A plant-based negative oxygen ion coating and preparation method thereof
A plant-based negative oxygen ion coating using natural emulsions and ion slurry addresses the environmental impact of petrochemical coatings by forming low-odor films and purifying indoor air, enhancing scrub resistance and health benefits.
Patent Information
- Application Number
- CN202310887501.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-07-19
AI Technical Summary
Existing architectural coatings rely on non-renewable petrochemical products, leading to high carbon emissions and air pollution during the painting process, and lack the ability to purify indoor air effectively.
A plant-based negative oxygen ion coating using natural emulsions from plants like vegetable oil and starch, combined with negative oxygen ion slurry, to form films without volatile organic compounds and release ions that purify indoor air.
The coating achieves low-carbon, low-odor film formation with enhanced scrub resistance, fast hardness build-up, and effective indoor air purification, improving health and reducing pollutants like formaldehyde and VOCs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to but is not limited to the field of plant-based coatings, and in particular to but is not limited to plant-based negative oxygen ion coatings and preparation methods thereof. Background Art
[0002] At present, the base materials used in architectural coatings on the market, such as ethyl acetate emulsions and acrylic emulsions, are mostly petrochemical products from petroleum cracking. As the source of petrochemical products, petroleum is a non-renewable resource. It takes millions of years to form, and a large amount of carbon emissions and polluting products are generated in the actual mining and production process, which are slowly harming people's daily lives. In order to seek sustainable development, actively developing renewable bio-based materials and transforming to a low-carbon economy are inevitable strategies for solving global environmental problems and long-term human development. The Chinese coatings industry plan also mentions the need to "develop bio-based renewable monomers and resins to replace carbon-based monomers and synthetic resins to promote the sustainable development of the coatings industry." Therefore, bio-based products are a major trend in the development of architectural coatings in the future.
[0003] For architectural coatings, bio-based materials are mainly bio-based emulsions, while taking into account the selection of low-carbon emission pigments, fillers and additives. Bio-based materials have the advantages of being green, low-carbon, and renewable raw materials. In recent years, bio-based emulsion interior wall coatings have developed rapidly in the Chinese market, and related products have gradually been recognized by consumers. With the improvement of living standards, consumers' environmental awareness and the concept of environmental sustainable development are also gradually deepening and understanding. Therefore, architectural coatings should not only have good performance and decorative effects, but also have good environmental protection effects and sustainable development effects. Summary of the invention
[0004] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0005] The present invention discloses a plant-based negative oxygen ion paint and a preparation method thereof. The emulsion is sourced from plants such as vegetable oil, starch, and beet. The film-forming temperature is low, and there is no need to add a film-forming aid that is easily volatile to organic compounds (VOCs). In addition, negative oxygen ions are specially added to purify indoor air to solve the problem in the prior art that latex paint relies on non-renewable petroleum cracking products, and releases acrylic acid small molecule monomers and various auxiliary volatiles during the painting process, causing air pollution.
[0006] The present disclosure provides a plant-based negative oxygen ion paint, which includes, by weight: 300 to 500 parts of plant-based emulsion, 20 to 100 parts of negative oxygen ion slurry, 30 to 100 parts of hollow microspheres, 200 to 300 parts of pigment, 80 to 250 parts of water, and 1 to 10 parts of non-ionic surfactant.
[0007] In some embodiments provided in the present disclosure, the plant-based negative oxygen ion coating includes, by weight: 300 to 400 parts of plant-based emulsion, 30 to 60 parts of negative oxygen ion slurry, 50 to 80 parts of hollow microspheres, 200 to 250 parts of pigment, 100 to 200 parts of water, and 2 to 7 parts of non-ionic surfactant.
[0008] In some embodiments provided by the present disclosure, the plant-based negative oxygen ion coating includes, by weight: 300 to 500 parts of plant-based emulsion, 20 to 100 parts of negative oxygen ion slurry, 30 to 100 parts of hollow microspheres, 200 to 300 parts of pigments, 80 to 250 parts of water, 1 to 10 parts of non-ionic surfactants, 2 to 6 parts of defoaming agents, 3 to 10 parts of dispersants, 2 to 5 parts of pH adjusters, 3 to 10 parts of antifreeze-thaw agents, 0 to 50 parts of formaldehyde removers, 0 to 100 parts of fillers, 1 to 10 parts of thickeners, and 20 to 50 parts of hydrophobic agents.
[0009] In some embodiments provided by the present disclosure, the plant-based negative oxygen ion coating includes, by weight: 300 to 400 parts of plant-based emulsion, 30 to 60 parts of negative oxygen ion slurry, 50 to 80 parts of hollow microspheres, 200 to 250 parts of pigment, 100 to 200 parts of water, 2 to 7 parts of non-ionic surfactant, 3 to 5 parts of defoaming agent, 5 to 8 parts of dispersant, 2 to 4 parts of pH adjuster, 4 to 8 parts of antifreeze-thaw agent, 0 to 30 parts of formaldehyde remover, 0 to 90 parts of filler, 3 to 8 parts of thickener, and 20 to 40 parts of hydrophobic agent.
[0010] In some embodiments provided by the present disclosure, the plant-based emulsion is any one or more of a plant-based pure acrylic emulsion, a plant-based styrene acrylic emulsion, and a plant-based acetic acid acrylic emulsion.
[0011] In some embodiments provided in the present disclosure, the pigment is any one or more of rutile titanium dioxide and anatase titanium dioxide.
[0012] In some embodiments provided by the present disclosure, the negative oxygen ion slurry includes tourmaline powder, nano titanium dioxide crystal colloid, mixed rare earth containing lanthanide elements, scandium, yttrium and water, and the particle size of the tourmaline powder is 20-30nm;
[0013] The tourmaline powder accounts for 60-70 wt.% of the negative oxygen ion slurry.
[0014] In some embodiments provided by the present disclosure, the hollow microspheres are polymethacrylic acid-divinylbenzene hollow microspheres.
[0015] In some embodiments provided by the present disclosure, the defoaming agent is selected from any one or more of silicone-based defoaming agents and mineral oil-based defoaming agents.
[0016] In some embodiments provided by the present disclosure, the dispersant is selected from any one or more of a modified polyacrylic acid dispersant and a modified polycarboxylate dispersant.
[0017] In some embodiments provided in the present disclosure, the modified polyacrylic acid dispersant is modified by grafting hydrophilic polymer side chains on the basis of a polyacrylate auxiliary agent; the modified polycarboxylate dispersant is modified by introducing an organosilicon reagent with excellent hydrolysis resistance during the polymerization reaction of a sulfonic acid compound and an antelope acid monomer.
[0018] In some embodiments provided by the present disclosure, the pH adjuster is selected from any one or more of an alkali metal pH adjuster, an alcohol ammonia pH adjuster, and a silanol pH adjuster.
[0019] In some embodiments provided by the present disclosure, the antifreeze-thaw agent is selected from any one or more of alcohol antifreeze solvents and alcohol ether antifreeze solvents.
[0020] In some embodiments provided by the present disclosure, the formaldehyde scavenger is titanium dioxide.
[0021] In some embodiments provided in the present disclosure, the filler is a non-calcined filler. Considering that the carbon emissions of calcined fillers during the production process are very large, ranging from 500kg / t to 700kg / t, while the carbon emissions of non-calcined fillers during the production process are relatively small, ranging from 10kg / t to 20kg / t.
[0022] In some embodiments provided by the present disclosure, the filler is selected from any one or more of wet-process sericite powder and talc powder.
[0023] In some embodiments provided in the present disclosure, the thickener is selected from any one or more of hydroxyethyl cellulose, modified bentonite, nano-gas-phase silica thickener, alkali swelling thickener, polyurethane thickener and hydroxyethyl cellulose; the modified bentonite is sodium-modified by using NaF, Na2CO3, NaCl and the like to replace the calcium ions in the bentonite solid layer.
[0024] In some embodiments provided by the present disclosure, the hydrophobic agent is selected from one or both of a wax emulsion or a silicone-modified polysiloxane emulsion.
[0025] In some embodiments provided by the present disclosure, the nonionic surfactant is selected from any one or more of phenolic polyoxyethylene ether and alkyl polyoxyethylene ether.
[0026] In another aspect, the present disclosure provides a method for preparing the above-mentioned plant-based negative oxygen ion coating, the preparation method comprising:
[0027] 1) mixing water, a thickener, a dispersant, a defoamer, a nonionic surfactant and an antifreeze-thaw agent to obtain a first mixed solution;
[0028] 2) mixing the pigment, filler, and formaldehyde scavenger with the first mixed solution to obtain a second mixed solution;
[0029] 3) mixing the pH regulator and the defoaming agent with the second mixed solution to obtain a third mixed solution;
[0030] 4) mixing the plant-based emulsion, hollow microspheres, thickener and hydrophobic agent with the third mixed solution to obtain the plant-based negative oxygen ion coating;
[0031] In some embodiments provided by the present disclosure, the weight ratio of the defoaming agent in step 1) to the defoaming agent in step 3) is 1:(1.5 to 2.5);
[0032] In some embodiments provided by the present disclosure, the weight ratio of the thickener in step 1) to the thickener in step 4) is 1:(2.5 to 3.5);
[0033] In some embodiments provided by the present disclosure, the first mixing at least satisfies: a stirring rate of 300 to 500 rpm, and a mixing time of 5 to 10 minutes;
[0034] In some embodiments provided in the present disclosure, the second mixing at least satisfies: the stirring rate is 1500 rpm to 1800 rpm, and the mixing time is 15 minutes to 20 minutes; in some embodiments provided in the present disclosure, the end of the second mixing is marked by the particle size of the second mixed liquid being less than 50 μm.
[0035] In some embodiments provided by the present disclosure, the third mixing at least meets: a stirring rate of 900 to 1000 rpm, and a mixing time of 3 to 5 minutes;
[0036] In some embodiments provided by the present disclosure, the fourth mixing at least meets: a stirring rate of 600 to 800 rpm, and a mixing time of 10 to 17 minutes.
[0037] In some embodiments provided in the present disclosure, the fourth mixing includes: mixing the plant-based emulsion with the hollow microspheres and then mixing with a thickener, and then mixing with a hydrophobic agent after the thickener is fully swollen to a viscosity change rate close to 0.
[0038] The plant-based emulsion is an emulsion with water as the dispersion medium, which is obtained by polymerization reaction of polymerizable monomers obtained by transformation from plants as raw materials, for example, an emulsion with water as the dispersion medium is obtained by using plant oil, corn starch, cassava starch, corn starch, beet and other plants as basic raw materials. The plant-based emulsion belongs to a water-based emulsified alkyd polymer or a water-based dispersed polymer. The emulsion with water as the dispersion medium is obtained by polymerization reaction of polymerizable monomers obtained by transformation from plants, and is an environmentally friendly chemical product.
[0039] Compared with the prior art, the present invention has the following advantages:
[0040] 1) Use natural plant-based emulsions instead of acrylic emulsions, which are petrochemical products with high carbon emissions and are non-renewable:
[0041] The present invention discloses a plant-based coating using a plant-based emulsion as a main film-forming substance, with various pigments, fillers and additives added thereto to produce a plant-based coating having excellent scrub resistance, outstanding low-temperature film-forming properties, fast early hardness build-up, excellent anti-powdering properties and good stain resistance, and is a green, environmentally friendly, low-carbon product.
[0042] 2) No film-forming aid is used:
[0043] Film-forming aids promote the formation of latex paint films, but they will slowly evaporate in the entire film-forming process and are one of the main sources of VOC in paints. The formula provided by the present disclosure does not require the addition of volatile film-forming aids, and has no odor during production and construction, making it very safe and environmentally friendly.
[0044] 3) Add negative oxygen ions to purify indoor gas, which is beneficial to personal health:
[0045] When the indoor negative oxygen ion content increases, it will improve people's own immunity and resistance to viruses, reduce disease transmission, and enhance the self-repair ability of human cells. The present invention specifically adds negative oxygen ion slurry, which has the characteristics of high concentration and high release. The released negative oxygen ions can effectively decompose toxic and harmful gases such as formaldehyde, toluene, VOC, etc., effectively improve indoor air pollution, purify and maintain indoor air health.
[0046] Other features and advantages of the present disclosure will be described in the following description, and partly become apparent from the description, or be understood by implementing the present disclosure. Other advantages of the present disclosure can be invented and obtained by the schemes described in the description. DETAILED DESCRIPTION
[0047] To make the purpose, technical solution and advantages of the present disclosure more clear, the embodiments of the present disclosure are described in detail below. It should be noted that the embodiments and features in the embodiments of the present disclosure can be combined with each other arbitrarily without conflict.
[0048] The present disclosure will be described in detail below through examples.
[0049] In the following examples, the plant-based emulsion is selected from Archsol 8177, a pure propylene plant-based emulsion produced by Wanhua Chemical Company.
[0050] The negative oxygen ion slurry is selected from the negative ion paint additive produced by Guangdong Shunde Biang Negative Ion New Materials Co., Ltd. or the paint negative ion additive produced by Guilin Hsinchu Nature Biomaterials Co., Ltd. The negative oxygen ion slurry includes tourmaline powder, nano titanium dioxide crystal colloid, mixed rare earth and water. The weight ratio of the negative oxygen ion slurry including tourmaline powder, nano titanium dioxide crystal colloid, mixed rare earth and water is (75 to 78): (2 to 4): (3 to 5): (15 to 20); the particle size of the tourmaline powder is 20nm to 30nm; the mixed rare earth contains lanthanide elements, scandium and yttrium.
[0051] The hollow microspheres are selected from hollow microsphere emulsion ULTRA-E produced by Dow Chemical, which is a polymethacrylic acid-divinylbenzene hollow microsphere with a solid content of 30±0.5%.
[0052] Defoamer 1 is selected from SN-Defoamer 154, a silicone defoamer with high efficiency in foam suppression produced by San Nopco; and defoamer 2 is selected from FoamStar 2410, a mineral oil defoamer with high efficiency in foam breaking produced by BASF.
[0053] The dispersant is selected from modified polycarboxylate sodium salt dispersant 731A produced by Dow Chemical.
[0054] The pH regulator is selected from the alcohol-ammonia pH regulator AMP-95 produced by Angus Company.
[0055] The antifreeze-thaw agent is selected from the alcohol ether antifreeze solvent ZT5110 produced by Solvay.
[0056] The titanium dioxide formaldehyde removal agent is selected from the formaldehyde removal powder FC100 provided by Coneo Trading (Shanghai) Co., Ltd.
[0057] The pigment is selected from rutile titanium dioxide R-996 produced by Sichuan Longmang Titanium Industry Co., Ltd.
[0058] The filler is selected from wet-process sericite powder GM900 of Ge Rui Mining and talc powder MS425 produced by Guangfu Building Materials (Jiaoling) Refining Co., Ltd.
[0059] Thickener 1 is an alkali swelling thickener TT-935 produced by The Dow Chemical Company, and thickener 2 is a polyurethane thickener RM-8W produced by The Dow Chemical Company.
[0060] The hydrophobic agent is the silicone-modified polysiloxane emulsion BS1306 produced by Wacker Chemicals, which can improve the water repellency, water resistance and hydrophobicity of architectural coatings.
[0061] The nonionic surfactant is selected from the wetting agent PE100 produced by German Koning Company, and its component is alkyl polyoxyethylene ether.
[0062] Example 1
[0063] A. Raw material preparation: 350g plant-based emulsion, 40g negative oxygen ion slurry, 60g hollow microspheres, 1.5g defoamer 1, 2.5g defoamer 2, 6g dispersant, 2g thickener 1, 5g thickener 2, 2.5g pH regulator, 4g antifreeze-thaw agent, 30g formaldehyde remover, 230g pigment, 70g filler, 30g hydrophobic agent, 163.5g deionized water, 3g nonionic surfactant;
[0064] B. Product preparation: 1) Adjust the speed of the disperser to 300 to 500 rpm, and slowly add water, thickener TT-935, dispersant, defoamer SN-Defoamer154, nonionic surfactant and antifreeze-thaw agent in sequence under stirring, add the materials while stirring, and stir for 5 to 10 minutes after the addition is completed to obtain a mixed solution.
[0065] 2) Add pigment R-258, sericite powder GM900, talcum powder MS425 and formaldehyde remover TF100 to the mixed solution of step 1) in sequence, and gradually increase the speed of the disperser according to the viscosity of the slurry while adding the materials. After all the materials are added, the speed is increased to 1800 rpm, and the mixture is dispersed for 15 to 20 minutes to obtain the mixed solution. Test the fineness index of the mixed solution, and proceed to the next step if the fineness is less than 50 μm.
[0066] 3) Add defoamer FoamStar 2410 to the mixed solution obtained in step 2), and stir at a speed of 900 to 1000 rpm for 3 to 5 minutes. After sufficient defoaming, add pH adjuster and stir for 1 minute.
[0067] 4) Adjust the disperser to 600 rpm to 800 rpm, add the plant-based emulsion and hollow microspheres, stir for 1 minute to mix evenly, then slowly add the thickener RM-8W, stir for 10 to 15 minutes, allow the thickener to fully swell until the viscosity change rate is close to 0, then slowly add the hydrophobic agent, continue stirring for 1 minute, and obtain the plant-based negative oxygen ion coating.
[0068] Example 2
[0069] A. Raw material preparation: 300g plant-based emulsion, 30g negative oxygen ion slurry, 60g hollow microspheres, 1.5g defoamer 1, 2.5g defoamer 2, 6g dispersant, 2g thickener 1, 5g thickener 2, 2.5g pH regulator, 4g antifreeze-thaw agent, 30g formaldehyde remover, 210g pigment, 90g filler, 30g hydrophobic agent, 223.5g deionized water, 3g non-ionic surfactant;
[0070] B. The preparation method of this embodiment is the same as that of embodiment 1.
[0071] Example 3
[0072] A. Raw material preparation: 380g plant-based emulsion, 50g negative oxygen ion slurry, 60g hollow microspheres, 1.5g defoamer 1, 2.5g defoamer 2, 6g dispersant, 2g thickener 1, 5g thickener 2, 2.5g pH regulator, 4g antifreeze-thaw agent, 30g formaldehyde remover, 250g pigment, 50g filler, 30g hydrophobic agent, 123.5g deionized water, 3g nonionic surfactant;
[0073] B. The preparation method of this embodiment is the same as that of embodiment 1.
[0074] Example 4
[0075] A. Raw material preparation: 350g plant-based emulsion, 40g negative oxygen ion slurry, 60g hollow microspheres, 1.5g defoamer 1, 2.5g defoamer 2, 6g dispersant, 2g thickener 1, 5g thickener 2, 2.5g pH regulator, 4g antifreeze-thaw agent, 0g formaldehyde remover, 230g pigment, 70g filler, 30g hydrophobic agent, 193.5g deionized water, 3g non-ionic surfactant;
[0076] B. The preparation method of this embodiment is the same as that of embodiment 1.
[0077] Example 5
[0078] A. Raw material preparation: 350g plant-based emulsion, 40g negative oxygen ion slurry, 60g hollow microspheres, 1.5g defoamer 1, 2.5g defoamer 2, 6g dispersant, 2g thickener 1, 5g thickener 2, 2.5g pH regulator, 4g antifreeze-thaw agent, 15g formaldehyde remover, 230g pigment, 70g filler, 30g hydrophobic agent, 178.5g deionized water, 3g nonionic surfactant;
[0079] B. The preparation method of this embodiment is the same as that of embodiment 1.
[0080] Comparative Example 1
[0081] The difference between this comparative example and Example 1 is that petrochemical acrylic resin emulsion is used to replace the plant-based emulsion, and the other preparation processes and raw material types and amounts are exactly the same. The petrochemical acrylic resin emulsion is purchased from the model RS-939W acrylic emulsion produced by Badfu Company.
[0082] Comparative Example 2
[0083] The difference between this comparative example and Example 2 is that petrochemical acrylic resin emulsion (manufacturer model is the same as that of comparative example 1) is used to replace the plant-based emulsion, and other preparation processes and raw material types and amounts are exactly the same.
[0084] Comparative Example 3
[0085] The only difference between this comparative example and Example 3 is that petrochemical acrylic resin emulsion (manufacturer model is the same as that of comparative example 1) is used to replace the plant-based emulsion, and the other preparation processes and raw material types and amounts are exactly the same.
[0086] Effect test:
[0087] 1. Performance comparison
[0088] The main quality technical index inspection standards of the coatings prepared in Examples 1 to 5 and the odorless latex paint coatings of Comparative Examples 1 to 3 are based on the Chinese national standard GB / T9756-2018 "Synthetic Resin Emulsion Interior Wall Paints", and the test results are shown in Table 1.
[0089] Table 1 Performance results comparison
[0090]
[0091] 2. Comparison of environmental protection indicators
[0092] The environmental protection technical index inspection standards of the coatings obtained in Examples 1 to 5 and the odorless latex paint coatings of Comparative Examples 1 to 3 are based on the Chinese national standard GB18582-2020 "Limits of Hazardous Substances in Building Wall Coatings", and the test results are shown in Table 2.
[0093] Table 2 Comparison of environmental protection test results
[0094]
[0095]
[0096] 3. Comparison of formaldehyde purification efficiency
[0097] The formaldehyde purification performance test of the coatings prepared in Examples 1 to 5 and the odorless latex paint coatings of Comparative Examples 1 to 3 is based on the technical index requirements of Class I IS-W of China's building materials industry standard JCT1074-2021 "Purification Performance of Indoor Air Purification Functional Coating Materials", and the formaldehyde purification efficiency and purification durability are tested.
[0098] Table 3 Comparison of formaldehyde purification effects
[0099] Inspection items Formaldehyde purification efficiency / (%) Formaldehyde purification durability (C3) / (%) National Standards ≥80 ≥70 Example 1 97.8 88.5 Example 2 92.1 82.6 Example 3 98.1 89.2 Example 4 83.2 75.5 Example 5 90.1 78.8 Comparative Example 1 89.5 78.2 Comparative Example 2 88.7 75.0 Comparative Example 3 89.2 76.9
[0100] 4. Comparison of negative ion concentration
[0101] The coatings prepared in Examples 1 to 5 and the odorless latex paints of Comparative Examples 1 to 3 were tested according to the Chinese building materials industry standard JC / T2040-2010 "Negative ion functional building interior decoration materials" to record the negative ion release concentration.
[0102] Table 4 Comparison of negative ion concentration
[0103]
[0104] From the comparison of the performance results in Table 1, it can be seen that the scrubbing resistance of Examples 1 to 5 is more than 41,000 times, which is much greater than the 8,000-10,000 scrubbing resistance data of Comparative Examples 1 to 3. This is because plant-based emulsions can form films naturally as long as the ambient temperature is greater than 3 degrees Celsius, while most petrochemical acrylic resin emulsions need the help of film-forming aids to form films well, and film-forming aids are also one of the main sources of VOC. Comparing Examples 1 to 3, the contrast ratio of Example 1 is preferably 0.97. The performance of Comparative Examples 1 to 3 is close to that of Examples 1 to 3.
[0105] From the comparison of the environmental protection test results in Table 2, it can be seen that the environmental protection of Examples 1 to 5 is very good, and VOC, benzene, formaldehyde, total lead content, soluble heavy metals, and the total content of alkylphenol polyoxyethylene ether are all undetectable. However, VOC and formaldehyde are detected in the latex paints of Comparative Examples 1 to 3.
[0106] From the comparison of formaldehyde purification efficiency in Table 3, it can be seen that the formaldehyde purification function of Examples 1 to 5 is slightly better than that of Comparative Examples 1 to 3. This may be due to the better environmental performance of the plant-based emulsion and its synergy with the formaldehyde remover.
[0107] From the comparison of negative ion concentrations in Table 4, it can be seen that the Chinese national standard requires that the negative ion release concentration be ≥500 (pieces / s.cm 2), Examples 1 to 5 all have release amounts greater than 9000, and the release period is long. The release amount of Example 3 is the highest, followed by Example 1, and the effect of Example 2 is relatively poor. This is because in the formulas of Examples 1-5, the amount of negative oxygen ion slurry added in Example 2 is the lowest, and the amount of oxygen ion slurry added in Example 3 is the highest. The negative ion release concentration of Comparative Examples 1-3 is also higher than the Chinese national standard, but is slightly worse than that of Examples 1-3.
[0108] Therefore, considering the physical properties, environmental protection, formaldehyde removal performance, and negative ion release concentration of the product, it can be seen that the performance of plant-based negative oxygen ion paint is better than that of the odor-free latex paint products on the market. The formaldehyde removal and odor removal technology of the plant-based emulsion in the plant-based negative oxygen ion paint, the formaldehyde removal and odor removal technology of the formaldehyde removal agent, and the odor removal technology of the negative oxygen ion slurry, combined with the reasonable ratio of non-calcined pigments and fillers, have created very good physical and environmental performance of the product.
Claims
1. A plant-based negative oxygen ion coating, characterized in that: In parts by weight, the plant-based negative oxygen ion coating comprises: 300 to 500 parts of plant-based emulsion, 20 to 100 parts of negative oxygen ion slurry, 30 to 100 parts of hollow microspheres, 200 to 300 parts of pigment, 80 to 250 parts of water, and 1 to 10 parts of non-ionic surfactant; The plant-based emulsion is pure propylene plant-based emulsion Archsol 8177; The negative oxygen ion slurry includes tourmaline powder, nano titanium dioxide crystal colloid, mixed rare earth and water in a weight ratio of (75 to 78): (2 to 4): (3 to 5): (15 to 20); the mixed rare earth contains lanthanide elements, scandium and yttrium.
2. The plant-based negative oxygen ion coating according to claim 1, characterized in that: In parts by weight, the plant-based negative oxygen ion paint includes: 300 to 400 parts of plant-based emulsion, 30 to 60 parts of negative oxygen ion slurry, 50 to 80 parts of hollow microspheres, 200 to 250 parts of pigment, 100 to 200 parts of water, and 2 to 7 parts of non-ionic surfactant.
3. The plant-based negative oxygen ion coating according to claim 1, characterized in that: In parts by weight, the plant-based negative oxygen ion coating includes: 300 to 500 parts of plant-based emulsion, 20 to 100 parts of negative oxygen ion slurry, 30 to 100 parts of hollow microspheres, 200 to 300 parts of pigments, 80 to 250 parts of water, 1 to 10 parts of non-ionic surfactants, 2 to 6 parts of defoaming agents, 3 to 10 parts of dispersants, 2 to 5 parts of pH adjusters, 3 to 10 parts of antifreeze-thaw agents, 0 to 50 parts of formaldehyde removers, 0 to 100 parts of fillers, 1 to 10 parts of thickeners, and 20 to 50 parts of hydrophobic agents.
4. The plant-based negative oxygen ion coating according to claim 1, characterized in that: In parts by weight, the plant-based negative oxygen ion coating includes: 300 to 400 parts of plant-based emulsion, 30 to 60 parts of negative oxygen ion slurry, 50 to 80 parts of hollow microspheres, 200 to 250 parts of pigment, 100 to 200 parts of water, 2 to 7 parts of non-ionic surfactant, 3 to 5 parts of defoaming agent, 5 to 8 parts of dispersant, 2 to 4 parts of pH adjuster, 4 to 8 parts of antifreeze-thaw agent, 0 to 30 parts of formaldehyde remover, 0 to 90 parts of filler, 3 to 8 parts of thickener, and 20 to 40 parts of hydrophobic agent.
5. The plant-based negative oxygen ion coating according to any one of claims 1 to 4, characterized in that: The pigment is any one or more of rutile titanium dioxide and anatase titanium dioxide.
6. The plant-based negative oxygen ion coating according to any one of claims 1 to 4, characterized in that: The particle size of the tourmaline powder is 20nm to 30nm.
7. The plant-based negative oxygen ion coating according to any one of claims 1 to 4, characterized in that: The hollow microspheres are polymethacrylic acid-divinylbenzene hollow microspheres.
8. The plant-based negative oxygen ion coating according to claim 3 or 4, characterized in that: The defoaming agent is selected from any one or more of silicone-based defoaming agents and mineral oil-based defoaming agents.
9. The plant-based negative oxygen ion coating according to claim 3 or 4, characterized in that: The dispersant is selected from any one or more of a modified polyacrylic acid dispersant and a modified polycarboxylate dispersant.
10. The plant-based negative oxygen ion coating according to claim 3 or 4, characterized in that: The pH adjuster is selected from any one or more of an alkali metal pH adjuster, an alcohol ammonia pH adjuster and a silanol pH adjuster.
11. The plant-based negative oxygen ion coating according to claim 3 or 4, characterized in that: The antifreeze-thaw agent is selected from any one or more of alcohol antifreeze-thaw agents and alcohol ether antifreeze-thaw agents.
12. The plant-based negative oxygen ion coating according to claim 3 or 4, characterized in that: The filler is selected from any one or more of wet-process sericite powder and talc powder.
13. The plant-based negative oxygen ion coating according to claim 3 or 4, characterized in that: The thickener is selected from any one or more of hydroxyethyl cellulose, modified bentonite, nano-fumed silica thickener, alkali swelling thickener, and polyurethane thickener.
14. The plant-based negative oxygen ion coating according to claim 3 or 4, characterized in that: The hydrophobic agent is selected from any one or more of a wax emulsion and a silicone-modified polysiloxane emulsion.
15. The plant-based negative oxygen ion coating according to claim 3 or 4, characterized in that: The nonionic surfactant is selected from any one or more of phenolic polyoxyethylene ether and alkyl polyoxyethylene ether.
16. The method for preparing the plant-based negative oxygen ion coating according to any one of claims 3-4 and 8-15, characterized in that: The preparation method comprises: 1) performing a first mixing of the water, a portion of the thickener, the dispersant, a portion of the defoaming agent, the nonionic surfactant and the antifreeze-thaw agent to obtain a first mixed solution; 2) mixing the pigment, the filler, the formaldehyde remover and the first mixed solution to obtain a second mixed solution; 3) mixing the pH regulator, another portion of the defoaming agent and the second mixed solution to obtain a third mixed solution; 4) Mixing the plant-based emulsion, the hollow microspheres, the other part of the thickener and the hydrophobic agent with the third mixed liquid to obtain the plant-based negative oxygen ion coating.
17. The preparation method according to claim 16, characterized in that: The weight ratio of the defoaming agent in step 1) to the defoaming agent in step 3) is 1:(1.5 to 2.5).
18. The preparation method according to claim 16 or 17, characterized in that: The weight ratio of the thickener in step 1) to the thickener in step 4) is 1:(2.5 to 3.5).
19. The preparation method according to claim 16 or 17, characterized in that: The first mixing at least meets the following conditions: a stirring rate of 300 rpm to 500 rpm, and a mixing time of 5 minutes to 10 minutes.
20. The preparation method according to claim 16 or 17, characterized in that: The mixing in step 2) at least meets the following requirements: a stirring rate of 1500 to 1800 rpm, and a mixing time of 15 to 20 minutes.
21. The preparation method according to claim 20, characterized in that: The sign that the mixing in step 2) is completed is that the particle size in the second mixed liquid is less than 50 μm.
22. The preparation method according to claim 16 or 17, characterized in that: The mixing in step 3) at least meets the following requirements: a stirring rate of 900 to 1000 rpm and a mixing time of 3 to 5 minutes.
23. The preparation method according to claim 16 or 17, characterized in that: The mixing in step 3) includes: adding a pH regulator after the second mixed solution is fully defoamed by the defoaming agent.
24. The preparation method according to claim 16 or 17, characterized in that: The mixing in step 4) at least meets the following requirements: a stirring rate of 600 to 800 rpm, and a mixing time of 10 to 17 minutes.
25. The preparation method according to claim 16 or 17, characterized in that: The mixing in step 4) includes: mixing the plant-based emulsion with the hollow microspheres and then mixing with a thickener, and then mixing with a hydrophobic agent after the thickener is fully swollen to a viscosity change rate close to 0.