A microwave gyromagnetic ferrite material and preparation method thereof

By preparing La3-x-zCa0.5xBa0.5xBizFe5-x-2yMnyZryTixO12 microwave rotary magnet ferrite material, the existing problem of low dielectric constant is solved, and high dielectric constant and high magnetic performance is achieved, which is suitable for the integration of 5G communication products. and volume reduction requirements.

CN116903358BActive Publication Date: 2024-12-03上海阖煦微波技术有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311006773.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-10
Publication Date
2024-12-03
Estimated Expiration
2043-08-10

AI Technical Summary

Technical Problem

The existing rotary magnetic yttrium iron garnet ferrite has a low dielectric constant, making it difficult to meet the needs of further integration and volume reduction of 5G communication products.

Method used

La3-x-zCa0.5xBa0.5xBizFe5-x-2yMnyZryTixO12 is used as the chemical formula of microwave spiral ferrite material, and is prepared by wet ball milling, spray granulation and sintering, and the raw material ratio and process conditions are optimized to improve the dielectric of the material. Constant and magnetic properties.

Benefits of technology

The prepared microwave rotary ferrite material has high saturation magnetization, dielectric constant and Curie temperature, low loss, good performance consistency, suitable for mass production, and can reduce the size of ferrite to meet the circulator and isolator. performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004388958520000091
    Figure BDA0004388958520000091
  • Figure BDA0004388958520000101
    Figure BDA0004388958520000101
Patent Text Reader

Abstract

The present invention provides a microwave gyromagnetic ferrite material and a preparation method thereof, belonging to the technical field of communication materials. The chemical formula of the microwave gyromagnetic ferrite material of the present invention is La 3‑x‑ z Ca 0.5x Ba 0.5x Bi z Fe 5‑x‑2y Mn y Zr y Ti x O 12 , where 0.01
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of communication materials, and in particular to a microwave gyromagnetic ferrite material and a preparation method thereof. Background Art

[0002] Microwave ferrite circulators are essential components in 5G communications, and are mainly used in base stations and mobile station systems. With the continuous development of mobile communication technology, the basic requirements of mobile communication for communicators are increased frequency, high integration, and further reduction in size.

[0003] Gyromagnetic ferrite is a key material for circulators and should have stable saturation magnetization, high Curie temperature, narrow line width, high dielectric constant, and low loss. However, the dielectric constant of gyromagnetic yttrium iron garnet ferrite in existing circulators is about 15, and it needs to be used with dielectric materials. It is impossible to further reduce the size of the ferrite sleeve dielectric ring product, so it is difficult to meet the needs of further integration and volume reduction of 5G communication products. Therefore, it is of great significance to study a microwave gyromagnetic ferrite material with high saturation magnetization, high dielectric constant, and high Curie temperature and its preparation method. Summary of the invention

[0004] The object of the present invention is to provide a microwave gyromagnetic ferrite material and a preparation method thereof, so as to solve the problem of low dielectric constant of gyromagnetic ferrite in the prior art.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a microwave gyromagnetic ferrite material, the chemical formula of the microwave gyromagnetic ferrite material is La 3-x-z Ca 0.5x Ba 0.5x Bi z Fe 5-x-2y Mn y Zr y Ti x O 12 , where 0.01 <x<0.1,0.1<y<0.2,0.4<z<1.0。

[0007] Preferably, the chemical formula of the microwave gyromagnetic ferrite material is

[0008] La 2.47 Ca 0.015 Ba 0.015 Bi 0.5 Fe 4.73 Mn 0.12 Zr 0.12 Ti 0.03 O 12 ,

[0009] La 2.45 Ca 0.025 Ba 0.025 Bi 0.5 Fe 4.71 Mn 0.12 Zr 0.12 Ti 0.05 O 12 ,

[0010] La 2.42 Ca 0.04 Ba 0.04 Bi 0.5 Fe 4.68 Mn 0.12 Zr 0.12 Ti 0.08 O 12 ,

[0011] La 2.45 Ca 0.025 Ba 0.025 Bi 0.5 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 ,

[0012] La 2.45 Ca 0.025 Ba 0.025 Bi 0.5 Fe 4.59 Mn 0.18 Zr 0.18 Ti 0.05 O 12 ,

[0013] La 2.35 Ca 0.025 Ba 0.025 Bi 0.6 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 ,

[0014] La 2.25 Ca 0.025 Ba 0.025 Bi 0.7 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 ,

[0015] La2.15 Ca 0.025 Ba 0.025 Bi 0.8 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 ,

[0016] La 2.05 Ca 0.025 Ba 0.025 Bi 0.9 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 .

[0017] The present invention provides a method for preparing a microwave gyromagnetic ferrite material, comprising the following steps:

[0018] 1) weighing raw materials according to the stoichiometric ratio, and then mixing the raw materials and performing wet ball milling;

[0019] 2) mixing the wet ball-milled slurry with polyvinyl alcohol glue, and then sequentially performing spray granulation, pre-sintering, secondary wet ball milling, and secondary spray granulation to obtain a powder;

[0020] 3) The powder is pressed into shape and then sintered to obtain a microwave gyromagnetic ferrite material.

[0021] Preferably, in step 1), the raw materials include La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2.

[0022] Preferably, in step 1), the mass ratio of zirconia balls, raw materials and water during wet ball milling is 3.0-3.5:1:1, the rotation speed of the wet ball milling is 200-400 rpm, and the time is 40-60 min.

[0023] Preferably, in the step 2), the mass ratio of the slurry after wet ball milling to the polyvinyl alcohol glue is 1:8-12, wherein the content of polyvinyl alcohol in the polyvinyl alcohol glue is 1.0-1.4%.

[0024] Preferably, in step 2), the pre-sintering temperature is 700-800° C., and the holding time is 2-4 hours.

[0025] Preferably, in the step 2), the mass ratio of zirconia balls, raw materials and water during the secondary wet ball milling treatment is 3.0 - 3.5:1:0.4 - 0.6, the rotation speed of the secondary wet ball milling treatment is 300 - 500 rpm, and the time is 2 - 3 h.

[0026] Preferably, in the step 3), the pressure for pressing and forming is 0.3 - 1.5 MPa / cm 2 .

[0027] Preferably, in the step 3), the sintering temperature is 940 - 960 °C, and the heat preservation time is 5 - 7 h.

[0028] Advantages of the present invention:

[0029] The microwave rotating ferrite material prepared by the present invention has the advantages of high saturation magnetization intensity, high dielectric constant, high Curie temperature, low loss, good performance consistency, and suitability for mass production. The 4πMs of the microwave rotating ferrite material of the present invention is 1820 Gs, the Curie temperature Tc is 215 °C, the line width ΔH is 35 Oe, and the dielectric constant ε r is 22.1, all of which can well meet the s - parameter requirements of circulators and isolators, and the third - order intermodulation is good. At the same time, the ferrite size of the conventional 1800 Gs material can be reduced. Specific embodiments

[0030] The present invention provides a microwave rotating ferrite material, and the chemical formula of the microwave rotating ferrite material is La 3-x-z Ca 0.5x Ba 0.5x Bi z Fe 5-x-2y Mn y Zr y Ti x O 12 , where 0.01 < x < 0.1, 0.1 < y < 0.2, 0.4 < z < 1.0.

[0031] In the present invention, the chemical formula of the microwave rotating ferrite material is La 3-x-z Ca 0.5x Ba 0.5x Bi z Fe 5-x- 2y Mn y Zr y Ti x O 12 , where 0.01 < x < 0.1, preferably 0.03 ≤ x ≤ 0.08; 0.1 < y < 0.2, preferably 0.12 ≤ y ≤ 0.18; 0.4 < z < 1.0, preferably 0.5 ≤ z ≤ 0.9.

[0032] In the course of the present study, the chemical formula of the material of the wave-rotating iron and steel material is selected.

[0033] La 2.47 Ca 0.015 Ba 0.015 Bi 0.5 Fe 4.73 Mn 0.12 Zr 0.12 Ti 0.03 O 12 ,

[0034] La 2.45 Ca 0.025 Ba 0.025 Bi 0.5 Fe 4.71 Mn 0.12 Zr 0.12 Ti 0.05 O 12 ,

[0035] La 2.42 Ca 0.04 Ba 0.04 Bi 0.5 Fe 4.68 Mn 0.12 Zr 0.12 Ti 0.08 O 12 ,

[0036] La 2.45 Ca 0.025 Ba 0.025 Bi 0.5 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 ,

[0037] La 2.45 Ca 0.025 Ba 0.025 Bi 0.5 Fe 4.59 Mn 0.18 Zr 0.18 Ti 0.05 O 12 ,

[0038] La 2.35 Ca 0.025 Ba 0.025 Bi 0.6 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 ,

[0039] La 2.25 Ca 0.025 Ba 0.025 Bi 0.7 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 ,

[0040] La 2.15 Ca 0.025 Ba 0.025 Bi 0.8 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 ,

[0041] La 2.05 Ca 0.025 Ba 0.025 Bi 0.9 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 .

[0042] The present invention provides a method for preparing a microwave gyromagnetic ferrite material, comprising the following steps:

[0043] 1) weighing raw materials according to the stoichiometric ratio, and then mixing the raw materials and performing wet ball milling;

[0044] 2) mixing the wet ball-milled slurry with polyvinyl alcohol glue, and then sequentially performing spray granulation, pre-sintering, secondary wet ball milling, and secondary spray granulation to obtain a powder;

[0045] 3) The powder is pressed into shape and then sintered to obtain a microwave gyromagnetic ferrite material.

[0046] In the present invention, in the step 1), the raw materials include La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2.

[0047] In the present invention, in the step 1), the mass ratio of zirconia balls, raw materials and water during wet ball milling is 3.0-3.5:1:1, preferably 3.1-3.4:1:1, and more preferably 3.2-3.3:1:1; the rotation speed of the wet ball milling is 200-400 rpm, preferably 250-350 rpm, and more preferably 280-320 rpm; the time is 40-60 min, preferably 45-55 min, and more preferably 50 min.

[0048] In the present invention, in the step 2), the mass ratio of the slurry after wet ball milling to the polyvinyl alcohol glue is 1:8-12, preferably 1:9-11, and more preferably 1:10, wherein the content of polyvinyl alcohol in the polyvinyl alcohol glue is 1.0-1.4%, preferably 1.1-1.3%, and more preferably 1.2%.

[0049] In the present invention, in the step 2), the pre-sintering temperature is 700-800°C, preferably 720-780°C, and more preferably 750°C; the holding time is 2-4h, preferably 2.5-3.5h, and more preferably 3h.

[0050] In the present invention, in the step 2), the mass ratio of zirconia balls, raw materials and water during the secondary wet ball milling treatment is 3.0-3.5:1:0.4-0.6, preferably 3.1-3.4:1:0.45-0.55, and more preferably 3.2-3.3:1:0.55; the rotation speed of the secondary wet ball milling treatment is 300-500rpm, preferably 350-450rpm, and more preferably 400rpm; the time is 2-3h, preferably 2.2-2.6h, and more preferably 2.5h.

[0051] In the present invention, the D50 of the slurry obtained after the secondary ball milling treatment is ≤0.5 μm, preferably ≤0.4 μm.

[0052] In the present invention, in the step 2), the powder is obtained by sieving after the secondary spray granulation, and the particle size of the powder is 60 to 200 meshes, preferably 70 to 190 meshes, and more preferably 80 to 180 meshes.

[0053] In the present invention, in step 3), the pressure of the pressing molding is 0.3-1.5 MPa / cm 2 , preferably 0.6~1.2MPa / cm 2 , more preferably 0.9 to 1.1 MPa / cm 2 .

[0054] In the present invention, the density of the green body obtained after compression molding is 3.0 to 3.4 g / cm 3, preferably 3.1 to 3.3 g / cm 3 , more preferably 3.2 g / cm 3 .

[0055] In the present invention, in the step 3), the sintering temperature is 940-960° C., preferably 950° C.; the holding time is 5-7 hours, preferably 5.5-6.5 hours, and more preferably 6 hours.

[0056] In the present invention, the sintered microwave gyromagnetic ferrite material can be processed to the required size according to the finishing process list. In the present invention, it is preferably processed into a 2.0mm diameter ball, a D1.6*22 magnetic needle rod, a 1.0mm diameter ball, and a D25 / 20 / 8 magnetic ring.

[0057] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0058] Example 1

[0059] La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2 were weighed according to a molar ratio of 1.235:0.015:0.015:0.25:2.365:0.04:0.12:0.03, and the raw materials were mixed evenly. Then, the raw materials were put into a ball mill according to a mass ratio of 3.3:1:1 of zirconia balls, raw materials and deionized water, and wet ball milled at 300rpm for 50min to obtain slurry; the slurry and polyvinyl alcohol glue were mixed according to a mass ratio of 1:10, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then spray granulation and pre-sintering were carried out, wherein the pre-sintering temperature was 750°C and the insulation time was 3h.

[0060] After pre-sintering, the zirconia balls, raw materials, and deionized water were placed in a ball mill at a mass ratio of 3.3:1:0.55, and subjected to secondary wet ball milling at 400rpm for 2.5h to obtain a slurry with a D50 of 0.4μm; the slurry and polyvinyl alcohol glue were mixed at a mass ratio of 1:10, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then secondary spray granulation was performed, and a powder of 60 to 120 mesh was obtained after sieving. Finally, the powder was sieved at 1MPa / cm 2 After compression molding under pressure, the density is 3.2g / cm 3 The green body is sintered at 950℃ for 6h to obtain microwave gyromagnetic ferrite material.

[0061] Example 2

[0062] La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2 were weighed according to a molar ratio of 1.225:0.025:0.025:0.25:2.335:0.04:0.12:0.05, and the raw materials were mixed evenly. Then, the raw materials were put into a ball mill according to a mass ratio of 3.0:1:1 of zirconia balls, raw materials and deionized water, and wet ball milled at 200rpm for 60min to obtain slurry; the slurry and polyvinyl alcohol glue were mixed in a mass ratio of 1:11, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.1%, and then spray granulation and pre-sintering were carried out, wherein the pre-sintering temperature was 800℃ and the insulation time was 2h.

[0063] After pre-sintering, the zirconia balls, raw materials, and deionized water were placed in a ball mill at a mass ratio of 3.0:1:0.4, and subjected to secondary wet ball milling at 500rpm for 2h to obtain a slurry with a D50 of 0.3μm; the slurry and polyvinyl alcohol glue were mixed at a mass ratio of 1:11, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.1%, and then secondary spray granulation was performed, and a powder of 80 to 180 mesh was obtained after sieving. Finally, the powder was sieved at 1.2MPa / cm 2 After compression molding under pressure, the density is 3.3g / cm 3 The green body is sintered at 960℃ for 5h to obtain microwave gyromagnetic ferrite material.

[0064] Example 3

[0065] La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2 were weighed according to a molar ratio of 1.21:0.04:0.04:0.25:2.34:0.04:0.12:0.08, and the raw materials were mixed evenly. Then, according to the mass ratio of zirconia balls, raw materials and deionized water of 3.5:1:1, they were put into a ball mill, and wet ball milled at 200rpm for 40min to obtain slurry; the slurry and polyvinyl alcohol glue were mixed in a mass ratio of 1:9, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.4%, and then spray granulation and pre-sintering were carried out, wherein the pre-sintering temperature was 700℃, and the insulation time was 2h.

[0066] After pre-sintering, the zirconia balls, raw materials, and deionized water were placed in a ball mill at a mass ratio of 3.5:1:0.6, and subjected to secondary wet ball milling at 300 rpm for 3 hours to obtain a slurry with a D50 of 0.4 μm; the slurry and polyvinyl alcohol glue were mixed at a mass ratio of 1:9, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.4%, and then secondary spray granulation was performed to obtain a powder of 70 to 160 mesh. Finally, the powder was heated at 0.8 MPa / cm 2 After compression molding under pressure, the density is 3.1g / cm 3 The green body is sintered at 940℃ for 5h to obtain microwave gyromagnetic ferrite material.

[0067] Example 4

[0068] La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2 were weighed according to a molar ratio of 1.225:0.025:0.025:0.25:2.325:0.05:0.15:0.05, and the raw materials were mixed evenly. Then, according to the mass ratio of zirconia balls, raw materials and deionized water of 3.1:1:1, they were put into a ball mill, and wet ball milled at 220rpm for 45min to obtain slurry; the slurry and polyvinyl alcohol glue were mixed in a mass ratio of 1:9, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then spray granulation and pre-sintering were carried out, wherein the pre-sintering temperature was 720℃, and the insulation time was 2.5h.

[0069] After pre-sintering, the zirconia balls, raw materials, and deionized water were placed in a ball mill at a mass ratio of 3.1:1:0.4, and subjected to secondary wet ball milling at 320 rpm for 3 hours to obtain a slurry with a D50 of 0.2 μm; the slurry and polyvinyl alcohol glue were mixed at a mass ratio of 1:9, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then secondary spray granulation was performed to obtain a powder of 80 to 190 mesh. Finally, the powder was heated at 1.2 MPa / cm 2 After compression molding under pressure, the density is 3.3g / cm 3 The green body is sintered at 950℃ for 7h to obtain microwave gyromagnetic ferrite material.

[0070] Example 5

[0071] La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2 were weighed according to a molar ratio of 1.225:0.025:0.025:0.25:2.295:0.06:0.18:0.05, and the raw materials were mixed evenly. Then, according to the mass ratio of zirconia balls, raw materials and deionized water of 3.2:1:1, they were put into a ball mill, and wet ball milled at 260rpm for 55min to obtain slurry; the slurry and polyvinyl alcohol glue were mixed in a mass ratio of 1:11, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.3%, and then spray granulation and pre-sintering were carried out, wherein the pre-sintering temperature was 760℃, and the insulation time was 3h.

[0072] After pre-sintering, the zirconia balls, raw materials, and deionized water were placed in a ball mill at a mass ratio of 3.2:1:0.45, and subjected to secondary wet ball milling at 380 rpm for 2.5 hours to obtain a slurry with a D50 of 0.1 μm; the slurry and polyvinyl alcohol glue were mixed at a mass ratio of 1:11, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.3%, and then secondary spray granulation was performed to obtain a powder of 100 to 160 mesh. Finally, the powder was subjected to a pressure of 1.2 MPa / cm 2 After compression molding under pressure, the density is 3.3g / cm 3 The green body is sintered at 950℃ for 7h to obtain microwave gyromagnetic ferrite material.

[0073] Example 6

[0074] La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2 were weighed according to a molar ratio of 1.175:0.025:0.025:0.3:2.325:0.05:0.15:0.05, and the raw materials were mixed evenly. Then, according to the mass ratio of zirconia balls, raw materials and deionized water of 3.2:1:1, they were put into a ball mill, and wet ball milled at 280rpm for 55min to obtain slurry; the slurry and polyvinyl alcohol glue were mixed in a mass ratio of 1:8, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.4%, and then spray granulation and pre-sintering were carried out, wherein the pre-sintering temperature was 780℃, and the insulation time was 3h.

[0075] After pre-sintering, the zirconia balls, raw materials, and deionized water were placed in a ball mill at a mass ratio of 3.2:1:0.45, and subjected to secondary wet ball milling at 420 rpm for 2.5 hours to obtain a slurry with a D50 of 0.3 μm; the slurry and polyvinyl alcohol glue were mixed at a mass ratio of 1:8, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.4%, and then secondary spray granulation was performed to obtain a powder of 60 to 160 mesh. Finally, the powder was heated at 0.8 MPa / cm 2 After compression molding under pressure, the density is 3.1g / cm 3 The green body is sintered at 950℃ for 5h to obtain microwave gyromagnetic ferrite material.

[0076] Example 7

[0077] La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2 were weighed according to a molar ratio of 1.125:0.025:0.025:0.35:2.365:0.05:0.15:0.05, and the raw materials were mixed evenly. Then, the raw materials were put into a ball mill according to a mass ratio of 3.3:1:1 of zirconia balls, raw materials and deionized water, and wet ball milled at 300rpm for 50min to obtain slurry; the slurry and polyvinyl alcohol glue were mixed according to a mass ratio of 1:10, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then spray granulation and pre-sintering were carried out, wherein the pre-sintering temperature was 750°C and the insulation time was 3h.

[0078] After pre-sintering, the zirconia balls, raw materials, and deionized water were placed in a ball mill at a mass ratio of 3.3:1:0.55, and were subjected to secondary wet ball milling at 400rpm for 2.5h to obtain a slurry with a D50 of 0.5μm; the slurry and polyvinyl alcohol glue were mixed at a mass ratio of 1:10, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then secondary spray granulation was performed to obtain a powder of 100-160 mesh. Finally, the powder was subjected to a pressure of 1MPa / cm 2 After compression molding under pressure, the density is 3.2g / cm 3 The green body is sintered at 950℃ for 6h to obtain microwave gyromagnetic ferrite material.

[0079] Example 8

[0080] La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2 were weighed according to a molar ratio of 1.075:0.025:0.025:0.4:2.365:0.05:0.15:0.05, and the raw materials were mixed evenly. Then, according to the mass ratio of zirconia balls, raw materials and deionized water of 3.2:1:1, they were put into a ball mill, and wet ball milled at 320rpm for 45min to obtain slurry; the slurry and polyvinyl alcohol glue were mixed in a mass ratio of 1:10, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then spray granulation and pre-sintering were carried out, wherein the pre-sintering temperature was 740°C and the insulation time was 2h.

[0081] After pre-sintering, the zirconia balls, raw materials, and deionized water were placed in a ball mill at a mass ratio of 3.2:1:0.50, and subjected to secondary wet ball milling at 380 rpm for 3 hours to obtain a slurry with a D50 of 0.1 μm; the slurry and polyvinyl alcohol glue were mixed at a mass ratio of 1:10, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then secondary spray granulation was performed to obtain a powder of 80 to 150 mesh. Finally, the powder was heated at 0.8 MPa / cm 2 After compression molding under pressure, the density is 3.1g / cm 3 The green body is sintered at 950℃ for 6h to obtain microwave gyromagnetic ferrite material.

[0082] Example 9

[0083] La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2 were weighed according to a molar ratio of 1.025:0.025:0.025:0.45:2.365:0.05:0.15:0.05, and the raw materials were mixed evenly. Then, according to the mass ratio of zirconia balls, raw materials and deionized water of 3.2:1:1, they were put into a ball mill, and wet ball milled at 320rpm for 45min to obtain slurry; the slurry and polyvinyl alcohol glue were mixed in a mass ratio of 1:10, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then spray granulation and pre-sintering were carried out, wherein the pre-sintering temperature was 740°C and the insulation time was 2h.

[0084] After pre-sintering, the zirconia balls, raw materials, and deionized water were placed in a ball mill at a mass ratio of 3.2:1:0.50, and subjected to secondary wet ball milling at 380 rpm for 3 hours to obtain a slurry with a D50 of 0.2 μm; the slurry and polyvinyl alcohol glue were mixed at a mass ratio of 1:10, wherein the content of polyethylene in the polyvinyl alcohol glue was 1.2%, and then secondary spray granulation was performed to obtain a powder of 80 to 180 mesh. Finally, the powder was heated at 1.0 MPa / cm 2 After compression molding under pressure, the density is 3.2g / cm 3 The green body is sintered at 950℃ for 6h to obtain microwave gyromagnetic ferrite material.

[0085] The microwave gyromagnetic ferrite materials prepared in Examples 1 to 9 were subjected to performance tests, and the test method was as follows: the performance test method of gyromagnetic materials for microwave frequency applications in accordance with GB-T9633-2012.

[0086] The test results are shown in Table 1:

[0087] Table 1 Performance test results of microwave gyromagnetic ferrite materials prepared in Examples 1 to 9

[0088]

[0089] It can be seen from Table 1 that the microwave gyromagnetic ferrite material prepared in Example 7 has the best performance.

[0090] The microwave gyromagnetic ferrite material prepared in Example 7 was processed into a product D12.2 / 2.2 disc, which was loaded into the circulator cavity. The circulator performance was tested using a vector network analyzer and an intermodulation test platform (2G-18G solid-state power amplifier 80W, signal source E8257D, Agilent 8481H_10MHz_18GHz_-10dBm to+35dBm_power probe, power meter, Agilent spectrum analyzer). The test results are shown in Table 2:

[0091] Table 2 Circulator performance test results

[0092]

[0093] It can be seen from the above embodiments that the present invention provides a microwave gyromagnetic ferrite material and a preparation method thereof. The chemical formula of the microwave gyromagnetic ferrite material of the present invention is La 3-x-z Ca 0.5x Ba 0.5x Bi z Fe 5-x-2y Mn y Zr y Ti x O 12, where 0.01 < x < 0.1, 0.1 < y < 0.2, 0.4 < z < 1.0. First, the raw materials of the present invention are subjected to wet ball milling treatment, then mixed with polyvinyl alcohol glue, followed by spray granulation, pre-sintering, secondary wet ball milling treatment, and secondary spray granulation. Finally, the obtained powder is pressed into a shape and then sintered to obtain the microwave rotating ferrite material. The microwave rotating ferrite material prepared by the present invention has the advantages of high saturation magnetization intensity, high dielectric constant, high Curie temperature, low loss, good performance consistency, and suitability for mass production.

[0094] The above are only the preferred embodiments of the present invention. It should be noted that for those of ordinary skill in the art, without departing from the principle of the present invention, several improvements and refinements can be made, and these improvements and refinements should also be regarded as the protection scope of the present invention.

Claims

1. A microwave gyromagnetic ferrite material, characterized in that: The chemical formula of the microwave gyromagnetic ferrite material is La 3-x- z Ca 0.5x Ba 0.5x Bi z Fe 5-x-2y Mn y Zr y Ti x O 12 , where 0.01 <x<0.1,0.1<y<0.2,0.4<z<1.0。 2. The microwave gyromagnetic ferrite material according to claim 1, characterized in that: The chemical formula of the microwave gyromagnetic ferrite material is La 2.47 Ca 0.015 Ba 0.015 Bi 0.5 Fe 4.73 Mn 0.12 Zr 0.12 Ti 0.03 O 12 , La 2.45 Ca 0.025 Ba 0.025 Bi 0.5 Fe 4.71 Mn 0.12 Zr 0.12 Ti 0.05 O 12 , La 2.42 Ca 0.04 Ba 0.04 Bi 0.5 Fe 4.68 Mn 0.12 Zr 0.12 Ti 0.08 O 12 , La 2.45 Ca 0.025 Ba 0.025 Bi 0.5 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 , La 2.45 Ca 0.025 Ba 0.025 Bi 0.5 Fe 4.59 Mn 0.18 Zr 0.18 Ti 0.05 O 12 , La 2.35 Ca 0.025 Ba 0.025 Bi 0.6 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 , La 2.25 Ca 0.025 Ba 0.025 Bi 0.7 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 , La 2.15 Ca 0.025 Ba 0.025 Bi 0.8 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 , La 2.05 Ca 0.025 Ba 0.025 Bi 0.9 Fe 4.65 Mn 0.15 Zr 0.15 Ti 0.05 O 12 .

3. The method for preparing the microwave gyromagnetic ferrite material according to claim 1 or 2, characterized in that: The steps include: 1) weighing raw materials according to the stoichiometric ratio, and then mixing the raw materials and performing wet ball milling; 2) mixing the wet ball-milled slurry with polyvinyl alcohol glue, and then sequentially performing spray granulation, pre-sintering, secondary wet ball milling, and secondary spray granulation to obtain a powder; 3) Pressing the powder into a shape and then sintering it to obtain a microwave ferrite material; In the step 3), the sintering temperature is 940-960° C. and the holding time is 5-7 hours.

4. The preparation method according to claim 3, characterized in that: In the step 1), the raw materials include La2O3, CaCO3, BaCO3, Bi2O3, Fe2O3, Mn3O4, ZrO2 and TiO2.

5. The preparation method according to claim 3 or 4, characterized in that: In the step 1), the mass ratio of the zirconia balls, the raw materials and the water during the wet ball milling treatment is 3.0 to 3.5:1:1, the rotation speed of the wet ball milling treatment is 200 to 400 rpm, and the time is 40 to 60 minutes.

6. The preparation method according to claim 5, characterized in that: In the step 2), the mass ratio of the slurry after wet ball milling to the polyvinyl alcohol glue is 1:8-12, wherein the content of polyvinyl alcohol in the polyvinyl alcohol glue is 1.0-1.4%.

7. The preparation method according to claim 4 or 6, characterized in that: In the step 2), the pre-sintering temperature is 700-800° C., and the holding time is 2-4 hours.

8. The preparation method according to claim 7, characterized in that: In the step 2), the mass ratio of zirconia balls, raw materials and water during the secondary wet ball milling treatment is 3.0-3.5:1:0.4-0.6, the rotation speed of the secondary wet ball milling treatment is 300-500 rpm, and the time is 2-3 hours.

9. The preparation method according to claim 4, 6 or 8, characterized in that: In the step 3), the pressure of the pressing molding is 0.3-1.5 MPa / cm 2 .