ASA / ABS composite material and its preparation method and application
Through the design of ASA/ABS composite material, the polybutadiene content in ABS resin is controlled and other additives are combined, the toughness and abnormal noise problems of ASA materials under low temperature conditions are solved, and its weather resistance is improved, achieving excellent Low temperature toughness and anti-iron noise characteristics meet the high performance needs of automotive parts.
Patent Information
- Application Number
- CN202310644374.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-31
AI Technical Summary
In automotive parts, ASA materials are prone to appearance surface rupture and structural fracture under low temperature conditions, and abnormal noises are generated due to accidental relative friction, which affects the user experience. At the same time, degradation and yellowing are easily caused under light, affecting weather resistance and aesthetics. .
ASA/ABS composite material is used to control the mass content of polybutadiene in ABS resin to be 12% to 18%, and it is combined with ASA glue powder and SAN resin to add anti-irror noise additives, weather resistance agents, antioxidants and antioxidants. Lubricant, improves the low temperature toughness, weather resistance and anti-irror characteristics of the material.
The excellent low-temperature toughness, weather resistance and abnormal noise resistance of ASA/ABS composite materials under low temperature conditions were achieved. The test results show that the RPN is 1 to 3, and the appearance grayscale is above level 4 after the weather resistance test of 1600 hours, and the notch impact strength can reach 1.7kJ/m2 or above, significantly improving the overall performance of the material.
Smart Images

Figure BDA0004264361210000021 
Figure BDA0004264361210000022 
Figure BDA0004264361210000071
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer composite materials, in particular to an ASA / ABS composite material and a preparation method and application thereof. Background Art
[0002] Since Karl Benz invented the first gasoline internal combustion engine car in the 19th century, global automobile production reached 96.86 million units in 2017, driven by the continuous advancement of automotive technology and production. In today's world, where energy conservation and emission reduction are a global concern, lightweighting vehicles has always been a topic of constant concern for the automotive industry. The rapid development of polymer materials technology has made it possible to replace steel with plastic. Large-scale components such as bumpers, spoilers, and luggage racks are increasingly being made of plastic, reducing vehicle weight and significantly lowering fuel consumption. Industry estimates suggest that for every 10% reduction in vehicle weight, fuel consumption can be reduced by 6% to 8% and emissions by 5% to 6%.
[0003] Acrylonitrile-acrylate-styrene copolymer (ASA) is commonly used in the production of automotive parts such as grilles, spoilers, and rearview mirror housings. Automakers have discovered that when assembled with other components, plastic parts containing ASA can produce a "creaking" noise due to accidental friction. This noise is particularly common when the car is driven over uneven roads or exposed to drastic temperature fluctuations outdoors, significantly impacting the customer experience. Traditional solutions involve applying felt or lubricating oil to the buckles or guide rails, but this complicates processing and increases costs. Furthermore, components used outside the vehicle cockpit require extremely high weather resistance. Styrene-based high-molecular-weight copolymers are easily excited by light to produce free radicals. Once these free radicals are generated, a chain reaction of photoaging causes the copolymer to degrade, resulting in noticeable yellowing or even powdering, impacting the aesthetics and safety of the plastic part. Although ASA itself has good weather resistance, its low-temperature toughness is poor. When evaluating the low-temperature toughness of parts, there is a risk of surface cracking or even fracture in some structural positions.
[0004] How to provide an ASA material with good low-temperature toughness, weather resistance and anti-squeak properties, while solving the "creaking" problem of parts and ensuring that the parts have good weather resistance and good low-temperature toughness, has always been a difficult problem in the industry. Summary of the Invention
[0005] Based on this, the present invention provides an ASA / ABS composite material with good low-temperature toughness, weather resistance and anti-squeak properties, which can be used to prepare automotive parts.
[0006] The technical solution is as follows:
[0007] An ASA / ABS composite material comprises the following components in parts by weight:
[0008]
[0009] The mass content of polybutadiene in the ABS resin is 12% to 18%.
[0010] In some embodiments, the ASA / ABS composite material includes the following components in parts by weight:
[0011]
[0012] In some embodiments, the average particle size of the rubber phase of the ABS resin is 50 nm to 800 nm.
[0013] In some embodiments, the anti-squeaking agent is selected from vinyl copolymers and / or styrene copolymers.
[0014] In some embodiments, the vinyl copolymer is selected from one or more of ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-octene copolymer, ethylene-maleic anhydride copolymer, ethylene-styrene-maleic anhydride copolymer, ethylene-propylene-maleic anhydride copolymer and ethylene-octene-maleic anhydride copolymer.
[0015] In some embodiments, the styrene-based copolymer is selected from one or more of acrylonitrile-styrene-acrylate copolymer, acrylonitrile-styrene-butadiene copolymer, acrylonitrile-styrene-ethylene propylene rubber copolymer, acrylate-styrene-butadiene copolymer, styrene-ethylene-styrene copolymer, styrene-hydrogenated ethylene-styrene copolymer, styrene-ethylene-butylene-styrene copolymer and styrene-hydrogenated ethylene-styrene-maleic anhydride copolymer.
[0016] In some embodiments, the mass content of polystyrene in the SAN resin is 70% to 75%.
[0017] In some embodiments, the mass content of polystyrene in the ASA rubber powder is 35% to 40%.
[0018] In some embodiments, the average particle size of the ASA rubber powder is 100 nm to 300 nm.
[0019] In some embodiments, the ASA / ABS composite material further comprises one or more of a weathering agent, an antioxidant, a lubricant and a color powder.
[0020] In some embodiments, the weathering agent is selected from benzotriazole light stabilizers and / or triazine ultraviolet light absorbers.
[0021] In some embodiments, the antioxidant is selected from one or more of organic phosphates, alkylated monophenols, alkylated polyphenols, alkylation reaction products of polyphenols and dienes, butylation reaction products of p-cresol or dicyclopentadiene, alkylated hydroquinones, hydroxylated thiodiphenyl ethers, alkylidene bisphenols, benzyl compounds, esters of β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid and monohydric or polyhydric alcohols, esters of β-(5-tert-butyl-4-hydroxy-3-methylphenyl)-propionic acid and monohydric or polyhydric alcohols, esters of sulfanyl compounds, esters of sulfaryl compounds, and amides of β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid.
[0022] In some embodiments, the lubricant is selected from one or more of zinc stearate, calcium stearate, magnesium stearate, polyethylene wax, EVA wax, oleamide, erucamide, ethylene bisstearamide, silicone lubricant and pentaerythritol stearate.
[0023] In some embodiments, the toner is selected from pigments and / or dye additives.
[0024] In some embodiments, the ASA / ABS composite material further comprises 0.5 to 6 parts by weight of a weathering agent.
[0025] In some embodiments, the ASA / ABS composite material further comprises 0.1 to 2 parts of an antioxidant and 0.1 to 2 parts of a lubricant, based on weight.
[0026] The present invention also provides a method for preparing the ASA / ABS composite material as described above, and the technical solution is as follows:
[0027] A method for preparing the ASA / ABS composite material as described above comprises the following steps:
[0028] The components are blended and extruded.
[0029] In some embodiments, the blending temperature is 15°C to 30°C.
[0030] In some embodiments, the extrusion temperature is 200°C to 240°C.
[0031] The present invention also provides an application of the above-mentioned ASA / ABS composite material, and the technical solution is as follows:
[0032] A vehicle part comprises the ASA / ABS composite material as described above, or the ASA / ABS composite material prepared according to the preparation method as described above.
[0033] The present invention has the following beneficial effects:
[0034] The ASA / ABS composite material provided by the present invention comprises ASA rubber powder, a specific ABS resin, a SAN resin, and an anti-squeak additive in a specific ratio. The inventors have discovered that ABS can be used as a toughening agent for ASA, improving its low-temperature toughness while also impacting its squeak and weather resistance. By controlling the mass content of polybutadiene in the ABS resin to 12% to 18%, it can synergize with the ASA rubber powder, SAN resin, and anti-squeak additive to produce an ASA / ABS composite material with excellent low-temperature toughness, weather resistance, and anti-squeak properties. The composite material can be used in automotive parts.
[0035] The test shows that the RPN of the ASA / ABS composite material is 1 to 3, showing excellent anti-squeaking performance; after 1600 hours of weathering test, the product appearance grayscale is above level 4, showing excellent weathering resistance; the notched impact strength at -30°C can reach 1.7kJ / m 2 Above, some can reach 7.5kJ / m 2 , showing excellent low temperature toughness.
[0036] In addition, the preparation method of the ASA / ABS composite material of the present invention is simple in process, environmentally friendly and safe, and suitable for scale-up production. DETAILED DESCRIPTION
[0037] To make the above-mentioned objects, features, and advantages of the present invention more readily apparent, specific embodiments of the present invention are described in detail below. The following description sets forth numerous specific details to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art may make similar modifications without departing from the scope of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention pertains. The terms used in this specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0039] In the present invention, when referring to numerical ranges, unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Furthermore, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges subsumed therein.
[0040] The temperature parameters in the present invention, unless otherwise specified, allow for either constant temperature treatment or treatment within a certain temperature range. The constant temperature treatment allows for temperature fluctuations within the precision range controlled by the instrument.
[0041] In the present invention, when referring to a data range, if the unit is only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 150-160°C means that the units of the left endpoint "150" and the right endpoint "160" are both °C (Celsius).
[0042] In the present invention, in the description of the invention, "several" means at least two, such as two, three, etc., unless otherwise clearly and specifically limited. In the description of the present application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically limited.
[0043] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.
[0044] Unless otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0045] Where “including,” “having,” and “comprising” are used herein, it is intended to cover a non-exclusive inclusion, and another component may also be added unless a clear limiting term such as “only,” “consisting of,” etc. is used.
[0046] Unless mentioned otherwise, terms in the singular may include plural forms and should not be construed as having one number.
[0047] The invention provides an ASA / ABS composite material with good low-temperature toughness, weather resistance and noise prevention properties, which can be used for preparing vehicle parts.
[0048] The technical solution is as follows:
[0049] An ASA / ABS composite material comprises the following components in parts by weight:
[0050]
[0051] The mass content of polybutadiene in the ABS resin is 12% to 18%.
[0052] ABS resin is a terpolymer of acrylonitrile, butadiene, and styrene. The inventors discovered that the polybutadiene rubber in ABS has a lower glass transition temperature than the acrylic rubber in ASA. Therefore, ABS can serve as a toughening agent to improve the low-temperature toughness of ASA. Furthermore, ABS has softer chains than ASA, making it a synergistic additive for improving ASA's squeak and squeal properties. However, polybutadiene rubber contains unsaturated double bonds, which easily break open under light to form other substances, causing the material to yellow. Compounding with ASA protects ABS from a loss of weather resistance. This means that ABS resin can serve as a toughening agent for ASA rubber powder, improving its low-temperature toughness while also impacting its squeak and squeal properties and weather resistance. By controlling the polybutadiene content in ABS resin to 12% to 18% by weight, it can synergize with ASA rubber powder, SAN resin, and an anti-squeak additive to produce an ASA / ABS composite with excellent low-temperature toughness, weather resistance, and anti-squeak properties.
[0053] It can be understood that in the present invention, the mass content of polybutadiene in the ABS resin is 12% to 18%, including but not limited to 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5% and 18%.
[0054] Furthermore, in the present invention, the mass content of polystyrene in the ABS resin is 63% to 66%, including but not limited to 63%, 63.5%, 64%, 64.5%, 65%, 65.5% and 66%.
[0055] Furthermore, in the present invention, the mass content of polyacrylonitrile in the ABS resin is 19% to 25%, including but not limited to 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5% and 25%.
[0056] It can be understood that in the present invention, the ASA / ABS composite material contains 5 to 15 parts of ABS resin in parts by weight, including but not limited to 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts and 15 parts, preferably 5 to 10 parts.
[0057] In some embodiments, the average particle size of the rubber phase of the ABS resin is 50nm to 800nm. Such ABS resin can make the composite material have better low-temperature toughness and anti-squeak properties. It is understood that the average particle size of the rubber phase of the ABS resin includes but is not limited to 50nm, 60nm, 80nm, 100nm, 120nm, 150nm, 160nm, 180nm, 200nm, 250nm, 280nm, 300nm, 350nm, 380nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm, 750nm and 800nm. Preferably, the average particle size of the rubber phase of the ABS resin is 200nm to 400nm. Such ABS resin can further synergize the low-temperature toughness and anti-squeak properties of the composite material.
[0058] In some embodiments, the ABS resin is Chimei 757, the average particle size of the rubber phase is 200 nm, and the mass content of polybutadiene is 14%.
[0059] In some embodiments, the ABS resin is prepared by blending SAN 80HF and Kumho Petrochemical ABS high-rubber powder HR181 in a mass ratio of 70:30, wherein the average particle size of the rubber phase is 400 nm and the mass content of polybutadiene is 18%;
[0060] In some embodiments, the ABS resin is Sinopec ABS 275, the average particle size of the rubber phase is 800 nm, and the mass content of polybutadiene is 12%.
[0061] In some embodiments, the ABS resin is prepared by blending SAN 80HF and Kumho Petrochemical ABS high-rubber powder HR192 in a mass ratio of 70:30, wherein the average particle size of the rubber phase is 50 nm and the mass content of polybutadiene is 15%.
[0062] In the present invention, ASA resin is an impact-modified resin copolymerized from styrene, acrylonitrile, and acrylic rubber, exhibiting excellent mechanical and physical properties, weather resistance, and relatively good high-temperature resistance. It is understood that, by weight, the ASA / ABS composite material comprises 20 to 35 parts of ASA rubber powder, including but not limited to 20, 22, 25, 28, 30, 32, 34, and 35 parts, preferably 25 to 35 parts.
[0063] In some embodiments, the polystyrene content of the ASA rubber powder is 35% to 40% by weight. Such ASA rubber powder can provide the composite material with better low-temperature toughness, weather resistance, and anti-squeak properties. It is understood that in the present invention, the polystyrene content of the ASA rubber powder includes, but is not limited to, 35%, 35.5%, 36%, 36.5%, 37%, 37.5%, 38%, 38.5%, 39%, 39.5%, and 40% by weight.
[0064] In some embodiments, the average particle size of the ASA rubber powder is 100 nm to 300 nm. Such ASA rubber powder can provide the composite material with better low-temperature toughness, weather resistance, and anti-squeak properties. It is understood that the average particle size of the ASA rubber powder includes, but is not limited to, 100 nm, 120 nm, 150 nm, 180 nm, 200 nm, 220 nm, 250 nm, 280 nm, and 300 nm.
[0065] In some embodiments, the ASA rubber powder is Kumho Petrochemical XC540, with a polystyrene content of 38% by mass and an average particle size of 300 nm.
[0066] In some embodiments, the ASA rubber powder 2 is Donghai Chemical 600sm-1, with a polystyrene content of 40% by mass and an average particle size of 200nm;
[0067] In some embodiments, the ASA rubber powder 3 is Donghai Chemical Q100, with a polystyrene content of 35% by mass and an average particle size of 100 nm.
[0068] In the present invention, SAN resin is a copolymer of styrene and polyacrylonitrile. It is a colorless, transparent, and mechanically strong polypropylene-based engineering plastic that primarily functions as a dispersant and toughening agent. The ASA / ABS composite material can contain 50 to 75 parts of SAN resin by weight, including but not limited to 50, 55, 60, 65, 70, and 75 parts, preferably 50 to 65 parts.
[0069] In some embodiments, the polystyrene content of the SAN resin is 70% to 75% by weight. Such SAN resin can provide the composite material with better low-temperature toughness, weather resistance, and anti-squeak properties. It is understood that in the present invention, the polystyrene content of the SAN resin includes, but is not limited to, 70%, 70.5%, 71%, 71.5%, 72%, 72.5%, 73%, 73.5%, 74%, 74.5%, and 75% by weight.
[0070] In some embodiments, the SAN resin is LG 80HF, and the mass content of polystyrene is 75%.
[0071] In some embodiments, the SAN resin is Kumho Petrochemical SAN 350, and the mass content of polystyrene is 70%.
[0072] It can be understood that in the present invention, the ASA / ABS composite material contains 2 to 6 parts of the anti-sounding agent by weight, including but not limited to 2 parts, 3 parts, 4 parts, 5 parts and 6 parts, preferably 3 to 5 parts.
[0073] In some embodiments, the anti-squeaking agent is selected from vinyl copolymers and / or styrene copolymers. Such an anti-squeaking agent can make the composite material have better anti-squeaking properties.
[0074] Furthermore, the vinyl copolymer is selected from one or more of ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-octene copolymer, ethylene-maleic anhydride copolymer, ethylene-styrene-maleic anhydride copolymer, ethylene-propylene-maleic anhydride copolymer and ethylene-octene-maleic anhydride copolymer; the styrene-based copolymer is selected from one or more of acrylonitrile-styrene-acrylate copolymer, acrylonitrile-styrene-butadiene copolymer, acrylonitrile-styrene-ethylene propylene rubber copolymer, acrylate-styrene-butadiene copolymer, styrene-ethylene-styrene copolymer, styrene-hydrogenated ethylene-styrene copolymer, styrene-ethylene-butylene-styrene copolymer and styrene-hydrogenated ethylene-styrene-maleic anhydride copolymer.
[0075] In some embodiments, the anti-squeak additive is ethylene-octene copolymer POE 7447, which is purchased from Dow.
[0076] In some embodiments, the ASA / ABS composite material further comprises one or more of a weathering agent, an antioxidant, a lubricant, and a color powder.
[0077] The inventors have discovered that polybutadiene rubber contains unsaturated double bonds, which easily break open under light to form other substances, causing the material to yellow. By optimizing the combination of ASA and weathering agents, ABS can be protected to avoid a decrease in weather resistance. Therefore, by appropriately controlling the combination ratio of ABS / ASA and weathering agents, the low-temperature toughness, weather resistance and noise prevention of ASA / ABS composite materials can be optimized.
[0078] In some embodiments, the ASA / ABS composite material contains 0.5 to 6 parts of weathering agent by weight, including but not limited to 0.5 parts, 0.6 parts, 0.8 parts, 1 part, 1.5 parts, 1.8 parts, 2 parts, 2.5 parts, 2.8 parts, 3 parts, 3.5 parts, 3.8 parts, 4 parts, 4.5 parts, 4.8 parts, 4 parts, 4.5 parts, 4.8 parts and 6 parts, preferably 3 to 5 parts.
[0079] In some embodiments, the weathering agent is selected from benzotriazole light stabilizers and / or triazine ultraviolet light absorbers. Further, the benzotriazole light stabilizer is selected from one or more of 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)-benzotriazole and 2-hydroxy-4-n-octyloxybenzophenone; the triazine ultraviolet light absorber is selected from one or more of 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxy-phenol, 2-(2-hydroxy-4-malonic acid diacetyloxyphenyl)-4,6-diphenyl-1,3,5-triazine and 2-(2-hydroxy-4-malonic acid diacetyloxyphenyl)-4,6-di(4,-methyl)phenyl-1,3,5-triazine.
[0080] In some embodiments, the weathering agent is a combination of benzotriazole and triazine, purchased from BASF.
[0081] In some embodiments, the ASA / ABS composite material further comprises 0.1 to 2 parts of an antioxidant, by weight, including but not limited to 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 and 2 parts. Preferably, it is 0.3 to 1 part.
[0082] In some embodiments, the antioxidant is selected from one or more of organic phosphates, alkylated monophenols, alkylated polyphenols, alkylation reaction products of polyphenols and dienes, butylation reaction products of p-cresol or dicyclopentadiene, alkylated hydroquinones, hydroxylated thiodiphenyl ethers, alkylidene bisphenols, benzyl compounds, esters of β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid and monohydric or polyhydric alcohols, esters of β-(5-tert-butyl-4-hydroxy-3-methylphenyl)-propionic acid and monohydric or polyhydric alcohols, esters of sulfanyl compounds, esters of sulfaryl compounds, and amides of β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid.
[0083] Furthermore, the organic phosphate is one or more selected from tris(nonylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, di(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, and distearyl pentaerythritol diphosphite. The alkylation reaction product of the polyphenol and the diene is selected from tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane; the ester of the sulfanyl compound is selected from one or more selected from distearylthiopropionate, dilaurylthiopropionate, and di(tridecyl)thiopropionate; and the ester of the sulfaryl compound is selected from octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)thiopropionate and pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)]thiopropionate.
[0084] In some embodiments, the antioxidant is tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane, which is purchased from Sanfeng Chemical.
[0085] In some embodiments, the ASA / ABS composite material further comprises 0.1 to 2 parts of a lubricant, in parts by weight, including but not limited to 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 and 2 parts, preferably 0.3 to 1 part.
[0086] In some embodiments, the lubricant is selected from one or more of zinc stearate, calcium stearate, magnesium stearate, polyethylene wax, EVA wax, oleamide, erucamide, ethylene bisstearamide, silicone lubricant and pentaerythritol stearate.
[0087] In some embodiments, the lubricant is pentaerythritol stearate, which is purchased from Warsaw.
[0088] In some embodiments, the ASA / ABS composite material further includes 0.1 to 2 parts of color powder, including but not limited to 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1 part, 1.1 part, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts and 2 parts, preferably 0.1 to 1 part.
[0089] In some embodiments, the toner is selected from pigments and / or dye additives.
[0090] Furthermore, the pigment is selected from inorganic pigments and / or organic pigments. The inorganic pigment is selected from metal oxides and mixed metal oxides such as zinc oxide, titanium dioxide, iron oxide, etc.; sulfides such as zinc sulfide, etc.; aluminates; sodium thiosilicates, sulfates, chromates, etc.; carbon black; zinc ferrite; ultramarine blue; Pigment Brown 24; Pigment Red 101; Pigment Yellow 119; the organic pigment is selected from azo, diazo, quinacridone, perylene, naphthalene tetracarboxylic acid, flavanone, isoindolinone, tetrachloroisoindolinone, anthraquinone, anthracene diquinone, dioxazine, phthalocyanine, azo lake, Pigment Blue 60, Pigment Red 122, Pigment Red 149, Pigment Red 177, Pigment Red 179, Pigment Red 202, Pigment White 29, Pigment Blue 15, Pigment Green 7, Pigment Yellow 147 and Pigment Yellow 150, or a combination comprising at least one of the foregoing pigments. Preferred inorganic pigments are one or more selected from carbon black, ferric oxide (ie, iron red) and titanium dioxide.Suitable dyes may be organic materials, for example coumarin dyes such as coumarin 460 (blue), coumarin 6 (green), Nile red light; lanthanide complexes; hydrocarbon and substituted hydrocarbon dyes; polycyclic aromatic hydrocarbon dyes; scintillating dyes such as oxazole or oxadiazole dyes; aryl or heteroaryl substituted poly (C2-8) olefin dyes; carbocyanine dyes; indanthrone dyes; phthalocyanine dyes; oxazine dyes; quinolone dyes; naphthalenetetracarboxylic acid dyes; porphyrin dyes; distyryl biphenyl dyes; acridine dyes; anthraquinone dyes; cyanine dyes; methine dyes; arylmethane dyes; azo dyes; indigoid dyes. dyes, thioindigo dyes; diazo dyes; nitro dyes; quinoneimine dyes; aminoketone dyes; tetrazolium dyes; thiazole dyes; perylene dyes; perylone dyes; bis-benzoxazolylthiophene; triarylmethane dyes; thioxanthene dyes; naphthalimide dyes; lactone dyes; fluorophores, such as anti-Stokes shift dyes, which absorb in the near infrared and emit in the visible; luminescent dyes, such as 7-amino-4-methylcoumarin; 3-(2'-benzothiazolyl)-7-diethylaminocoumarin; 2-(4-biphenyl)-5-(4-tert-butylphenyl)-1,3,4-dimethylthiophene; -oxadiazole; 2,5-di-(4-biphenyl)-oxazole; 2,2'-dimethyl-p-quaterphenyl; 2,2'-dimethyl-p-terphenyl; 3,5,3",5"-tetra-tert-butyl-p-pentaphenyl; 2,5-diphenylfuran; 2,5-diphenyloxazole; 4,4'-diphenylstilbene; 4-dicyanomethylethylene-2-methyl-6-(p-dimethylaminophenyl)-4H-pyran; 1,1'-diethyl-2,2'-carbocyanine iodide; 3,3'-diethyl-4,4',5,5'-dibenzothiotriene. Carbocyanine iodide; 7-dimethylamino-1-methyl-4-methoxy-8-azaquinolone-2-one; 7-dimethylamino-4-methylquinolone-2-one; 2-(4-(4-dimethylaminophenyl))-1,3-butadienyl)-3-ethylbenzothiazole perchlorate; 3-diethylamino-7-diethyliminophenoxazole perchlorate; 2-(1-naphthyl)-5-phenyloxazole; 2,2'-p-phenylene-bis(5-phenyloxazole); Rhodamine 700; Rhodamine 800; pyrene; 1,2-triphenylene; rubrene; coronene, etc.
[0091] In some embodiments, the ASA / ABS composite material includes the following components in parts by weight:
[0092]
[0093] The mass content of polybutadiene in the ABS resin is 12% to 18%.
[0094] In some embodiments, the ASA / ABS composite material includes the following components in parts by weight:
[0095]
[0096]
[0097] The mass content of polybutadiene in the ABS resin is 12% to 18%.
[0098] In some embodiments, the ASA / ABS composite material includes the following components in parts by weight:
[0099]
[0100] The mass content of polybutadiene in the ABS resin is 12% to 18%.
[0101] In some embodiments, the ASA / ABS composite material includes the following components in parts by weight:
[0102]
[0103] The mass content of polybutadiene in the ABS resin is 12% to 18%.
[0104] The present invention also provides a method for preparing the ASA / ABS composite material as described above, comprising the following steps:
[0105] The ASA rubber powder, ABS resin, SAN resin and anti-sounding auxiliary agent are blended and extruded.
[0106] In some embodiments, the blending temperature is 15°C to 30°C.
[0107] In some embodiments, the extrusion temperature is 200°C to 240°C.
[0108] In some embodiments, the method for preparing the ASA / ABS composite material comprises the following steps:
[0109] Mix SAN resin, ASA rubber powder, ABS resin, anti-squeak additive (and other additives such as weathering agent, antioxidant, lubricant and color powder) in a certain proportion, then put them into a twin-screw extruder for blending and extrusion into granules. The extrusion temperature is 200℃~240℃, and the screw speed is 300r / min~1000r / min.
[0110] In one embodiment, after extrusion, the extruded product is cooled and pelletized.
[0111] The present invention also provides an automobile part, comprising the ASA / ABS composite material as described above, or the ASA / ABS composite material prepared according to the preparation method as described above.
[0112] In one embodiment, the vehicle part is selected from one or more of a rearview mirror housing, a spare tire cover, a bumper trim, and a vehicle body trim.
[0113] The present invention also provides a vehicle comprising the vehicle parts described above. It is understood that the vehicle described in the present invention includes but is not limited to a car, a truck, a motorcycle, a tricycle, a bicycle and a toy car.
[0114] The following is a specific embodiment:
[0115] (1) Raw material description:
[0116] 1.SAN resin:
[0117] SAN resin 1: LG, 80HF, polystyrene content of 75% by mass;
[0118] SAN resin 2: Kumho Petrochemical SAN 350, with a polystyrene content of 70% by mass.
[0119] ②ASA rubber powder:
[0120] ASA rubber powder 1: Kumho Petrochemical, XC540, polystyrene content is 38% by mass, and the average particle size is 300 nm.
[0121] ASA rubber powder 2: Donghai Chemical, 600sm-1, polystyrene content of 40%, average particle size of 200nm;
[0122] ASA rubber powder 3: Donghai Chemical, Q100, the mass content of polystyrene is 35%, and the average particle size is 100nm.
[0123] ③ABS resin:
[0124] ABS resin 1: Chimei 757, average rubber phase particle size of 200 nm, polybutadiene mass content of 14%;
[0125] ABS resin 2: Homemade, blended with SAN 80HF and Kumho Petrochemical ABS high-rubber powder HR181 at a mass ratio of 70:30, with an average rubber phase particle size of 400 nm and a polybutadiene content of 18%;
[0126] ABS resin 3: Sinopec, ABS 275, average rubber phase particle size of 800nm, polybutadiene mass content of 12%;
[0127] ABS resin 4: Homemade, blended with SAN 80HF and Kumho Petrochemical ABS high-rubber powder HR192 at a mass ratio of 70:30, with an average rubber phase particle size of 50 nm and a polybutadiene content of 15%;
[0128] ABS resin 5: Dagu DG-MG94, the average particle size of the rubber phase is 200 nm, and the mass content of polybutadiene is 10%.
[0129] ⑤Anti-noise additives:
[0130] Anti-squeaking agent 1: ethylene-octene copolymer POE 7447, Dow;
[0131] Anti-squeaking agent 2: styrene-ethylene-butylene-styrene copolymer, 7551, Li Changrong.
[0132] ⑥ Weathering agent: BASF, TINUVIN 234, low volatility benzotriazole UV absorber.
[0133] ⑦Antioxidant: Tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane, Sanfeng Chemical.
[0134] ⑧Lubricant: Pentaerythritol stearate, Warsaw. (2) Specific embodiments:
[0136] Example 1:
[0137] This embodiment provides an ASA / ABS composite material and a preparation method thereof, which are specifically as follows:
[0138] (1) The ASA / ABS composite material provided in this embodiment is composed of the following components in parts by weight:
[0139]
[0140] (2) The preparation method of the ASA / ABS composite material provided in this embodiment is as follows:
[0141] SAN resin 1, ASA rubber powder 1, ABS resin 1, anti-squeak additive 1, weathering agent, lubricant and antioxidant were mixed uniformly in proportion, and then put into a twin-screw extruder for blending, extrusion and granulation. The extrusion temperature was 220°C and the screw speed was 600 r / min to obtain an ASA / ABS composite material 1.
[0142] Examples 2 to 15 and Comparative Examples 1 to 6
[0143] The formulations of the ASA / ABS composite materials in Examples 2 to 15 and Comparative Examples 1 to 6 are shown in Tables 1 to 3 below. The amounts of the raw materials added are in parts by weight. The preparation methods are similar to those in Example 1.
[0144] Table 1
[0145]
[0146]
[0147] Table 2
[0148]
[0149]
[0150] Table 3
[0151]
[0152] The performance tests of the ASA / ABS composite materials prepared in Examples 1 to 19 and Comparative Examples 1 to 6 were performed using the following test methods:
[0153] 1) Squeak / Noise Reduction: Tested according to VDA 230-206, with a force of 40N and a speed of 4mm / s. This standard uses a RPN scale of 1 to 10. RPN = 1 to 3 indicates squeak / noise reduction; RPN = 4 to 6 indicates moderate noise; and RPN = 7 to 10 indicates high noise.
[0154] 2) Weathering Resistance: The test was conducted according to SAE J 2527 for 1600 hours. After testing, the grayscale of the sample's appearance was evaluated according to GB250, which has a grayscale range of 1-5. A grayscale of 4 or higher was considered acceptable, while a grayscale of less than 4 was considered unacceptable. Lower values indicate poorer weathering resistance.
[0155] 3) Low-temperature toughness: The test is conducted according to ISO 180, 1eA notch, sample size 100mmx10mmx4mm, pendulum force 2.75J, temperature at -30℃, and notched impact strength is tested.
[0156] The test results are shown in Table 2 below:
[0157] Table 2
[0158]
[0159]
[0160] As shown in Table 2, after adding appropriate amounts of specific ABS resin in Examples 1 to 19, the RPN of the ASA / ABS composite materials obtained in each Example is 1 to 3, showing excellent anti-squeaking performance; after 1600 hours of weathering test, the appearance grayscale of the product is above level 4, showing excellent weather resistance; the notched impact strength at -30°C can reach 1.7 kJ / m 2 Above, some can reach 7.5kJ / m 2, showing excellent low-temperature toughness. In particular, when the rubber particle size combination of ABS resin is 200nm and 400nm, the ASA / ABS composite material has excellent low-temperature toughness, and the overall performance of weather resistance, anti-squeak characteristics and toughness is optimal.
[0161] Compared to Example 1, Comparative Example 1, which added a small amount of anti-squeak additive and an appropriate amount of ABS resin, achieved high low-temperature notched impact strength, but poor anti-squeak and weather resistance. Comparative Example 2, which added an excessive amount of anti-squeak additive and a small amount of ABS resin, showed improved anti-squeak and low-temperature notched impact strength, but poor weather resistance. Comparative Example 3, which added an excessive amount of ABS resin, achieved high low-temperature notched impact strength and excellent toughness, but sacrificed both weather resistance and anti-squeak properties. Comparative Example 4, which added an excessive amount of SAN resin, exhibited poor anti-squeak, weather resistance, and toughness. Comparative Example 5 also added an appropriate amount of ABS, but the polybutadiene content was outside the scope of the present invention, making it difficult to effectively improve the toughness of the composite material. Comparative Example 6, which added an excessive amount of ASA rubber powder, struggled to achieve a balanced balance of weather resistance, anti-squeak, and toughness. In summary, the amounts of each raw material and the type of ABS used significantly impact the weather resistance, anti-squeak, and toughness of the composite material.
[0162] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0163] The above-described embodiments merely illustrate several implementations of the present invention, and while their descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.
Claims
1. An ASA / ABS composite material, It is characterized in that The composition comprises the following components in parts by weight: The mass content of polybutadiene in the ABS resin is 12% to 18%; The average particle size of the rubber phase of the ABS resin is 50nm to 800nm; The anti-sounding auxiliary agent is selected from vinyl copolymers and / or styrene-based copolymers; The vinyl copolymer is selected from one or more of ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-octene copolymer, ethylene-maleic anhydride copolymer, ethylene-styrene-maleic anhydride copolymer, ethylene-propylene-maleic anhydride copolymer and ethylene-octene-maleic anhydride copolymer; The styrene-based copolymer is selected from one or more of acrylonitrile-styrene-acrylate copolymer, acrylonitrile-styrene-butadiene copolymer, acrylonitrile-styrene-ethylene-propylene rubber copolymer, acrylate-styrene-butadiene copolymer, styrene-ethylene-styrene copolymer, styrene-hydrogenated ethylene-styrene copolymer, styrene-ethylene-butylene-styrene copolymer and styrene-hydrogenated ethylene-styrene-maleic anhydride copolymer.
2. The ASA / ABS composite material according to claim 1, It is characterized in that The composition comprises the following components in parts by weight:
3. The ASA / ABS composite material according to claim 1 or 2, It is characterized in that The average particle size of the rubber phase of the ABS resin is 200nm to 400nm.
4. The ASA / ABS composite material according to claim 1 or 2, It is characterized in that The average particle size of the ASA rubber powder is 100nm to 300nm.
5. The ASA / ABS composite material according to claim 1 or 2, It is characterized in that The mass content of polystyrene in the ASA rubber powder is 35% to 40%.
6. The ASA / ABS composite material according to claim 1 or 2, It is characterized in that The mass content of polystyrene in the SAN resin is 70% to 75%.
7. The ASA / ABS composite material according to claim 1 or 2, It is characterized in that Also includes one or more of weathering agent, antioxidant, lubricant and toner; The weathering agent is selected from benzotriazole light stabilizers and / or triazine ultraviolet light absorbers; The antioxidant is selected from one or more of organic phosphates, alkylated monophenols, alkylated polyphenols, alkylation reaction products of polyphenols and dienes, butylation reaction products of p-cresol or dicyclopentadiene, alkylated hydroquinones, hydroxylated thiodiphenyl ethers, alkylidene bisphenols, benzyl compounds, esters of β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid and monohydric alcohols or polyhydric alcohols, esters of β-(5-tert-butyl-4-hydroxy-3-methylphenyl)-propionic acid and monohydric alcohols or polyhydric alcohols, esters of sulfanyl compounds, esters of sulfaryl compounds, and amides of β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid; The lubricant is selected from one or more of zinc stearate, calcium stearate, magnesium stearate, polyethylene wax, EVA wax, oleic acid amide, erucic acid amide, ethylene bis stearic acid amide, silicone lubricant and pentaerythritol stearate; The toner is selected from pigments and / or dye additives.
8. The ASA / ABS composite material according to claim 7, It is characterized in that In parts by weight, the ASA / ABS composite material further comprises 0.5 to 6 parts of a weathering agent, 0.1 to 2 parts of an antioxidant and 0.1 to 2 parts of a lubricant.
9. A method for preparing the ASA / ABS composite material according to any one of claims 1 to 8, It is characterized in that The steps include: The components are blended and extruded.
10. The method for preparing the ASA / ABS composite material according to claim 9, It is characterized in that The extrusion temperature is 200°C to 240°C.
11. A car part, It is characterized in that The invention relates to an ASA / ABS composite material comprising the ASA / ABS composite material according to any one of claims 1 to 8, or an ASA / ABS composite material prepared according to the preparation method according to claim 9 or 10.