A carbide ceramic composite coating and preparation method thereof

By optimizing the ratio of the carbide ceramic composite coating and laser deposition technology, the problem of poor bonding force between the carbide coating and the substrate was solved, and a carbide ceramic composite coating with high density, wear resistance and corrosion resistance was achieved. layer, suitable for the protection of steel materials, reducing preparation costs.

CN116891646BActive Publication Date: 2024-10-25SHANDONG AGRI & ENG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310852168.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-12
Publication Date
2024-10-25
Estimated Expiration
2043-07-12

AI Technical Summary

Technical Problem

The existing carbide coating has poor bonding force with the substrate, causing the coating to be easily damaged in highly reactive or corrosive environments, and cannot meet the protection needs of steel materials.

Method used

Using an optimized ratio of carbides, inert fillers, alkaline compounds, composite additives and binders, the carbide ceramic composite coating is prepared through laser deposition technology to improve its density, bonding strength and corrosion resistance.

Benefits of technology

It significantly improves the bonding strength, hardness and wear resistance of the carbide ceramic composite coating, extends the service life of the steel material, and reduces the preparation cost, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004334624380000071
    Figure BDA0004334624380000071
Patent Text Reader

Abstract

The present invention belongs to the technical field of carbide coatings. The present invention provides a carbide ceramic composite coating and a preparation method thereof. The carbide ceramic composite coating comprises the following components in parts by weight: 10 to 20 parts of carbide, 2 to 6 parts of inert filler, 0.5 to 1 part of alkaline compound, 1.5 to 3 parts of composite additive material, 0.2 to 0.4 parts of binder, and 8 to 15 parts of solvent. The carbide ceramic composite coating prepared by the present invention is firmly bonded to the metal substrate, the coating structure is dense, the hardness is large, the wear resistance and corrosion resistance are good, the bonding force of the composite coating can reach 74MPa, the hardness can reach 1950HV, no rust spots appear in the salt spray test for 72 hours, and the wear amount of the composite coating is 0.09 to 0.13mg when the sphere diameter is 6mm, the load is 10N, the rotation rate is 200r / min, and the wear time is 1800s; and the preparation process is simple, the cost is low, and it is suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbide coatings, and in particular to a carbide ceramic composite coating and a preparation method thereof. Background Art

[0002] Steel components that are exposed to highly reactive or corrosive environments for a long time are very susceptible to corrosion damage due to oxidation. However, the cost of maintaining and replacing these materials is high, resulting in a serious waste of resources. Coatings can effectively protect steel from oxidation corrosion. Carbides have the characteristics of high stability, high hardness, and excellent wear resistance. Therefore, carbide coatings can be used to protect steel materials and extend the service life of steel materials.

[0003] The preparation methods of carbide coating mainly include electroplating, chemical plating, thermal spraying, and vapor deposition. However, due to the problems of complex procedures, large thermal stress, and high production conditions, the obtained carbide coating has poor bonding with the substrate, and cracks are easily generated at the interface between the coating and the substrate, which cannot meet the actual production needs. Therefore, the research and development of a carbide ceramic composite coating with good density, wear resistance, corrosion resistance, and bonding and its preparation method have good application prospects. Summary of the invention

[0004] The object of the present invention is to provide a carbide ceramic composite coating and a preparation method thereof in view of the deficiencies in the prior art.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a carbide ceramic composite coating, comprising the following components in parts by weight:

[0007] 10 to 20 parts of carbide, 2 to 6 parts of inert filler, 0.5 to 1 part of alkaline compound, 1.5 to 3 parts of composite additive, 0.2 to 0.4 parts of binder, and 8 to 15 parts of solvent.

[0008] Preferably, the carbide is one or more of tungsten carbide, titanium carbide and chromium carbide, and the particle size of the carbide is 15-20 μm.

[0009] Preferably, the inert filler is one or more of alumina, zirconium dioxide and titanium dioxide; and the alkaline compound is sodium silicate, sodium carbonate or calcium oxide.

[0010] Preferably, the composite additive material is ferrous oxide and cuprous oxide, and the mass ratio of ferrous oxide to cuprous oxide is 1:2-3.

[0011] Preferably, the binder is an aqueous phosphoric acid solution or an acid phosphate; and the solvent is tetrahydrofuran, toluene or carbon tetrachloride.

[0012] The present invention also provides a method for preparing the carbide ceramic composite coating, comprising the following steps:

[0013] 1) mixing the carbide and part of the solvent to obtain a mixture I;

[0014] 2) mixing the inert filler, the composite additive material and the remaining solvent to obtain a mixture II;

[0015] 3) mixing mixture I, mixture II, a basic compound and a binder to obtain a mixed powder;

[0016] 4) The mixed powder is laser-clad onto the surface of the substrate by coaxial powder feeding to obtain a carbide ceramic composite coating.

[0017] Preferably, the mixing speed in steps 1) to 3) is independently 150 to 200 r / min, the mixing temperature is independently 20 to 30° C., and the mixing time is independently 30 to 40 min.

[0018] Preferably, the mass ratio of the partial solvent in step 1) to the remaining solvent in step 2) is 1:1-2.

[0019] Preferably, the power of the laser cladding in step 4) is 3-5 kW, and the scanning speed is 50-80 mm / s.

[0020] The beneficial effects of the present invention include the following:

[0021] 1) The carbide ceramic composite coating prepared by the present invention is firmly bonded to the metal substrate, the coating structure is dense, the hardness is high, the wear resistance and corrosion resistance are good, the bonding force of the composite coating can reach 74MPa, the hardness can reach 1950HV, no rust spots appear in the salt spray test for 72 hours, and the wear loss of the composite coating is 0.09-0.13mg under the conditions of a sphere diameter of 6mm, a load of 10N, a rotation rate of 200r / min, and a wear time of 1800s.

[0022] 2) The present invention significantly improves the density, bonding, wear resistance and corrosion resistance of the carbide ceramic composite coating by optimizing the types and dosage ratios of carbides, inert fillers, alkaline compounds, composite additives, binders and solvents.

[0023] 3) When the present invention adopts laser cladding to prepare the carbide ceramic composite coating, the mixed powder and the thin layer on the surface of the substrate are melted at the same time and solidified rapidly to form a surface coating with extremely low dilution and metallurgically bonded to the substrate, thereby significantly improving the wear resistance and corrosion resistance of the coating surface.

[0024] 4) The carbide ceramic composite coating of the present invention has a simple preparation process, low cost and is suitable for industrial application. DETAILED DESCRIPTION

[0025] The present invention provides a carbide ceramic composite coating, comprising the following components in parts by weight:

[0026] 10 to 20 parts of carbide, 2 to 6 parts of inert filler, 0.5 to 1 part of alkaline compound, 1.5 to 3 parts of composite additive, 0.2 to 0.4 parts of binder, and 8 to 15 parts of solvent.

[0027] The carbide ceramic composite coating of the present invention contains 10 to 20 parts of carbide, preferably 12 to 18 parts, more preferably 14 to 16 parts, and even more preferably 15 parts.

[0028] In the present invention, the carbide is preferably one or more of tungsten carbide, titanium carbide and chromium carbide; the particle size of the carbide is preferably 15 to 20 μm, more preferably 16 to 18 μm, and more preferably 17 μm.

[0029] The carbide ceramic composite coating of the present invention contains 2 to 6 parts of inert filler, preferably 3 to 5 parts, more preferably 3.5 to 4.5 parts, and more preferably 4 parts.

[0030] In the present invention, the inert filler is preferably one or more of alumina, zirconium dioxide and titanium dioxide.

[0031] In the present invention, the inert filler can effectively inhibit the volume shrinkage generated during the preparation of the carbide ceramic composite coating, thereby improving the density of the carbide ceramic composite coating and its bonding with the substrate.

[0032] The carbide ceramic composite coating of the present invention contains 0.5 to 1 part of the basic compound, preferably 0.6 to 0.9 part, more preferably 0.7 to 0.8 part, and more preferably 0.75 part.

[0033] In the present invention, the alkaline compound is preferably sodium silicate, sodium carbonate or calcium oxide.

[0034] In the present invention, the alkaline compound can fill the cracks and pores generated in the preparation process of the carbide ceramic composite coating, thereby improving the density of the coating, and at the same time can effectively improve the corrosion resistance of the coating.

[0035] The carbide ceramic composite coating of the present invention contains 1.5 to 3 parts of composite additives, preferably 1.8 to 2.6 parts, more preferably 2 to 2.4 parts, and even more preferably 2.2 parts.

[0036] In the present invention, the composite additive material is preferably ferrous oxide and cuprous oxide; the mass ratio of ferrous oxide to cuprous oxide is preferably 1:2-3, more preferably 1:2.2-2.8, and more preferably 1:2.4-2.6.

[0037] In the present invention, the composite additive material can improve the compactness of the carbide ceramic composite coating and the bonding strength between the carbide ceramic composite coating and the substrate.

[0038] The carbide ceramic composite coating of the present invention contains 0.2 to 0.4 parts of a binder, preferably 0.25 to 0.35 parts, more preferably 0.28 to 0.32 parts, and even more preferably 0.3 parts.

[0039] In the present invention, the binder is preferably a phosphoric acid aqueous solution or an acid phosphate; the mass fraction of the phosphoric acid aqueous solution is preferably 30-50%, more preferably 35-45%, and more preferably 40%; the acid phosphate is preferably sodium dihydrogen phosphate or aluminum dihydrogen phosphate.

[0040] The carbide ceramic composite coating of the present invention contains 8 to 15 parts of solvent, preferably 9 to 14 parts, more preferably 10 to 12 parts, and even more preferably 11 parts.

[0041] In the present invention, the solvent is preferably tetrahydrofuran, toluene or carbon tetrachloride.

[0042] The present invention also provides a method for preparing the carbide ceramic composite coating, comprising the following steps:

[0043] 1) mixing the carbide and part of the solvent to obtain a mixture I;

[0044] 2) mixing the inert filler, the composite additive material and the remaining solvent to obtain a mixture II;

[0045] 3) mixing mixture I, mixture II, a basic compound and a binder to obtain a mixed powder;

[0046] 4) The mixed powder is laser-clad onto the surface of the substrate by coaxial powder feeding to obtain a carbide ceramic composite coating.

[0047] In the present invention, the mixing speed of steps 1) to 3) is independently preferably 150 to 200 r / min, more preferably 160 to 180 r / min, and more preferably 170 r / min; the mixing temperature is independently preferably 20 to 30°C, more preferably 24 to 26°C, and more preferably 25°C; the mixing time is independently preferably 30 to 40 min, more preferably 32 to 38 min, and more preferably 34 to 36 min.

[0048] In the present invention, the mass ratio of the partial solvent in step 1) to the remaining solvent in step 2) is preferably 1:1-2, more preferably 1:1.2-1.8, and more preferably 1:1.4-1.6.

[0049] In the present invention, the power of the laser cladding in step 4) is preferably 3-5 kW, more preferably 3.5-4.5 kW, and more preferably 4 kW; the scanning speed is preferably 50-80 mm / s, more preferably 60-70 mm / s, and more preferably 65 mm / s.

[0050] In the present invention, the substrate in step 4) is preferably a pretreated substrate, and the pretreatment process is preferably to wash and dry the substrate in sequence; the washing agent is preferably acetone or anhydrous ethanol, and the washing is performed until the oil stains on the surface of the substrate are completely removed; the drying temperature is preferably 60-100°C, more preferably 70-80°C, more preferably 75°C, and the drying time is preferably 1-2h, more preferably 1.2-1.6h, more preferably 1.5h.

[0051] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0052] The substrates described in the following examples and comparative examples are all pretreated Q235 steel, and the pretreatment process is: after removing the oil stains on the surface of the substrate with anhydrous ethanol, the substrate is dried in an insulated box at a temperature of 80° C. for 2 hours.

[0053] Example 1

[0054] 15g of tungsten carbide with a particle size of 18μm and 5g of tetrahydrofuran were mixed at a speed of 180r / min and a temperature of 25°C for 35min to obtain a mixture I; 4g of aluminum oxide, 1g of ferrous oxide, 2g of cuprous oxide and 5g of tetrahydrofuran were mixed at a speed of 150r / min and a temperature of 20°C for 40min to obtain a mixture II; mixture I, mixture II, 0.7g of sodium silicate and 0.3g of a 40% by mass phosphoric acid aqueous solution were mixed at a speed of 200r / min and a temperature of 30°C for 35min to obtain a mixed powder.

[0055] The mixed powder was laser-clad onto the surface of the substrate by coaxial powder feeding using a semiconductor laser. The power of the laser cladding was 4 kW and the scanning speed was 70 mm / s to obtain a carbide ceramic composite coating.

[0056] The carbide ceramic composite coating prepared in this embodiment has a bonding force of 72 MPa and a hardness of 1900 HV.

[0057] Example 2

[0058] 10g of titanium carbide with a particle size of 15μm and 3.2g of toluene were mixed at a speed of 150r / min and a temperature of 20°C for 30min to obtain a mixture I; 2g ​​of zirconium dioxide, 0.5g of ferrous oxide, 1.5g of cuprous oxide and 4.8g of toluene were mixed at a speed of 160r / min and a temperature of 25°C for 30min to obtain a mixture II; mixture I, mixture II, 0.5g of sodium carbonate and 0.2g of sodium dihydrogen phosphate were mixed at a speed of 150r / min and a temperature of 20°C for 30min to obtain a mixed powder.

[0059] The mixed powder was laser-clad onto the surface of the substrate by coaxial powder feeding using a semiconductor laser. The power of the laser cladding was 3 kW and the scanning speed was 50 mm / s to obtain a carbide ceramic composite coating.

[0060] The carbide ceramic composite coating prepared in this embodiment has a bonding force of 74 MPa and a hardness of 1950 HV.

[0061] Example 3

[0062] 20 g of chromium carbide with a particle size of 20 μm and 5 g of carbon tetrachloride were mixed at a speed of 200 r / min and a temperature of 30°C for 40 min to obtain a mixture I; 6 g of titanium dioxide, 0.5 g of ferrous oxide, 1 g of cuprous oxide and 10 g of carbon tetrachloride were mixed at a speed of 200 r / min and a temperature of 30°C for 35 min to obtain a mixture II; mixture I, mixture II, 1 g of calcium oxide and 0.4 g of aluminum dihydrogen phosphate were mixed at a speed of 160 r / min and a temperature of 25°C for 40 min to obtain a mixed powder.

[0063] The mixed powder was laser-clad onto the surface of the substrate by coaxial powder feeding using a semiconductor laser. The power of the laser cladding was 5 kW and the scanning speed was 80 mm / s to obtain a carbide ceramic composite coating.

[0064] The carbide ceramic composite coating prepared in this embodiment has a bonding force of 70 MPa and a hardness of 1800 HV.

[0065] Example 4

[0066] 16 g of titanium carbide with a particle size of 15 μm and 5 g of tetrahydrofuran were mixed at a speed of 200 r / min and a temperature of 25°C for 30 minutes to obtain a mixture I; 4 g of titanium dioxide, 2 g of aluminum oxide, 0.5 g of ferrous oxide, 1 g of cuprous oxide and 10 g of tetrahydrofuran were mixed at a speed of 200 r / min and a temperature of 30°C for 30 minutes to obtain a mixture II; mixture I, mixture II, 0.6 g of calcium oxide and 0.35 g of a 50% by mass phosphoric acid aqueous solution were mixed at a speed of 160 r / min and a temperature of 25°C for 35 minutes to obtain a mixed powder.

[0067] The mixed powder was laser-clad onto the surface of the substrate by coaxial powder feeding using a semiconductor laser. The power of the laser cladding was 4.5 kW and the scanning speed was 65 mm / s to obtain a carbide ceramic composite coating.

[0068] The carbide ceramic composite coating prepared in this embodiment has a bonding force of 68 MPa and a hardness of 1850 HV.

[0069] Comparative Example 1

[0070] The aluminum oxide in Example 1 was omitted, the amount of sodium silicate was changed to 0.1 g, and other conditions were the same as in Example 1 to obtain a carbide ceramic composite coating.

[0071] The carbide ceramic composite coating prepared in this comparative example has a bonding force of 42 MPa and a hardness of 1100 HV.

[0072] Comparative Example 2

[0073] The ferrous oxide and cuprous oxide in Example 1 were omitted, the amount of the phosphoric acid aqueous solution was changed to 0.7 g, the power of the laser cladding was changed to 8 kW, and the other conditions were the same as in Example 1, to obtain a carbide ceramic composite coating.

[0074] The carbide ceramic composite coating prepared in this comparative example has a bonding force of 38 MPa and a hardness of 1200 HV.

[0075] Comparative Example 3

[0076] The scanning speed of Example 1 was modified to 30 mm / s, ferrous oxide was omitted, the power of laser cladding was modified to 2 kW, and other conditions were the same as those of Example 1 to obtain a carbide ceramic composite coating.

[0077] The carbide ceramic composite coating prepared in this comparative example has a bonding force of 40 MPa and a hardness of 1000 HV.

[0078] The carbide ceramic composite coatings obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to wear tests using a ball-disc friction and wear tester of model MPX-3 produced by Jinan Hengxu Testing Machine Technology Co., Ltd. During the test, the sphere diameter was 6 mm, the load was 10 N, the rotation rate was 200 r / min, and the wear time was 1800 s; in accordance with the relevant provisions of GJB548B-2005 method 1009.2 neutral salt spray test, a salt spray test chamber of model Q-FOG / CCT600 produced by the Fifth Institute of Electronics of the Ministry of Industry and Information Technology was used to perform salt spray tests on the carbide ceramic composite coatings obtained in Examples 1 to 4 and Comparative Examples 1 to 3. During the test, the temperature of the salt spray test chamber was 40 ° C, and the salt spray deposition rate was 1.5 mL / 80 cm 2 h, the spray pressure is 30 psi, the mass fraction of the sodium chloride solution is 1%, the placement angle is 20°, and the test time is 72 h. The wear amount and salt spray test results of the carbide ceramic composite coating surfaces prepared in Examples 1 to 4 and Comparative Examples 1 to 3 are shown in Table 1.

[0079] Table 1 Wear loss and salt spray test results of different carbide ceramic composite coating surfaces

[0080]

[0081] As can be seen from Table 1, the present invention significantly improves the wear resistance and corrosion resistance of the carbide ceramic composite coating by optimizing the types and dosage ratios of carbides, inert fillers, alkaline compounds, composite additives, binders and solvents.

[0082] The coating preparation method of the present invention can not only obtain a carbide ceramic composite coating which is firmly bonded to a metal substrate, has a dense coating structure, high hardness, and good wear resistance and corrosion resistance, but also has a simple preparation process, low cost, and is suitable for industrial application.

[0083] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A carbide ceramic composite coating, characterized in that: Contains the following components in parts by weight: 10-20 parts of carbide, 2-6 parts of inert filler, 0.5-1 parts of alkaline compound, 1.5-3 parts of composite additive, 0.2-0.4 parts of binder, 8-15 parts of solvent; The carbide is one or more of tungsten carbide, titanium carbide and chromium carbide, and the particle size of the carbide is 15 to 20 μm; The composite additive material is ferrous oxide and cuprous oxide, and the mass ratio of ferrous oxide to cuprous oxide is 1:2-3; The solvent is tetrahydrofuran, toluene or carbon tetrachloride; The method for preparing the carbide ceramic composite coating comprises the following steps: 1) mixing the carbide and part of the solvent to obtain a mixture I; 2) mixing the inert filler, the composite additive material and the remaining solvent to obtain a mixture II; 3) mixing mixture I, mixture II, a basic compound and a binder to obtain a mixed powder; 4) Laser-cladding the mixed powder onto the surface of the substrate by coaxial powder feeding to obtain a carbide ceramic composite coating; Step 4) The power of the laser cladding is 3-5 kW, and the scanning speed is 50-80 mm / s.

2. The carbide ceramic composite coating according to claim 1, characterized in that: The inert filler is one or more of aluminum oxide, zirconium dioxide and titanium dioxide; the alkaline compound is sodium silicate, sodium carbonate or calcium oxide.

3. The carbide ceramic composite coating according to claim 2, characterized in that: The binder is a phosphoric acid aqueous solution or an acid phosphate.

4. The method for preparing the carbide ceramic composite coating according to any one of claims 1 to 3, characterized in that: The following steps are included: 1) mixing the carbide and part of the solvent to obtain a mixture I; 2) mixing the inert filler, the composite additive material and the remaining solvent to obtain a mixture II; 3) mixing mixture I, mixture II, a basic compound and a binder to obtain a mixed powder; 4) Laser-cladding the mixed powder onto the surface of the substrate by coaxial powder feeding to obtain a carbide ceramic composite coating; Step 4) The power of the laser cladding is 3-5 kW, and the scanning speed is 50-80 mm / s.

5. The preparation method according to claim 4, characterized in that: The mixing speed of step 1) to step 3) is independently 150-200 r / min, the mixing temperature is independently 20-30° C., and the mixing time is independently 30-40 min.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the partial solvent in step 1) to the remaining solvent in step 2) is 1:1-2.