A method for preparing ZnCdS alloy quantum dots
Through a multi-step method under the protection of inert gas, ZnCdS alloy quantum dots with uniform composition are formed, which solves the problems of low yield and uneven element distribution in the existing technology, and achieves efficient fluorescence emission peak control and high yield of ZnCdS. Quantum dot preparation.
Patent Information
- Application Number
- CN202210395378.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-04-14
AI Technical Summary
The existing ZnCdS alloy quantum dot preparation method has problems such as low yield and uneven distribution of zinc and cadmium elements, resulting in a large half-height-to-width ratio of the fluorescence emission peak.
Using a multi-step method under the protection of inert gas, through vacuum evacuation and temperature control, CdS/nZnS core-shell quantum dots are formed, and ZnCdS alloy quantum dots with uniform composition are formed under the action of copper ion catalyst and soft alkali. Realize the diffusion of zinc and cadmium elements and the exchange of lattice cation sites.
The regulation of the fluorescence emission peak in the range of 400 to 470 nm is achieved, the fluorescence half-maximum width is less than 25 nm, the yield is high, the size distribution is uniform, it is suitable for blue light sources and QLED materials, and the synthesis method is simple and repeatable.
Smart Images

Figure BDA0003597150470000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of quantum dot synthesis, and in particular to a method for preparing ZnCdS alloy quantum dots. Background Art
[0002] Quantum dots are a type of luminescent material with excellent fluorescent properties. Due to the quantum size effect, they can achieve fluorescence emission peak regulation, narrow fluorescence half-width, high fluorescence quantum yield and other characteristics, which have attracted widespread attention from academia and industry, and have broad applications in the fields of display, solid-state lighting, and solid-state light sources. In addition, quantum dots have good solution processing properties, and various complex display patterns can be achieved through industrial technologies such as screen printing, inkjet printing, and scraping, thereby reducing the manufacturing cost of quantum dot light-emitting diodes.
[0003] Binary quantum dots can only control the energy gap of quantum dots by controlling size and morphology, while alloy quantum dots can also control the energy gap of quantum dots by adjusting the molar ratio of each element in the quantum dot composition. For example, with the same diameter size, the energy gap of CdZnS quantum dots is larger than that of CdS quantum dots, but smaller than that of ZnS quantum dots.
[0004] The fluorescence emitted by ZnCdS alloy quantum dots can be regulated in the range of 380-470nm from violet to blue, and is an excellent violet and blue material. At present, there are two main approaches to the synthesis of ternary ZnCdS alloy quantum dots: the first approach is the "hot injection method", which is to hot-inject the sulfur precursor into the mixture of the zinc precursor and the cadmium precursor. For example, in 2003, Zhong Xinhua et al. synthesized large-sized ZnCdS alloy quantum dots with different diameters and different proportions of the three elements Zn, Cd, and S by this method, and the fluorescence emission peak was regulated in the range of 391nm to 474nm (J.Am.Chem.Soc.2003,125(44),13559–13563.); the second approach is the "one-pot method", which is to mix the zinc precursor, cadmium precursor, and sulfur precursor at room temperature and then heat them to the reaction temperature. For example, Yu Kui et al. synthesized ZnCdS gradient alloy quantum dots by a one-pot method in 2008 (J. Phys. Chem. C 2008, 112 (13), 4908–4919.).
[0005] The patents for synthesizing ZnCdS quantum dots using the "hot injection method" are as follows: the patent with application number 201010158928.4, application publication date 2010.04.28, and title "A CdxZn1-xS / ZnS ternary core-shell quantum dot and preparation method thereof" discloses a method of using cadmium oxide or an inorganic cadmium salt as a cadmium source, zinc oxide or an inorganic zinc salt as a zinc source, and then injecting a sulfur precursor solution into it to form ZnCdS core quantum dots; the patent with application number 201611003252.5, application publication date 2016.11.15, and title "A CdxZn1-xS / ZnS ternary core-shell quantum dot and preparation method thereof" discloses a method of using cadmium oxide or an inorganic cadmium salt as a cadmium source, zinc oxide or an inorganic zinc salt as a zinc source, and then injecting a sulfur precursor solution into it to form ZnCdS core quantum dots; The patent of "An alloy quantum dot core with uniform internal and external components and its preparation method" discloses a method of mixing two pre-prepared cationic precursor solutions and heating them to a predetermined temperature, and then injecting another prepared anionic precursor solution to carry out a nucleation reaction, and by continuing to inject the cationic precursor solution or the anionic precursor solution or the cationic precursor solution and the anionic precursor solution at a gradually changing rate during the nucleation reaction, so that the reaction rate of each component in the nucleation reaction remains relatively stable and the stoichiometric ratio of nucleation is relatively consistent, thereby producing an alloy quantum dot core with uniform internal and external components.
[0006] The patents for synthesizing ZnCdS quantum dots using the "one-pot method" are as follows: the patent application with application number 202010554538.2, application publication date 2020.06.17, and name "Method for preparing Cu:ZnCdS / ZnS quantum dot luminescent materials by one-pot method" discloses a method for preparing a precursor solution using a zinc source, a cadmium source, a copper source, and a sulfur source, and then placing each precursor solution in the same reaction container, removing water and oxygen, and then heating the reaction to generate a Cu-doped ZnCdS quantum dot luminescent material with a cubic sphalerite structure; the patent application with application number 201010192189.0, application publication date 2010.05.31, and name "Method for preparing Mn-doped ZnCdS quantum dots" discloses a method for preparing Mn-doped ZnCdS quantum dots by a microwave aqueous phase method. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing ZnCdS alloy quantum dots with uniform internal and external components, aiming to solve the problems of low yield in the existing preparation method, uneven distribution of zinc and cadmium elements, resulting in a large half-height width ratio of the fluorescence emission peak, etc.
[0008] The present invention is further described in detail in the following examples. The present invention discloses a method for preparing ZnCdS alloy quantum dots, comprising the following steps:
[0009] S1. The octadecene solution of CdS quantum dots is vacuum-evacuated at room temperature for 10 to 60 minutes, and then the temperature is raised to 120° C. and vacuum-evacuated for 60 to 120 minutes;
[0010] S2, adding a single precursor solution under the protection of an inert gas and in the first temperature range, raising the temperature to the second temperature range and keeping the temperature for a certain period of time to perform epitaxial growth of a first layer of ZnS shell, and then lowering the temperature to the first temperature range, repeating the above operation, after n times of operation, epitaxially growing an nth layer of ZnS shell, and obtaining a CdS / nZnS core-shell quantum dot solution;
[0011] S3. Purify the CdS / nZnS core-shell quantum dot solution and dissolve it in octadecene. Then, heat it to a third temperature range under the protection of an inert gas, add a copper ion catalyst solution and a soft alkali solution, keep the temperature and anneal for a certain period of time to form ZnCdS alloy quantum dots.
[0012] In some embodiments, the concentration of the octadecene solution of CdS quantum dots in step S1 is 30 nmol / mL to 1000 nmol / mL, preferably 40 nmol / mL to 120 nmol / mL.
[0013] Preferably, in step S1, the average radius of the CdS quantum dots in the octadecene solution of CdS quantum dots is less than or equal to the exciton Bohr radius of the bulk material thereof, and preferably the diameter size is 3 nm to 5 nm.
[0014] Preferably, the single precursor solution added in step S2 is a dispersion of zinc diethyldithiocarbamate in oleylamine, and preferably, the molar concentration is 0.05 mol / L to 0.5 mol / L.
[0015] Preferably, the copper ion catalyst solution added in step S3 is an octadecene solution of copper oleate solution, preferably, the molar concentration is 0.1 mmol / L-0.4 mmol / L.
[0016] Preferably, the copper oleate added in step S3 can be prepared by reacting copper acetate and oleic acid in a molar ratio of 1:2, or can be prepared by any other feasible method.
[0017] Preferably, the first temperature in step S2 is in the range of 60 to 120°C.
[0018] Preferably, the second temperature in step S2 is in the range of 160-200°C.
[0019] Preferably, the third temperature in step S3 is in the range of 280-320°C.
[0020] Preferably, the number n of ZnS shells of the CdS / nZnS core-shell quantum dots in step S3 is 6-12.
[0021] Preferably, the number of ZnS shell layers of the CdS / ZnS core-shell quantum dots in the third system in step S2 is 6 to 8.
[0022] Preferably, the soft alkali solution added in step S3 is trioctylphosphine, and the volume ratio of trioctylphosphine to the copper ion catalyst solution is 1:1 to 1:3.
[0023] Preferably, in step S2, the amount of the copper ion material injected in step S3 is 0.5 to 2 times the amount of the CdS quantum dot material in step S1.
[0024] Preferably, the hardness of the soft alkali solution is in the range of 5.5 to 6.5 eV; the copper ion catalyst solution is selected from saturated or unsaturated alkanes containing monovalent or divalent copper ions, such as an octadecene solution of copper oleate.
[0025] In the present invention, except for vacuum pumping, the reaction is carried out under the protection of an inert gas, preferably argon or nitrogen.
[0026] Compared with the prior art, the beneficial effects of the present invention are embodied in the following aspects: (1) Through a special copper ion catalyst solution, the zinc element in the ZnS shell layer in the CdS / ZnS core-shell quantum dot and the cadmium element in the CdS core quantum dot diffuse with each other and exchange lattice cation sites, and finally form ZnCdS alloy quantum dots with uniform components; (2) The fluorescence emission peak of the ZnCdS alloy quantum dots prepared by this method is regulated in the range of 400 to 470 nm from purple light to blue light, and the fluorescence half-width is less than 25 nanometers, which can be widely used in various blue light sources, QLED blue light materials, etc.; (3) The synthesis method is simple, highly repeatable, and has a high synthesis yield; (4) The product size distribution is uniform and the gel dispersibility is good; (5) The average radius of the ZnCdS quantum dots synthesized by this synthesis method is close to the exciton Bohr radius of its bulk material, which is a large-sized ZnCdS alloy quantum dot that is difficult to synthesize by the "one-pot method" and the "hot injection method". DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] At room temperature, 2 mL of 60 nmol / mL octadecene solution of CdS quantum dots with a diameter of 3.7 nm was vacuumed for 30 minutes at room temperature, then heated to 120°C and vacuumed for 60 minutes. Then, 0.5 mL of 0.1 mol / L single precursor solution was added under argon protection, and then the temperature was raised to 180°C and kept for 30 minutes to epitaxially grow the first layer of ZnS shell. Then the temperature was lowered to 120°C, 0.65 mL of a single precursor solution with a concentration of 0.1 mol / L was added, and then the temperature was raised to 180°C and kept for 30 min to epitaxially grow a second layer of ZnS shell, and then the temperature was lowered to 120°C, and the above operation was repeated 4 times (the volume of the single precursor solution with a concentration of 0.1 mol / L was added each time was 0.85 mL, 1.05 mL, 1.30 mL, and 1.55 mL, respectively), and 6 layers of ZnS shells were epitaxially grown to obtain a CdS / 6ZnS core-shell quantum dot solution; the CdS / 6ZnS core-shell quantum dot solution was then purified and dissolved in 2 mL of octadecene, and vacuum pumped at room temperature for 30 minutes, and then the temperature was raised to 120°C and vacuum pumped for 60 min. Then, the temperature was raised to 280° C. under the protection of inert gas, and 0.6 mL of 0.2 mmol / L copper oleate octadecene solution and 1.2 mL of trioctylphosphine were added. The temperature was kept and annealed for 120 min, and the reaction was stopped to purify ZnCdS alloy quantum dots from the reaction solution.
[0030] Example 2
[0031] At room temperature, 3 mL of 40 nmol / mL octadecene solution of CdS quantum dots with a diameter of 5 nm was vacuumed for 60 minutes at room temperature, then heated to 120°C and vacuumed for 120 minutes. Then, 0.25 mL of 0.5 mol / L single precursor solution was added under argon protection, and then the temperature was raised to 200°C and kept for 50 minutes to epitaxially grow the first layer of ZnS shell. Then the temperature was lowered to 60°C, 0.55 mL of a single precursor solution with a concentration of 0.5 mol / L was added, and then the temperature was raised to 200°C and kept for 60 min to epitaxially grow a second layer of ZnS shell, and then the temperature was lowered to 60°C, and the above operation was repeated 10 times (the volume of the single precursor solution with a concentration of 0.86 mol / L added each time was 1.19 mL, 1.52 mL, 1.95 mL, 2.38 mL, 2.81 mL, 3.33 mL, 3.65 mL, 3.97 mL, 4.34 mL, and 4.81 mL, respectively), 10 layers of ZnS shells were epitaxially grown to obtain a CdS / 12ZnS core-shell quantum dot solution; the CdS / 12ZnS core-shell quantum dot solution was then purified and dissolved in 3 mL of octadecene, and vacuumed at room temperature for 30 minutes, and then heated to 120°C and vacuumed for 120 min. Then, the temperature was raised to 320° C. under the protection of inert gas, and 0.3 mL of 0.4 mmol / L copper oleate octadecene solution and 0.3 mL of trioctylphosphine were added. The temperature was kept and annealed for 240 min, and the reaction was stopped to purify ZnCdS alloy quantum dots from the reaction solution.
[0032] Example 3
[0033] At room temperature, 1 mL of 120 nmol / mL octadecene solution of CdS quantum dots with a diameter of 3 nm was vacuumed for 60 minutes at room temperature, then heated to 120°C and vacuumed for 120 minutes. Then, argon gas was passed through and 1.5 mL of 0.05 mol / L single precursor solution was added, followed by heating to 160°C and keeping warm for 20 minutes to epitaxially grow the first ZnS shell. Then the temperature was lowered to 80°C, 2.15 mL of a single precursor solution with a concentration of 0.05 mol / L was added, and then the temperature was raised to 160°C and kept for 30 min to epitaxially grow a second layer of ZnS shell, and then the temperature was lowered to 80°C, and the above operation was repeated 6 times (the volume of the single precursor solution with a concentration of 0.05 mol / L added each time was 2.89 mL, 3.52 mL, 3.93 mL, 4.41 mL, 4.91 mL, and 5.53 mL, respectively), and 8 layers of ZnS shells were epitaxially grown to obtain a CdS / 8ZnS core-shell quantum dot solution; the CdS / 8ZnS core-shell quantum dot solution was then purified and dissolved in 3 mL of octadecene, and vacuum pumped at room temperature for 30 minutes, and then the temperature was raised to 120°C and vacuum pumped for 120 min. Then, the temperature was raised to 300° C. under the protection of inert gas, and 1.2 mL of 0.1 mmol / L copper oleate octadecene solution and 0.4 mL of trioctylphosphine were added. The temperature was kept and annealed for 180 min, and the reaction was stopped to purify ZnCdS alloy quantum dots from the reaction solution.
[0034] Example 4
[0035] At room temperature, 1.2 mL of 100 nmol / mL octadecene solution of CdS quantum dots with a diameter of 4.2 nm was vacuumed for 30 minutes at room temperature, then heated to 120°C and vacuumed for 120 minutes. Then, 0.4 mL of 0.25 mol / L single precursor solution was added under argon protection, and then the temperature was raised to 190°C and kept for 30 minutes to epitaxially grow the first layer of ZnS shell. Then the temperature was lowered to 90°C, 0.61 mL of a single precursor solution with a concentration of 0.25 mol / L was added, and then the temperature was raised to 190°C and kept for 30 min to epitaxially grow a second layer of ZnS shell, and then the temperature was lowered to 90°C, and the above operation was repeated 7 times (the volume of the single precursor solution with a concentration of 0.25 mol / L added each time was 1.19 mL, 1.52 mL, 1.93 mL, 2.41 mL, 2.85 mL, 3.34 mL, and 3.80 mL, respectively), and 9 layers of ZnS shells were epitaxially grown to obtain a CdS / 9ZnS core-shell quantum dot solution; the CdS / 9ZnS core-shell quantum dot solution was then purified and dissolved in 3 mL of octadecene, and vacuum pumped at room temperature for 30 minutes, and then the temperature was raised to 120°C and vacuum pumped for 120 min. Then, the temperature was raised to 290° C. under the protection of inert gas, and 0.8 mL of 0.15 mmol / L copper oleate octadecene solution and 0.6 mL of trioctylphosphine were added. The temperature was kept and annealed for 160 min, and the reaction was stopped to purify ZnCdS alloy quantum dots from the reaction solution.
[0036] Comparative Example 1
[0037] At room temperature, 1.2 mL of 100 nmol / mL octadecene solution of CdS quantum dots with a diameter of 4.2 nm was vacuumed for 30 minutes at room temperature, then heated to 120°C and vacuumed for 120 minutes. Then, 0.4 mL of 0.25 mol / L single precursor solution was added under argon protection, and then the temperature was raised to 190°C and kept for 30 minutes to epitaxially grow the first layer of ZnS shell. Then the temperature was lowered to 90°C, 0.61 mL of a single precursor solution with a concentration of 0.25 mol / L was added, and then the temperature was raised to 190°C and kept for 30 min to epitaxially grow a second layer of ZnS shell, and then the temperature was lowered to 90°C, and the above operation was repeated 7 times (the volume of the single precursor solution with a concentration of 0.25 mol / L added each time was 1.19 mL, 1.52 mL, 1.93 mL, 2.41 mL, 2.85 mL, 3.34 mL, and 3.80 mL, respectively), and 9 layers of ZnS shells were epitaxially grown to obtain a CdS / 9ZnS core-shell quantum dot solution; the CdS / 9ZnS core-shell quantum dot solution was then purified and dissolved in 3 mL of octadecene, and vacuum pumped at room temperature for 30 minutes, and then the temperature was raised to 120°C and vacuum pumped for 120 min. Then, the temperature was raised to 260° C. under the protection of inert gas, and 0.8 mL of 0.15 mmol / L copper oleate octadecene solution was added. The temperature was kept and annealed for 160 min, and the reaction was stopped. The sample was purified from the reaction solution.
[0038] Comparative Example 2
[0039] At room temperature, 1.2 mL of 100 nmol / mL octadecene solution of CdS quantum dots with a diameter of 4.2 nm was vacuumed for 30 minutes at room temperature, then heated to 120°C and vacuumed for 120 minutes. Then, 0.4 mL of 0.25 mol / L single precursor solution was added under argon protection, and then the temperature was raised to 190°C and kept for 30 minutes to epitaxially grow the first layer of ZnS shell. Then the temperature was lowered to 90°C, 0.61 mL of a single precursor solution with a concentration of 0.25 mol / L was added, and then the temperature was raised to 190°C and kept for 30 min to epitaxially grow a second layer of ZnS shell, and then the temperature was lowered to 90°C, and the above operation was repeated 7 times (the volume of the single precursor solution with a concentration of 0.25 mol / L added each time was 1.19 mL, 1.52 mL, 1.93 mL, 2.41 mL, 2.85 mL, 3.34 mL, and 3.80 mL, respectively), and 9 layers of ZnS shells were epitaxially grown to obtain a CdS / 9ZnS core-shell quantum dot solution; the CdS / 9ZnS core-shell quantum dot solution was then purified and dissolved in 3 mL of octadecene, and vacuum pumped at room temperature for 30 minutes, and then the temperature was raised to 120°C and vacuum pumped for 120 min. Then, the temperature was raised to 260° C. under the protection of inert gas, and 0.6 mL of trioctylphosphine was added. The temperature was kept and annealed for 160 min. The reaction was stopped and the sample was purified from the reaction solution.
[0040] Experimental results: The fluorescence emission peak wavelength and half-peak width of the samples obtained in Examples 1-4 and Comparative Examples 1-2 were respectively detected, and the results are shown in Table 1. The fluorescence half-peak width of the samples in Examples 1-4 is less than 20 nm, which is much better than the fluorescence half-peak width of the samples in Comparative Examples 1-2, and has higher color purity and higher fluorescence performance.
[0041] Table 1
[0042]
[0043] In summary, the present invention provides a method for preparing an alloy quantum dot core with uniform internal and external components. Under the action of a copper ion catalytic solution, copper ions can diffuse from the surface of CdS / ZnS core-shell quantum dots to the CdS core quantum dot core and the ZnS shell quantum dot, and replace the Cd site and the Zn site in the quantum dot, and make the Cd site diffuse into the entire ZnS shell layer, the Zn site diffuse into the entire CdS core quantum dot, and the S site remains unchanged, finally forming a statistically uniform ZnCdS alloy quantum dot. The method of the present invention effectively solves the problems of uneven internal and external components of the alloy quantum dot core, low luminous efficiency, and too wide fluorescence emission peak, and the method provided by the present invention has the advantages of simple operation, easy regulation, and high repeatability.
[0044] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing ZnCdS alloy quantum dots, characterized in that: The steps include: S1, evacuating an octadecene solution of CdS quantum dots at room temperature for a certain period of time, then heating the solution to a first temperature range, and evacuating the solution again for a certain period of time; in the octadecene solution of CdS quantum dots, an average radius of the CdS quantum dots is less than or equal to the exciton Bohr radius of the bulk material thereof; S2, adding a single precursor solution under the protection of an inert gas and in the first temperature range, heating to the second temperature range and keeping the temperature for a certain period of time to epitaxially grow a first layer of ZnS shell, then cooling to the first temperature range, repeating the above operation, after n operations, epitaxially growing an nth layer of ZnS shell, and obtaining a CdS / nZnS core-shell quantum dot solution, wherein the number of ZnS shell layers n is 6 to 12; S3, purifying the CdS / nZnS core-shell quantum dot solution and dissolving it in octadecene, then heating it to a third temperature range under the protection of an inert gas, adding a copper ion catalyst and a soft alkali solution, keeping the temperature and annealing for a certain period of time to form ZnCdS alloy quantum dots; Wherein, the first temperature range is 60-120°C, the second temperature range is 160-200°C; in step S3, the third temperature range is 280-320°C.
2. The preparation method according to claim 1, characterized in that: In step S1, the concentration of the octadecene solution of CdS quantum dots is 30 nmol / mL to 200 nmol / mL.
3. The preparation method according to claim 1, characterized in that: In step S2, the single precursor solution added is a dispersion of zinc diethyldithiocarbamate in oleylamine, and its molar concentration is 0.05 mol / L to 0.5 mol / L.
4. The preparation method according to claim 1, characterized in that: In step S3, the copper ion catalyst solution added has a concentration of 0.1 mmol / L-0.4 mmol / L.
5. The preparation method according to claim 1, characterized in that: In step S3 , the amount of copper ions injected is 0.5 to 2 times the amount of the CdS / nZnS core-shell quantum dot material in step S3 .
6. The preparation method according to claim 1, characterized in that: In step S3, the hardness of the soft alkali solution is in the range of 5.5 to 6.5 eV; and the copper ion catalyst solution is selected from saturated or unsaturated alkanes containing monovalent or divalent copper ions.
7. The preparation method according to claim 6, characterized in that: The soft alkali solution is trioctylphosphine, the copper ion catalyst solution is an octadecene solution of copper oleate, and the volume ratio of the soft alkali solution to the copper ion catalyst solution is 1:1 to 1:3.
Citation Information
Patent Citations
CdxZn1-xS / ZnS ternary core-shell quantum dot and method for preparing same
CN101824317A
Preparation method of Mn-doped ZnCdS quantum dots
CN101875843A
Alloy quantum dot core with uniform internal and external components and preparation method thereof
CN106590633A
Method for preparing Cu: ZnCdS / ZnS quantum dot luminescent material by one-pot method
CN111662707A