Foaming sound-absorbing shading antibacterial mildew-proof soft curtain and preparation method thereof

By setting a flame-retardant light-shielding layer, sound-insulating layer and printing layer in the curtains, combined with non-woven fabrics and polyester chemical fiber fabrics, the problem of mold and single function of soft curtains is solved, and flame-retardant, sound-absorbing, light-shielding, antibacterial and mildew-proof are achieved. Function and support for digital painting, improving convenience and health and safety.

CN119058174AActive Publication Date: 2024-12-03WEIFANG UNIVERSITY +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410989922.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-12-03
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing soft curtains are prone to mold when encountering continuous rainy weather, and cannot achieve digital printing, flame retardant and sound insulation functions, which are inconvenient to disassemble and clean, which affects the decorative effect and health and safety.

Method used

The non-woven fabric layer is combined with the polyester chemical fiber fabric layer, and a flame retardant light shielding layer, sound insulation layer and printing layer are arranged. The specific composition includes deionized water, acrylic resin, composite flame retardant, nano-grade titanium dioxide slurry, foaming agent and Thickener, supports a variety of printing methods such as UV, weak solvents and latex.

Benefits of technology

It realizes the flame retardant, sound absorption, light-shading, antibacterial and anti-mold functions of soft curtains, and supports digital spray painting, which improves the scrubbing and water swelling resistance, avoids the problem of hanging curling, and enhances the decorative effect and health and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119058174A_ABST
    Figure CN119058174A_ABST
Patent Text Reader

Abstract

The invention discloses a foaming sound-absorbing shading antibacterial mildew-proof soft curtain and a preparation method thereof, and belongs to the technical field of decorative materials. The foaming sound-absorbing shading antibacterial mildewproof soft curtain comprises a non-woven fabric layer, a polyester chemical fabric layer, a flame-retardant shading layer, a sound insulation layer and a printing layer. The flame-retardant shading layer, the sound insulation layer and the printing layer are arranged, and the composition of the flame-retardant shading layer, the sound insulation layer and the printing layer is specifically limited, so that the soft curtain has the functions of flame retardance, sound absorption, shading, antibiosis and mildew prevention, can be used for digital painting, and supports various printing modes such as UV, weak solvents and latex.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain and a preparation method thereof, and belongs to the technical field of decorative materials. Background Art

[0002] Curtains are made of cloth, bamboo, reed, hemp, yarn, plastic, metal and other materials to block or adjust indoor light. With the improvement of people's living standards, people have higher requirements for living environment. Curtains are the most common indoor necessities. In addition to decorative functions, they also have functions such as shading and heat absorption. Suitable curtains can significantly improve the indoor living environment.

[0003] In the prior art, soft curtains are mostly printed by silk screen printing, embroidery and other methods, and digital printing is not possible, which is inefficient and relatively simple. Continuous rainy weather can easily lead to mold, which not only loses the decorative effect, but also harms people's health. Once the curtains are installed, it is extremely inconvenient to disassemble and clean them.

[0004] Chinese patent CN115434158B provides a method for preparing antibacterial light-shielding curtain fabrics, which specifically discloses mixing menthol / folic acid / dopamine polymer micro-nano particles and polyacrylate emulsion, coating the surface of the curtain fabric, and giving the curtain fabric good antibacterial, UV protection and light-shielding properties. However, the curtain fabric cannot be digitally printed and does not have flame retardant and sound insulation functions. Summary of the invention

[0005] In order to solve the above problems, a foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain is provided. By arranging a flame-retardant light-shielding layer, a sound-insulating layer and a printing layer, and specifically limiting the components of the flame-retardant light-shielding layer, the sound-insulating layer and the printing layer, the soft curtain has the functions of flame-retardant, sound-absorbing, light-shielding, antibacterial and mildew-proof, and can be digitally sprayed, and supports multiple printing methods, such as UV, eco-solvent, latex, etc.

[0006] According to one aspect of the present application, a foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain is provided, comprising a non-woven fabric layer, a polyester chemical fiber fabric layer, a flame-retardant light-shielding layer, a sound-insulating layer and a printing layer;

[0007] In terms of weight, the flame retardant light-shielding layer includes 10-20 parts of deionized water, 30-40 parts of acrylic resin, 20-30 parts of compound flame retardant, 20-30 parts of nano-grade titanium dioxide slurry, 0.5-1.5 parts of foam stabilizer, 0.5-1.5 parts of foaming agent, 3-6 parts of carbon black and 1-2 parts of thickener;

[0008] The sound insulation layer comprises 10-20 parts of deionized water, 30-40 parts of acrylic resin, 20-30 parts of nano-grade titanium dioxide slurry, 5-10 parts of foamed microspheres and 0.8-1.5 parts of thickener;

[0009] The printing layer comprises 10-15 parts of deionized water, 30-40 parts of acrylic acid mixed emulsion, 30-40 parts of compound dispersion liquid, 0.5-1 part of defoamer, 0.5-1.5 parts of brightener, 0.5-2 parts of crosslinking agent and 0.5-1.5 parts of thickener.

[0010] Optionally, the acrylic mixed emulsion includes tg-40°C pure acrylic acid and tg-20°C special fluororesin copolymer anionic emulsion, and the mass ratio of the tg-40°C acrylic acid to the tg-20°C special fluororesin copolymer anionic emulsion is 1:(0.8~1.2).

[0011] Optionally, the compound dispersion liquid comprises water, ultrafine silica, polytetrafluoroethylene emulsion, defoamer, dispersant, mildew preventer and antibacterial agent; the mass ratio of water, ultrafine silica, polytetrafluoroethylene emulsion, defoamer, dispersant, mildew preventer and antibacterial agent is (55-65): (15-25): (5-15): (0.5-3): (0.5-2): (1-5): (2-7); the particle size of the ultrafine silica is 10-20 um.

[0012] Optionally, the composite flame retardant comprises water, decabromodiphenylethane, antimony trioxide and a dispersant, and the mass ratio of the water, decabromodiphenylethane, antimony trioxide and the dispersant is (20-40): (35-45): (15-25): (5-15).

[0013] Optionally, the foamed microspheres are obtained by copolymerizing acrylonitrile, methyl methacrylate, butyl methacrylate and hydroxyethyl methacrylate as comonomers through suspension polymerization, the foaming agent used in the copolymerization is low-boiling point isopentane, and the dispersant is magnesium hydroxide.

[0014] Specifically, the specific preparation method of foamed microspheres can be found in the literature Plastics Industry 2023, 51(09), 156-162.

[0015] Optionally, the acrylic resin is -35°C pure acrylic resin;

[0016] The thickener is a star-shaped polyurethane thickener;

[0017] The nano-scale titanium dioxide slurry comprises rutile titanium dioxide with a solid content of 60-65%;

[0018] The foam stabilizer is a fluorocarbon anionic surfactant;

[0019] The defoamer is polyether modified silicone oil;

[0020] The cross-linking agent is trimethylolpropane trimethacrylate;

[0021] The brightener is of stilbene triazine type;

[0022] The foaming agent is polyoxyethylene ether sulfate;

[0023] The dispersant is fatty alcohol polyoxyethylene ether ester sulfonate or fatty alcohol polyoxyethylene ether;

[0024] The non-woven fabric layer is a 70g fully cross non-woven fabric; the polyester chemical fiber fabric layer is 150D / 96F, black and white yarn cross-woven with an inch density of 50*50, and the weight of the polyester chemical fiber fabric layer is 140gsm / m 2 .

[0025] Optionally, the mildew inhibitor is isothiazolinone; and the antibacterial agent is nano-scale copper zinc ions.

[0026] According to another aspect of the present application, a method for preparing the above-mentioned foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain is also provided, comprising the following steps:

[0027] (1) Laminating the non-woven fabric layer and the polyester chemical fiber fabric layer at a laminating temperature of 150-170°C;

[0028] (2) According to weight proportions, 10-20 parts of deionized water, 30-40 parts of acrylic resin, 20-30 parts of compound flame retardant, 20-30 parts of nano-grade titanium dioxide slurry, 0.5-1.5 parts of foam stabilizer, 0.5-1.5 parts of foaming agent, 3-6 parts of carbon black and 1-2 parts of thickener are mixed and stirred, and the pH is adjusted to 7-8, the viscosity is 6000-8000cps / 4#30R, and the foaming ratio is 2-4 times to obtain a flame retardant light-shielding layer coating; the flame retardant light-shielding layer coating is suspended and coated on the surface of the polyester chemical fiber cloth layer, and dried to obtain a flame retardant light-shielding layer;

[0029] (3) Mixing 10-20 parts of deionized water, 30-40 parts of acrylic resin, 20-30 parts of nano-grade titanium dioxide slurry, 5-10 parts of foamed microspheres and 0.8-1.5 parts of thickener according to weight, adjusting the pH to 7-8 and the viscosity to 10000-12000cps / 4#30R to obtain a sound insulation layer coating; applying the sound insulation layer coating on the surface of the flame retardant light shielding layer, and drying to obtain a sound insulation layer;

[0030] (4) According to the weight proportions, 10-15 parts of deionized water, 30-40 parts of acrylic mixed emulsion, 30-40 parts of compounded dispersion, 0.5-1 part of defoaming agent, 0.5-1.5 parts of brightener, 0.5-2 parts of crosslinking agent and 0.5-1.5 parts of thickener are mixed and stirred, and the pH value is adjusted to 7-8 and the viscosity is 6000-8000cps / 4#30R to obtain a printing layer coating; the printing layer coating is evenly scraped and applied on the surface of the sound insulation layer with a flat knife, and dried to obtain a foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain.

[0031] Optionally, the drying in step (2), step (3) and step (4) are all carried out in a nine-section oven; the temperature of the nine-section oven drying in step (2) is: 70-80° C. in the first section oven, 80-120° C. in the second section oven, 150-160° C. in the third, fourth, fifth, sixth, seventh and eighth sections ovens, and 70-90° C. in the ninth section oven;

[0032] The drying temperatures in the nine ovens in step (3) are: 70-80° C. in the first oven, 80-120° C. in the second, third, fourth, fifth, sixth, seventh and eighth ovens, and 70-90° C. in the ninth oven;

[0033] The drying temperatures of the nine ovens in step (4) are: 70-80°C for the first oven, 80-120°C for the second oven, 150-160°C for the third, fourth, fifth, sixth, seventh and eighth ovens, and 70-90°C for the ninth oven.

[0034] Optionally, the vehicle speed in step (1) is 10-20 m / min;

[0035] In step (2), the vehicle speed is 10-20 m / min; the flame retardant light-shielding layer has a dry weight of 50-60 g and a thickness of 100-200 um;

[0036] In step (3), the vehicle speed is 5-15 m / min; the dry weight of the sound insulation layer is 50-60 g, and the coating thickness is 200-300 um;

[0037] In step (4), the vehicle speed is 10-20 m / min; the dry weight of the printed layer is 10-20 g, and the coating thickness is 30-50 um.

[0038] The beneficial effects of this application include but are not limited to:

[0039] 1. According to the foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain of the present application, by setting a flame-retardant light-shielding layer, a sound-insulating layer, and a printing layer, and specifically limiting the component composition of the flame-retardant light-shielding layer, the sound-insulating layer, and the printing layer, the soft curtain has the functions of flame-retardant, sound-absorbing, light-shielding, antibacterial and mildew-proof, and can be digitally sprayed, supporting multiple printing methods, such as UV, eco-solvent, latex, etc.

[0040] 2. According to the foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain of the present application, the printing layer adopts TG-40℃ pure acrylic acid and TG-20℃ special fluororesin copolymer anionic emulsion to form an acrylic mixed emulsion in a specific proportion. Since acrylic acid is a water-based emulsion, it swells after being damp, and then shrinks after air drying, which can easily cause hanging and curling, affecting the use and appearance. The TG-20℃ special fluororesin copolymer anionic emulsion is compounded with acrylic acid in a specific proportion. On the one hand, it can realize scrubbing of stains and sewage on the soft curtain and effectively improve the scrub resistance. On the other hand, it can achieve water swelling resistance, solving the problem of hanging and curling of the soft curtain after being damp.

[0041] 3. According to the foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain of the present application, nano-scale copper-zinc ions are used as antibacterial agents. On the one hand, copper ions can participate in the generation of hydroxyl radicals with strong oxidizing properties. The generated hydroxyl radicals can attack the cell membranes, nucleic acids and proteins of bacteria, thereby causing the inactivation of cell components and killing bacteria; on the other hand, when inside bacterial cells, copper ions can attack the cell membranes, nucleic acids and proteins of bacteria, thereby causing the inactivation of cell components and killing bacteria. Copper ions have very good antibacterial effects at room temperature and can complete the antibacterial task without special conditions; at the same time, zinc ions also have antibacterial effects. Adding zinc ions not only reduces costs, but also provides a wider range of sterilization performance; isothiazolinone is used as a mildew preventer, which can achieve long-term resistance to bacteria, yeasts and molds, and improve the antibacterial and mildew-proof effects.

[0042] 4. According to the foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain of the present application, the flame-retardant light-shielding layer is compounded by decabromodiphenylethane and antimony trioxide to obtain a bromine antimony flame retardant, which effectively achieves a flame retardant effect. A foaming agent is added for foaming treatment to increase the thickness of the flame-retardant light-shielding layer and improve the light-shielding effect. The sound insulation layer is prepared by a suspension polymerization method to obtain low-temperature thermal expansion foamed microspheres with a low starting foaming temperature, and a non-woven fabric layer and a polyester chemical fiber fabric layer are bonded to improve the sound absorption effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0044] Figure 1 This is a schematic diagram of the cross-sectional structure of the foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain involved in an embodiment of the present application.

[0045] List of parts and reference numerals:

[0046] 1. Non-woven fabric layer; 2. Polyester chemical fiber fabric layer; 3. Flame retardant light-shielding layer; 4. Sound insulation layer; 5. Printing layer. DETAILED DESCRIPTION

[0047] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0048] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in this patent are for demonstration purposes only.

[0049] refer to Figure 1 The embodiment of the present application discloses a foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain, which includes, from bottom to top, a non-woven fabric layer 1, a polyester chemical fiber fabric layer 2, a flame-retardant light-shielding layer 3, a sound-insulating layer 4 and a printing layer 5, so that the soft curtain has the functions of flame-retardant, sound-absorbing, light-shielding, antibacterial and mildew-proof, and can be digitally sprayed, supporting multiple printing methods, such as UV, eco-solvent, latex, etc.

[0050] Example 1

[0051] (1) A 70g fully cross nonwoven fabric layer is cross-woven with 150D / 96F black and white yarn with an inch density of 50*50 to produce a 140gsm / m 2 The polyester chemical fiber fabric layer is bonded by a bonding machine at a bonding temperature of 150°C, with white latex as the bonding glue and a speed of 10m / min;

[0052] (2) According to weight proportions, 10 parts of deionized water, 30 parts of -35°C pure acrylic resin, 20 parts of compound flame retardant, 20 parts of nano-grade titanium dioxide paste, 0.5 parts of foam stabilizer carbon fluoride anion surfactant, 0.5 parts of foaming agent polyoxyethylene ether sulfate, 3 parts of carbon black and 1 part of star-shaped polyurethane thickener are mixed and stirred, wherein the nano-grade titanium dioxide paste comprises rutile titanium dioxide with a solid content of 60-65%, the compound flame retardant comprises water, decabromodiphenylethane, antimony trioxide and dispersant fatty alcohol polyoxyethylene ether sulfonate, water, decabromodiphenylethane, antimony trioxide and dispersant fatty alcohol polyoxyethylene ether sulfonate, The mass ratio of oxyethylene ether ester sulfonate is 20:35:15:5, the pH is adjusted to 7, the viscosity is 6000cps / 4#30R, and the foaming ratio is 2 times to obtain a flame retardant light-shielding layer coating; the flame retardant light-shielding layer coating is suspended and coated on the surface of the polyester chemical fiber cloth layer, and the temperature of the nine-section oven drying is: 70°C in the first section oven, 80°C in the second section oven, 150°C in the third, fourth, fifth, sixth, seventh and eighth sections ovens, and 70°C in the ninth section oven to obtain a flame retardant light-shielding layer; the vehicle speed is 10m / min, the dry weight of the flame retardant light-shielding layer is 50g, and the thickness is 100um;

[0053] (3) According to weight parts, 10 parts of deionized water, 30 parts of -35°C pure acrylic resin, 20 parts of nano-grade titanium dioxide paste, 5 parts of foamed microspheres and 0.8 parts of star-shaped polyurethane thickener are mixed and stirred, wherein the nano-grade titanium dioxide paste includes rutile titanium dioxide with a solid content of 60%, the foamed microspheres are obtained by suspension polymerization of acrylonitrile, methyl methacrylate, butyl methacrylate and hydroxyethyl methacrylate as copolymer monomers, the foaming agent used in the copolymerization is low-boiling point isopentane, and the dispersant is hydroxide Magnesium, the expansion ratio of the foamed microspheres is 5 times, the pH is adjusted to 7, the viscosity is 10000cps / 4#30R, and a sound insulation layer coating is obtained; the sound insulation layer coating is suspended and coated on the surface of the flame retardant light shielding layer, and the temperature of the nine-section oven drying is: 70°C in the first section, 80°C in the second, third, fourth, fifth, sixth, seventh and eighth sections, and 70°C in the ninth section to obtain a sound insulation layer; the vehicle speed is 5m / min, the dry weight of the sound insulation layer is 50g, and the coating thickness is 200um;

[0054] (4) According to the weight ratio, 10 parts of deionized water, 30 parts of acrylic mixed emulsion, 30 parts of compound dispersion, 0.5 parts of defoaming agent polyether modified silicone oil, 0.5 parts of whitening agent distilben triazine type, 0.5 parts of cross-linking agent trimethylolpropane trimethacrylate and 0.5 parts of star-shaped polyurethane thickener are mixed and stirred. The acrylic mixed emulsion includes tg-40℃ pure acrylic acid and tg-20℃ special fluororesin copolymer anionic emulsion, and the mass ratio of tg-40℃ acrylic acid to tg-20℃ special fluororesin copolymer anionic emulsion is 1:0.8. The compound dispersion includes water, ultrafine silica, polytetrafluoroethylene emulsion, defoaming agent polyether modified silicone oil, dispersant fatty alcohol polyoxyethylene ether ester sulfonate, mildew inhibitor isothiazolinone and antibacterial agent nano-copper zinc ion; water, ultrafine silica The mass ratio of silicon dioxide, polytetrafluoroethylene emulsion, defoaming agent polyether modified silicone oil, dispersant fatty alcohol polyoxyethylene ether sulfonate, mildew inhibitor isothiazolinone and antibacterial agent nano-copper zinc ion is 55:15:5:0.5:0.5:1:2, and the particle size of ultrafine silica is 10um; the pH is adjusted to 7, and the viscosity is 6000cps / 4#30R to obtain a printing layer coating; the printing layer coating is evenly scraped on the surface of the sound insulation layer with a flat knife, and the drying temperature of the nine-section oven is: 70℃ in the first section oven, 80℃ in the second section oven, 150℃ in the third, fourth, fifth, sixth, seventh and eighth sections oven, 70℃ in the ninth section oven, and the vehicle speed is 10m / min; the dry weight of the printing layer is 10g, and the coating thickness is 30um; a foaming sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain is obtained.

[0055] Example 2

[0056] (1) A 70g fully cross nonwoven fabric layer is cross-woven with 150D / 96F black and white yarn with an inch density of 50*50 to produce a 140gsm / m 2 The polyester chemical fiber fabric layer is bonded by a bonding machine at a bonding temperature of 170°C, with white latex as the bonding glue and a speed of 20m / min;

[0057] (2) According to weight percentage, 20 parts of deionized water, 40 parts of -35°C pure acrylic resin, 30 parts of compound flame retardant, 30 parts of nano-grade titanium dioxide paste, 1.5 parts of foam stabilizer carbon fluoride anion surfactant, 1.5 parts of foaming agent polyoxyethylene ether sulfate, 6 parts of carbon black and 2 parts of star-shaped polyurethane thickener are mixed and stirred, wherein the nano-grade titanium dioxide paste comprises rutile titanium dioxide with a solid content of 60-65%, the compound flame retardant comprises water, decabromodiphenylethane, antimony trioxide and dispersant fatty alcohol polyoxyethylene ether, water, decabromodiphenylethane, antimony trioxide and dispersant fatty alcohol polyoxyethylene ether, The mass ratio of vinyl ether is 40:45:25:15, the pH is adjusted to 8, the viscosity is 8000cps / 4#30R, the foaming ratio is 4 times, and a flame retardant light-shielding layer coating is obtained; the flame retardant light-shielding layer coating is suspended and coated on the surface of the polyester chemical fiber cloth layer, and the temperature of the nine-section oven drying is: 80°C in the first section oven, 120°C in the second section oven, 160°C in the third, fourth, fifth, sixth, seventh and eighth sections ovens, and 90°C in the ninth section oven to obtain a flame retardant light-shielding layer; the vehicle speed is 20m / min, the dry weight of the flame retardant light-shielding layer is 60g, and the thickness is 200um;

[0058] (3) According to weight proportions, 20 parts of deionized water, 40 parts of -35°C pure acrylic resin, 30 parts of nano-grade titanium dioxide paste, 10 parts of foamed microspheres and 1.5 parts of star-shaped polyurethane thickener are mixed and stirred, wherein the nano-grade titanium dioxide paste comprises rutile titanium dioxide with a solid content of 65%, the foamed microspheres are obtained by suspension polymerization of acrylonitrile, methyl methacrylate, butyl methacrylate and hydroxyethyl methacrylate as copolymer monomers, the foaming agent used in the copolymerization is low-boiling point isopentane, and the dispersant is magnesium hydroxide. , the expansion ratio of the foamed microspheres is 5 times, the pH is adjusted to 8, the viscosity is 12000cps / 4#30R, and the sound insulation layer coating is obtained; the sound insulation layer coating is suspended and coated on the surface of the flame retardant light shielding layer, and the temperature of the nine-section oven drying is: 80°C in the first section, 120°C in the second, third, fourth, fifth, sixth, seventh and eighth sections, and 90°C in the ninth section to obtain the sound insulation layer; the vehicle speed is 15m / min, the dry weight of the sound insulation layer is 60g, and the coating thickness is 300um;

[0059] (4) According to the weight proportions, 15 parts of deionized water, 40 parts of acrylic mixed emulsion, 40 parts of compound dispersion, 1 part of defoaming agent polyether modified silicone oil, 1.5 parts of whitening agent distilben triazine type, 2 parts of cross-linking agent trimethylolpropane trimethacrylate and 1.5 parts of star-shaped polyurethane thickener are mixed and stirred, wherein the acrylic mixed emulsion comprises tg-40℃ pure acrylic acid and tg-20℃ special fluororesin copolymer anionic emulsion, and the mass ratio of tg-40℃ acrylic acid to tg-20℃ special fluororesin copolymer anionic emulsion is 1:1.2; the compound dispersion comprises water, ultrafine silica, polytetrafluoroethylene emulsion, defoaming agent polyether modified silicone oil, dispersant fatty alcohol polyoxyethylene ether, mildewproof agent isothiazolinone and antibacterial agent nano-copper zinc ion; water, ultrafine silica The mass ratio of silicon, polytetrafluoroethylene emulsion, defoaming agent polyether modified silicone oil, dispersant fatty alcohol polyoxyethylene ether, mildew inhibitor isothiazolinone and antibacterial agent nano-copper zinc ion is 65:25:15:3:2:5:7, and the particle size of ultrafine silica is 20um; the pH is adjusted to 8, and the viscosity is 8000cps / 4#30R to obtain a printing layer coating; the printing layer coating is evenly scraped on the surface of the sound insulation layer with a flat knife, and the drying temperature of the nine-section oven is: 80℃ in the first section oven, 120℃ in the second section oven, 160℃ in the third, fourth, fifth, sixth, seventh and eighth sections oven, 90℃ in the ninth section oven, and the vehicle speed is 20m / min; the dry weight of the printing layer is 20g, and the coating thickness is 50um; a foaming sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain is obtained.

[0060] Example 3

[0061] (1) A 70g fully cross nonwoven fabric layer is cross-woven with 150D / 96F black and white yarn with an inch density of 50*50 to produce a 140gsm / m 2 The polyester chemical fiber fabric layer is bonded by a bonding machine at a bonding temperature of 150°C, with white latex as the bonding glue and a speed of 15m / min;

[0062] (2) According to weight proportions, 15 parts of deionized water, 35 parts of -35°C pure acrylic resin, 25 parts of compound flame retardant, 25 parts of nano-grade titanium dioxide paste, 1 part of foam stabilizer carbon fluoride anion surfactant, 1 part of foaming agent polyoxyethylene ether sulfate, 5 parts of carbon black and 1 part of star-shaped polyurethane thickener are mixed and stirred, wherein the nano-grade titanium dioxide paste comprises rutile titanium dioxide with a solid content of 60-65%, the compound flame retardant comprises water, decabromodiphenylethane, antimony trioxide and dispersant fatty alcohol polyoxyethylene ether, water, decabromodiphenylethane, antimony trioxide and dispersant fatty alcohol polyoxyethylene ether The mass ratio of ether is 30:40:20:10, the pH is adjusted to 7, the viscosity is 6000cps / 4#30R, and the foaming ratio is 3 times to obtain a flame retardant light-shielding layer coating; the flame retardant light-shielding layer coating is suspended and coated on the surface of the polyester chemical fiber cloth layer, and the temperature of the nine-section oven drying is: 75°C in the first section oven, 100°C in the second section oven, 160°C in the third, fourth, fifth, sixth, seventh and eighth sections ovens, and 80°C in the ninth section oven to obtain a flame retardant light-shielding layer; the vehicle speed is 15m / min, the dry weight of the flame retardant light-shielding layer is 60g, and the thickness is 150um;

[0063] (3) According to weight proportions, 15 parts of deionized water, 35 parts of -35°C pure acrylic resin, 25 parts of nano-grade titanium dioxide paste, 8 parts of foamed microspheres and 1 part of star-shaped polyurethane thickener are mixed and stirred, wherein the nano-grade titanium dioxide paste comprises rutile titanium dioxide with a solid content of 63%, the foamed microspheres are obtained by suspension polymerization of acrylonitrile, methyl methacrylate, butyl methacrylate and hydroxyethyl methacrylate as copolymer monomers, the foaming agent used in the copolymerization is low-boiling-point isopentane, and the dispersant is magnesium hydroxide. The expansion ratio of the foamed microspheres is 5 times, the pH is adjusted to 7, and the viscosity is 10000cps / 4#30R to obtain a sound insulation layer coating; the sound insulation layer coating is suspended and coated on the surface of the flame retardant light shielding layer, and the temperature of the nine-section oven drying is: 75°C in the first section oven, 100°C in the second, third, fourth, fifth, sixth, seventh and eighth sections ovens, and 80°C in the ninth section oven to obtain a sound insulation layer; the vehicle speed is 10m / min, the dry weight of the sound insulation layer is 50g, and the coating thickness is 250um;

[0064] (4) According to the weight ratio, 10 parts of deionized water, 35 parts of acrylic mixed emulsion, 35 parts of compound dispersion, 1 part of defoaming agent polyether modified silicone oil, 1 part of whitening agent distilben triazine type, 1 part of cross-linking agent trimethylolpropane trimethacrylate and 1 part of star-shaped polyurethane thickener are mixed and stirred. The acrylic mixed emulsion includes tg-40℃ pure acrylic acid and tg-20℃ special fluororesin copolymer anionic emulsion, and the mass ratio of tg-40℃ acrylic acid to tg-20℃ special fluororesin copolymer anionic emulsion is 1:1. The compound dispersion includes water, ultrafine silica, polytetrafluoroethylene emulsion, defoaming agent polyether modified silicone oil, dispersant fatty alcohol polyoxyethylene ether ester sulfonate, mildew inhibitor isothiazolinone and antibacterial agent nano-copper zinc ion; water, ultrafine silica, The mass ratio of polytetrafluoroethylene emulsion, defoaming agent polyether modified silicone oil, dispersant fatty alcohol polyoxyethylene ether ester sulfonate, mildew inhibitor isothiazolinone and antibacterial agent nano-copper zinc ion is 60:20:10:1:1:3:5, and the particle size of ultrafine silica is 15um; the pH is adjusted to 7, the viscosity is 6000cps / 4#30R, and a printing layer coating is obtained; the printing layer coating is evenly scraped on the surface of the sound insulation layer with a flat knife, and the drying temperature of the nine-section oven is: 70°C in the first section oven, 80°C in the second section oven, 160°C in the third, fourth, fifth, sixth, seventh and eighth sections oven, 80°C in the ninth section oven, and the vehicle speed is 15m / min; the dry weight of the printing layer is 15g, and the coating thickness is 40um; a foaming sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain is obtained.

[0065] Comparative Example 1

[0066] The difference between Comparative Example 1 and Example 3 is that the antibacterial agent used in step (4) is a silver-based antibacterial agent, and the rest are the same.

[0067] Comparative Example 2

[0068] The difference between Comparative Example 2 and Example 3 is that the non-woven fabric layer is not included, and the rest is the same.

[0069] Comparative Example 3

[0070] The difference between Comparative Example 3 and Example 3 is that the acrylic acid mixed liquid does not include the tg-20°C special fluororesin copolymer anionic emulsion, and the rest are the same.

[0071] Comparative Example 4

[0072] The difference between Comparative Example 4 and Example 3 is that no brightener is added in step (4), and the rest are the same.

[0073] Comparative Example 5

[0074] The difference between Comparative Example 5 and Example 3 is that the mildew inhibitor isothiazolinone and the antibacterial agent nano-copper zinc ion are not added in step (4), and the rest are the same.

[0075] Comparative Example 6

[0076] The difference between Comparative Example 6 and Example 3 is that the compound flame retardant is replaced by the phosphorus-based flame retardant resorcinol bis(diphenyl phosphate), and the rest are the same.

[0077] Comparative Example 7

[0078] The difference between Comparative Example 7 and Example 3 is that the mass ratio of tg-40°C acrylic acid to tg-20°C special fluororesin copolymer anionic emulsion in the acrylic mixed emulsion is 2:1, and the rest are the same.

[0079] Experimental Example 1

[0080] The soft curtains prepared in Examples 1 to 3 and Comparative Examples 1 to 7 were subjected to performance tests, and the test results are shown in Table 1.

[0081] Table 1 Performance test results

[0082]

[0083]

[0084] The foamed sound-absorbing, light-shading, antibacterial and mildew-proof soft curtain provided in the present application has the functions of sound-absorbing, light-shading, antibacterial and mildew-proof and flame-retardant, and can be digitally printed, supports multiple printing methods, and has a high degree of sunlight resistance.

[0085] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.

Claims

1. A foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain, characterized in that: It includes a non-woven fabric layer, a polyester chemical fiber fabric layer, a flame retardant light-shielding layer, a sound insulation layer and a printing layer; In terms of weight, the flame retardant light-shielding layer includes 10-20 parts of deionized water, 30-40 parts of acrylic resin, 20-30 parts of compound flame retardant, 20-30 parts of nano-grade titanium dioxide slurry, 0.5-1.5 parts of foam stabilizer, 0.5-1.5 parts of foaming agent, 3-6 parts of carbon black and 1-2 parts of thickener; The sound insulation layer comprises 10-20 parts of deionized water, 30-40 parts of acrylic resin, 20-30 parts of nano-grade titanium dioxide slurry, 5-10 parts of foamed microspheres and 0.8-1.5 parts of thickener; The printing layer comprises 10-15 parts of deionized water, 30-40 parts of acrylic acid mixed emulsion, 30-40 parts of compound dispersion liquid, 0.5-1 part of defoamer, 0.5-1.5 parts of brightener, 0.5-2 parts of crosslinking agent and 0.5-1.5 parts of thickener.

2. The foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain according to claim 1, characterized in that: The acrylic mixed emulsion comprises tg-40°C pure acrylic acid and tg-20°C special fluororesin copolymer anionic emulsion, and the mass ratio of the tg-40°C acrylic acid to the tg-20°C special fluororesin copolymer anionic emulsion is 1:(0.8-1.2).

3. The foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain according to claim 1, characterized in that: The compound dispersion liquid comprises water, ultrafine silicon dioxide, polytetrafluoroethylene emulsion, defoamer, dispersant, mildew preventer and antibacterial agent; the mass ratio of water, ultrafine silicon dioxide, polytetrafluoroethylene emulsion, defoamer, dispersant, mildew preventer and antibacterial agent is (55-65): (15-25): (5-15): (0.5-3): (0.5-2): (1-5): (2-7); the particle size of the ultrafine silicon dioxide is 10-20 μm.

4. The foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain according to claim 3, characterized in that: The composite flame retardant comprises water, decabromodiphenylethane, antimony trioxide and a dispersant, wherein the mass ratio of the water, decabromodiphenylethane, antimony trioxide and the dispersant is (20-40): (35-45): (15-25): (5-15).

5. The foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain according to claim 1, characterized in that: The foaming microspheres are obtained by copolymerizing acrylonitrile, methyl methacrylate, butyl methacrylate and hydroxyethyl methacrylate as comonomers through suspension polymerization. The foaming agent used in the copolymerization is low-boiling-point isopentane, and the dispersant is magnesium hydroxide.

6. The foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain according to claim 4, characterized in that: The acrylic resin is -35°C pure acrylic resin; The thickener is a star-shaped polyurethane thickener; The nano-scale titanium dioxide slurry comprises rutile titanium dioxide with a solid content of 60-65%; The foam stabilizer is a fluorocarbon anionic surfactant; The defoamer is polyether modified silicone oil; The cross-linking agent is trimethylolpropane trimethacrylate; The brightener is of stilbene triazine type; The foaming agent is polyoxyethylene ether sulfate; The dispersant is fatty alcohol polyoxyethylene ether ester sulfonate or fatty alcohol polyoxyethylene ether; The non-woven fabric layer is a 70g fully cross non-woven fabric; the polyester chemical fiber fabric layer is 150D / 96F, black and white yarn cross-woven with an inch density of 50*50, and the weight of the polyester chemical fiber fabric layer is 140gsm / m 2 .

7. The foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain according to claim 3, characterized in that: The mildew preventer is isothiazolinone; the antibacterial agent is nano-grade copper-zinc ions.

8. The method for preparing the foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Laminating the non-woven fabric layer and the polyester chemical fiber fabric layer at a laminating temperature of 150-170°C; (2) According to weight proportions, 10-20 parts of deionized water, 30-40 parts of acrylic resin, 20-30 parts of compound flame retardant, 20-30 parts of nano-grade titanium dioxide slurry, 0.5-1.5 parts of foam stabilizer, 0.5-1.5 parts of foaming agent, 3-6 parts of carbon black and 1-2 parts of thickener are mixed and stirred, and the pH is adjusted to 7-8, the viscosity is 6000-8000cps / 4#30R, and the foaming ratio is 2-4 times to obtain a flame retardant light-shielding layer coating; the flame retardant light-shielding layer coating is suspended and coated on the surface of the polyester chemical fiber cloth layer, and dried to obtain a flame retardant light-shielding layer; (3) Mixing 10-20 parts of deionized water, 30-40 parts of acrylic resin, 20-30 parts of nano-grade titanium dioxide slurry, 5-10 parts of foamed microspheres and 0.8-1.5 parts of thickener according to weight, adjusting the pH to 7-8 and the viscosity to 10000-12000cps / 4#30R to obtain a sound insulation layer coating; applying the sound insulation layer coating on the surface of the flame retardant light shielding layer, and drying to obtain a sound insulation layer; (4) According to the weight proportions, 10-15 parts of deionized water, 30-40 parts of acrylic mixed emulsion, 30-40 parts of compounded dispersion, 0.5-1 part of defoaming agent, 0.5-1.5 parts of brightener, 0.5-2 parts of crosslinking agent and 0.5-1.5 parts of thickener are mixed and stirred, and the pH value is adjusted to 7-8 and the viscosity is 6000-8000cps / 4#30R to obtain a printing layer coating; the printing layer coating is evenly scraped and applied on the surface of the sound insulation layer with a flat knife, and dried to obtain a foamed sound-absorbing, light-shielding, antibacterial and mildew-proof soft curtain.

9. The preparation method according to claim 8, characterized in that: The drying in step (2), step (3) and step (4) is all carried out in a nine-section oven; The drying temperatures of the nine ovens in step (2) are: 70-80°C in the first oven, 80-120°C in the second oven, 150-160°C in the third, fourth, fifth, sixth, seventh and eighth ovens, and 70-90°C in the ninth oven; The drying temperatures in the nine ovens in step (3) are: 70-80° C. in the first oven, 80-120° C. in the second, third, fourth, fifth, sixth, seventh and eighth ovens, and 70-90° C. in the ninth oven; The drying temperatures of the nine ovens in step (4) are: 70-80°C for the first oven, 80-120°C for the second oven, 150-160°C for the third, fourth, fifth, sixth, seventh and eighth ovens, and 70-90°C for the ninth oven.

10. The preparation method according to claim 9, characterized in that: In step (1), the vehicle speed is 10-20 m / min; In step (2), the vehicle speed is 10-20 m / min; the flame retardant light shielding layer has a dry weight of 50-60 g and a thickness of 100-200 um; In step (3), the vehicle speed is 5-15 m / min; the dry weight of the sound insulation layer is 50-60 g, and the coating thickness is 200-300 um; In step (4), the vehicle speed is 10-20 m / min; The dry weight of the printed layer is 10-20g, and the coating thickness is 30-50um.

Citation Information

Patent Citations

  • A method for preparing antibacterial and light-blocking curtain fabric

    CN115434158B

  • Preparation method of heat-resistant foamed microcapsule

    CN102702449A

  • Liquid electronic ink receiving medium

    CN106915171A

  • High-covering-power flame-retardant wall cloth and preparation process thereof

    CN114808471A

  • Preparation method of sandwich structure sound insulation and noise reduction wall cloth and foaming machine

    CN114953494A