirred again at this temperature for 3 hours. 1.75 g of Harbolite 900 filter aid was added, the mixture was stirred, and filtered through a pressure filter. The SiH group content was determined by measuring the iodine value, which was found to be 4.81.

[0142] Step 2

[0143] The reaction of siloxane from step 1 with allyl succinic anhydride

[0144] In a flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet, 144.99 g of the siloxane from step 1 was added, and the mixture was heated to 75 °C. Then, 0.53 g of a 0.6% solution of H₂PtCl₆ in xylene was added. Subsequently, 5.01 g of allyl succinic anhydride was added via a dropping funnel. The reaction mixture was maintained at 100 °C for 3 hours. After this time, the conversion of SiH groups was found to be above 98%. Volatile substances were removed by rotary evaporation at 130 °C and 15 mbar.

[0145] GPC data of the obtained product: Mn 2094 g / mol, Mw 8247 g / mol, DPI 3.94.

[0146] Dispersant 6

[0147] Step 1

[0148] Preparation of MD with an average of 1 SiH group 86 M H siloxane

[0149] Add 4.35 g HMDSO, 328.31 g D5, and 17.33 g M to a flask equipped with a stirrer, thermometer, and reflux condenser. H 2D6. The mixture was heated to 75°C. At this temperature, 3.5 g of catalyst K20 was added to the mixture. The mixture was stirred at 80°C for 3 hours, then cooled to 50°C and stirred again at this temperature for 3 hours. 1.75 g of Harbolite 900 filter aid was added, the mixture was stirred, and filtered through a pressure filter. The content of SiH groups was determined by measuring the iodine value, which was found to be 3.48.

[0150] Step 2

[0151] The reaction of siloxane from step 1 with allyl succinic anhydride

[0152] In a flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet, 146.34 g of the siloxane from step 1 was added, and the mixture was heated to 75 °C. Then, 0.53 g of a 0.6% solution of H₂PtCl₆ in xylene was added. Subsequently, 3.66 g of allyl succinic anhydride was added via a dropping funnel. The reaction mixture was maintained at 100 °C for 3 hours. After this time, the conversion of SiH groups was found to be above 98%. Volatile substances were removed by rotary evaporation at 130 °C and 15 mbar.

[0153] GPC data of the obtained product: Mn 2240 g / mol, Mw 11034 g / mol, DPI 4.93.

[0154] Dispersant 7

[0155] Step 1

[0156] Preparation of MD with an average of 1 SiH group 106 M H siloxane

[0157] Add 3.55 g HMDSO, 332.33 g D5, and 14.12 g M to a flask equipped with a stirrer, thermometer, and reflux condenser. H 2D6. The mixture was heated to 75°C. At this temperature, 3.15 g of catalyst K20 was added to the mixture. The mixture was stirred at 80°C for 3 hours, then cooled to 50°C and stirred again at this temperature for 3 hours. 1.75 g of Harbolite 900 filter aid was added, the mixture was stirred, and filtered through a pressure filter. The content of SiH groups was determined by measuring the iodine value, which was found to be 2.95.

[0158] Step 2

[0159] The reaction of siloxane from step 1 with allyl succinic anhydride

[0160] In a flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet, 146.89 g of the siloxane from step 1 was added, and the mixture was heated to 75 °C. Then, 0.53 g of a 0.6% solution of H₂PtCl₆ in xylene was added. Subsequently, 3.11 g of allyl succinic anhydride was added via a dropping funnel. The reaction mixture was maintained at 100 °C for 3 hours. After this time, the conversion of SiH groups was found to be above 98%. Volatile substances were removed by rotary evaporation at 130 °C and 15 mbar.

[0161] GPC data of the obtained product: Mn 2255 g / mol, Mw 13177 g / mol, DPI 5.37.

[0162] Dispersant 8

[0163] Step 1

[0164] Preparation of MD with an average of 1 SiH group 133 M H siloxane

[0165] Add 2.84 g of HMDSO, 335.86 g of D5, and 11.30 g of M to a flask equipped with a stirrer, thermometer, and reflux condenser. H 2D6. The mixture was heated to 75°C. At this temperature, 3.15 g of catalyst K20 was added to the mixture. The mixture was stirred at 80°C for 3 hours, then cooled to 50°C and stirred again at this temperature for 3 hours. 1.75 g of Harbolite 900 filter aid was added, the mixture was stirred, and filtered through a pressure filter. The SiH group content was determined by measuring the iodine value, which was found to be 2.54.

[0166] Step 2

[0167] The reaction of siloxane from step 1 with allyl succinic anhydride

[0168] 147.31 g of the siloxane from step 1 was added to a flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet, and heated to 75 °C. Then, 0.53 g of a 0.6% solution of H₂PtCl₆ in xylene was added. Subsequently, 2.69 g of allyl succinic anhydride was added via a dropping funnel. The reaction mixture was maintained at 100 °C for 3 hours. After this time, the conversion of SiH groups was found to be above 98%. Volatile substances were removed by rotary evaporation at 130 °C and 15 mbar.

[0169] GPC data of the obtained product: Mn 2717 g / mol, Mw 16878 g / mol, DPI 6.21.

[0170] Dispersant 9

[0171] Hydrolyze dispersant 5 with deionized water:

[0172] In a flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet, 248.29 g of the above-mentioned dispersant 5 and 1.7 g of deionized water were added. The mixture was stirred and heated at 70 °C for 10 hours. After this time, 89 mol% of the cyclic carboxylic anhydride groups were found to have been hydrolyzed into dicarboxylic acid groups. The volatiles were removed by rotary evaporation at 130 °C and 15 mbar.

[0173] Dispersant 10

[0174] Salt formation of dispersant 9

[0175] In a glass beaker, 116.19 g of dispersant 9 was mixed with 3.81 g of N,N-dibutylethanolamine.

[0176] The application of dispersants in addition-curing RTV silicone formulations is described below.

[0177] To prepare addition-curing RTV silicone compositions, a dual asymmetric centrifugal mixer, namely the Speedmixer DAC 400.1FVZ, Hauschild GmbH & Co. KG, was used.

[0178] raw material:

[0179] • Addition-curing, RTV-2 silicone rubber part A (SilGel 612A, Wacker) - vinyl polydimethylsiloxane and additives

[0180] • Addition-curing, RTV-2 silicone rubber part B (SilGel 612B, Wacker), SiH-functionalized polydimethylsiloxane and polydimethylsiloxane with functional groups, and additives containing platinum catalyst.

[0181] Adhesion promoter - methacryloyloxypropyltrimethoxysilane

[0182] • Filler 1 - Alumina - Average particle size 1.4 μm

[0183] • Filler 2 - Alumina - Average particle size 45.0 μm

[0184] • Filler 3 - Alumina - Average particle size 0.2mm

[0185] To investigate the curing behavior of the silicone composition and the effect of the dispersant on application performance, the formulation was evaluated in an unfilled system. Parts A and B were prepared separately in a PE speed mixer cup by metering in all the corresponding raw materials of either part A or part B and homogenizing at 2,500 rpm for 30 seconds. Parts A and B were then mixed at a 1.5:1 ratio (A:B) using a speed mixer at 2,000 rpm for 30 seconds and stored in an oven at 100°C until the formulation was cured. The formulation was observed at 60-second intervals to evaluate the curing stage. Skin formation time was defined as the time when the first skin layer formed on the surface. Curing time was defined as the time when the formulation was completely cured and its hardness and viscosity no longer changed further.

[0186]

[0187] Results of using unfilled silicone compositions:

[0188] Cortical formation time [minutes] Curing time [minutes] Reference 3 5 Contrast dispersants No cortex Not cured Dispersant 1 5 15 Dispersant 3 8 25 Dispersant 2 3 12 Dispersant 4 3 12 Dispersant 5 3 12 Dispersant 6 8 15 Dispersant 7 8 15 Dispersant 8 4 10

[0189] The table above leads to the conclusion that the dispersant completely prevents the curing of silicone rubber. The dispersant according to the present invention has only a weak effect on curing properties, which can be adjusted by the amount of curing catalyst used.

[0190] To evaluate the effect of dispersants on the viscosity of highly filled silicone compositions, an addition-curing RTV-2 composition filled with alumina was formulated.

[0191] Part A of the RTV-2 composition was prepared in a PE speed mixer cup by metering in the silicone gel, adhesion promoter, and dispersant, and homogenizing it at 2,500 rpm for 30 seconds using a speed mixer. Then, Al2O3 filler was added in a single metering step and homogenized at 2,500 rpm for 30 seconds.

[0192] The viscosity of the prepared fraction A was measured using an AntonPaar MCR 201 rheometer under the following conditions: PP 25, shear rate 0.1-100 s⁻¹. -1 1.0mm gap, 23℃, sample trimming. Particular attention was paid to observation at 1 second. -1 and 10s -1 The viscosity is described below, thus illustrating the viscosity of the filled and modified composition.

[0193] Part B of the RTV-2 composition was prepared in a PE speed mixer cup by metering in the silicone gel and dispersant and homogenizing it at 2,500 rpm for 30 seconds using a speed mixer. Then, Al2O3 filler was added in a single metering step and homogenized at 2,500 rpm for 30 seconds.

[0194] Mix portions A and B at 2,000 rpm for 30 seconds using a speed mixer, and store in an oven at 100°C until the formulation is cured. Observe the formulation at 60-second intervals to evaluate the curing stage, similar to the unfilled system.

[0195]

[0196] Results of the application of the filled silicone composition:

[0197]

[0198] The table above shows that, compared to comparative dispersants, the dispersant of the present invention has a significantly stronger effect on reducing the viscosity of highly filled silicone compositions. Unlike comparative dispersants, the dispersant of the present invention does not prevent curing.

[0199] One of the main applications of silicone compositions filled with thermally conductive fillers is as thermal interface materials (TIMs), applied to copper substrates. For this application, the corrosion characteristics of the dispersant were evaluated on the corresponding substrate. Pure dispersant was dropped onto copper, covered with a cotton pad, and stored in a climate chamber at 55°C and 80% relative humidity for 14 days. In a second experiment, unfilled silicone compositions containing the dispersant were applied to copper with a spatula, covered with a cotton pad, and stored in a climate chamber at 55°C and 80% relative humidity for 14 days. The corrosion condition of the copper substrate was visually evaluated and rated on a scale of 1 to 6.

[0200]

[0201] The table above shows that, on copper substrates, the dispersant of the present invention results in less corrosion compared to the comparative dispersants.

[0202] The effect of dispersants on viscosity reduction when using different types of fillers was evaluated by altering fraction A of the formulation using calcium carbonate, boron nitride, aluminum hydroxide, and dispersing additives. The viscosity of fraction A was measured using an AntonPaar MCR 201 rheometer under the following conditions: PP 25, shear rate 0.1–100 s⁻¹. -1 1.0mm gap, 23℃, sample trimming. Recorded in 1 second. -1 The viscosity at that point.

[0203] filler:

[0204] Calcium carbonate (CaCO3) has an average particle size of 5 μm.

[0205] The average particle size of aluminum hydroxide (Al(OH)3) is 12 μm.

[0206] The average particle size of boron nitride (BN) is 16 μm.

[0207] Preparation of calcium carbonate:

[0208]

[0209] Preparation of aluminum hydroxide:

[0210]

[0211] Preparation of boron nitride:

[0212]

[0213] The effects of dispersants and the dispersing additives of the present invention on the reduction of viscosity of the composition are shown in the table below:

[0214] Reference Dispersant 5 <![CDATA[CaCO3]]> <![CDATA[Viscosity at 1 s -1 [Pa·s]]]> 987 123 <![CDATA[Al(OH)3]]> <![CDATA[Viscosity at 1s -1 [Pa·s]]]> 2448 481 BN <![CDATA[Viscosity at 1 s -1 [Pa·s]]]> 1722 1316

[0215] The table above shows that dispersant 5 significantly reduced the viscosity of addition-cured RTV-2 compositions containing different fillers.

Claims

1. Use of a polysiloxane as a dispersant for solid filler particles in a non-aqueous composition containing a dispersion medium, said polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group covalently linked to said polysiloxane, wherein the filler particles are present in an amount of 500 to 2500 parts by weight per 100 parts by weight of dispersion medium, said dispersion medium being different from said polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group. The cyclic carboxylic anhydride groups form a 5-membered ring.

2. The use according to claim 1, wherein the cyclic carboxylic anhydride group is linked to the polysiloxane via a Si-C bond.

3. The use according to claim 1 or 2, wherein an average of 0.7 to 3.0 cyclic carboxylic anhydride groups are covalently linked to the polysiloxane molecule.

4. The use according to claim 1, wherein the dispersion medium comprises organosilicon.

5. The use according to claim 1 or 2, wherein the non-aqueous composition is used as a thermal interface material.

6. The use according to claim 5, wherein the non-aqueous composition is used as a thermal interface material in electronic components.

7. A non-aqueous composition comprising: a) A polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group covalently linked to the polysiloxane. b) Dispersion medium, and c) Solid filler particles, The filler particles are present in an amount of 500 to 2500 parts by weight per 100 parts by weight of dispersion medium, wherein the dispersion medium is different from the polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group.

8. The composition according to claim 7, wherein the dispersion medium b) comprises an organosilicon different from that of polysiloxane a).

9. The composition according to claim 8, wherein the organosilicon is a crosslinkable organosilicon.

10. The composition according to claim 7 or 8, wherein the average particle size of the solid filler particles is from 0.1 to 500.0 μm.

11. The composition according to claim 7 or 8, wherein the solid filler particles comprise alumina particles.

12. The composition of claim 11, wherein the alumina particles comprise at least one of spherical alumina particles with an average particle size of 1.0 to 50.0 μm and alumina particles with an irregular shape having an average particle size of 0.1 to 50.0 μm.

13. The composition according to claim 7 or 8, wherein component a) has a number-average molecular weight Mn of 500 to 10000 g / mol.

14. The composition according to claim 7 or 8, wherein the amount of component a) is 0.010 to 10.000 by weight based on the total weight of the composition.

15. A method for dispersing solid filler particles in a non-aqueous composition, the method comprising: a) Provides a polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group covalently linked to the polysiloxane. b) Provide solid filler particles, and c) Incorporate the components provided in steps a) and b) into a non-aqueous composition containing a dispersion medium to form a dispersion base, and d) subject the dispersion base to shear force. The filler particles are present in an amount of 500 to 2500 parts by weight per 100 parts by weight of dispersion medium, wherein the dispersion medium is different from the polysiloxane having a plurality of siloxane groups and at least one cyclic carboxylic anhydride group.

Citation Information

Patent Citations

  • Dehydrogenative condensation of alcohol with organo-hydrogen-siloxane in presence of quat. ammonium hydroxide catalyst, used to make modified polyorgano-siloxane for use e.g. as emulsifier or in release coatings

    DE102005051939A1

  • Method for making silylnorbornane anhydrides

    EP0112845B1

  • A powder composition and a cosmetic composition containing said powder composition

    EP0931537B1

  • Organopolysiloxane having carboxyl groups

    EP2107078A1

  • Thiol modified silicone compound, dispersant, silicone treated zirconia, zirconia-silicone oil dispersant, cured article, and silicone LED encapsulation material