An explosive welding method for components with complex cavities

By casting filler metal in the cavity and combining explosive welding and heating and remelting processes, the problem of welding complex cavity components is solved, efficient and deformation-free welding effects are achieved, and the welding quality and performance of dissimilar metal cavity components are improved.

CN116967589BActive Publication Date: 2024-10-29HUNAN FORHOME COMPOSITE MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310561213.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-10-29
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

It is difficult to effectively weld complex cavity components, especially dissimilar metal cavity components, with existing technology, and traditional welding methods cannot guarantee the welding quality and overall performance of the component.

Method used

By pouring filler metal into the cavity, the filler alloy is used to hinder deformation during the explosive welding process, and through cavity processing, casting filling, explosive welding and heating and remelting processes, efficient welding of large cavity devices of the same or dissimilar metals is achieved .

Benefits of technology

It achieves high-strength, deformation-free welding of complex cavity components, improves welding speed and quality, ensures interface bonding performance, and solves the problem that traditional welding methods are difficult to handle large and complex cavity devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116967589B_ABST
    Figure CN116967589B_ABST
Patent Text Reader

Abstract

The present invention discloses an explosion welding method for a component with a complex cavity, and belongs to the field of metal material forming. The explosion welding method comprises the following steps: the first step is to select a high melting point alloy as a substrate, and process a cavity on the substrate; the second step is to cast a low melting point alloy in the cavity; the third step is to take out the solidified low melting point alloy, and put it back into the cavity after coating the contact surface with the substrate with an insulating powder; the fourth step is to explosively composite the two substrates of the cast filler; the fifth step is to heat the explosive composite component to above the melting point of the low melting temperature alloy; the sixth step is to discharge the molten alloy from the cavity. The method of the present invention solves the problem that conventional welding methods cannot achieve welding inside a complex cavity. The present invention has low manufacturing cost and high production efficiency, and can achieve large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an explosion welding method for a complex cavity component and belongs to the field of metal material forming. Background Art

[0002] In the context of the continuous pursuit of lightweight structures in many fields such as automotive electronics, aerospace, and rail transportation, topology optimization has become an important means of structural redesign to achieve significant weight reduction of components while ensuring that the strength of the device is not reduced. However, complex design schemes often lead to a large number of irregular cavities in the originally regular solid components, which also brings great difficulties to processing and forming. In addition, many components used in extreme environments often need to quickly remove heat through circulating coolant to ensure that the components have good heat dissipation performance at high temperatures, which requires the device to have a cavity structure inside, such as the hollow turbine blades of the engine.

[0003] At present, the processing and forming methods of small, simple, thin-walled cavity devices are relatively mature, that is, first milling out the upper and lower side parts, and then realizing the composite forming of both sides by resistance welding or brazing. However, when preparing large and complex cavity devices, traditional welding methods have great difficulties, and the performance of the welded joints cannot be guaranteed. Even in the context of structural and functional integration, more and more hollow devices are designed as composite components of dissimilar metals, such as copper is used on the side close to the heat source to ensure excellent thermal conductivity, and steel is used on the side away from the heat source to ensure the overall structural strength. Since different metals have completely different physical properties, traditional welding often cannot guarantee the welding quality of dissimilar metals. Explosive welding has become one of the important means of welding and forming of metal composite materials due to its advantages of fast forming speed, large welding area and high welding strength. At the same time, the characteristics of mechanical bonding + metallurgical bonding of the interface of explosive welding ensure that the composite components have excellent interface bonding strength. However, due to the technical characteristics of high-energy jets generated during explosive welding, if it is directly used for explosive forming of cavity devices, it will seriously damage the structure of the cavity. Therefore, the development of explosive welding technology for cavity devices has important industrial application value in promoting the lightweight development of components and improving the service performance of materials in extreme environments. Summary of the invention

[0004] In view of the difficulty of welding complex cavity components, even heterogeneous metal cavity components, and the problem that explosion welding cannot be directly used for cavity device molding in the prior art, the present invention provides an explosion welding method with complex cavity components. The method can realize the welding molding of the same or heterogeneous metal cavity components, and has many advantages such as fast molding speed, large welding area, high welding yield, superior interface bonding performance, and no deformation of complex cavity structure after welding.

[0005] The present invention proposes for the first time that a filler metal is cast into a cavity, and during the explosive welding process, the filler metal prevents the cavity from deforming, thereby realizing explosive welding of components with complex cavities.

[0006] The present invention proposes for the first time to realize the welding forming of large-scale cavity devices of the same or different metals through cavity processing, casting filling, explosion welding and heating remelting processes, including the following steps:

[0007] Step 1: Select two substrates and machine the cavity on them;

[0008] Step 2: Select the filler alloy, melt it, cast it into the cavity of the substrate, and process it flat;

[0009] The third step is to take out the solidified filler alloy, coat the contact surface with the substrate with isolation powder, and then put it back into the cavity;

[0010] Step 4: Explosion welding the substrate with the filler alloy as the base plate and the composite plate;

[0011] Step 5: Heat the entire component after explosion welding to above the melting point of the filler alloy until the filler alloy is completely melted;

[0012] Step 6: Continuously blow inert gas from the upper inlet to expel the molten filler alloy from the cavity.

[0013] As a preferred embodiment, the present invention provides an explosion welding method for a complex cavity component, wherein the substrate in the first step is one or two of carbon steel, stainless steel, aluminum and aluminum alloys, titanium and titanium alloys, copper and copper alloys, nickel and nickel alloys.

[0014] As a preferred embodiment, in the explosive welding method of a complex cavity component of the present invention, the melting temperature of the filling alloy in the second step is lower than the melting temperature of the substrate by more than 200°C, preferably a eutectic alloy, which can ensure that the substrate is not deformed and partially melted during the subsequent remelting process. The melting point difference between the substrate and the filling alloy is further preferably 200-500°C.

[0015] As a preferred embodiment, the present invention provides an explosion welding method for a complex cavity component, wherein the insulating powder in the third step is one of dry graphite powder, boron nitride powder, aluminum oxide powder, magnesium oxide powder, zinc oxide powder or molybdenum disulfide powder, which has the advantage of weakening the diffusion and interface bonding between the filler metal and the substrate during the explosion welding process, and can improve the surface quality of the internal cavity after the filler metal is remelted and discharged.

[0016] As a preferred embodiment, the present invention provides an explosion welding method for components with complex cavities, wherein the placement of the explosive welding in the fourth step is horizontal placement, and when the substrate and the composite plate are made of the same material, the substrate with a larger thickness is the substrate, and the substrate with a smaller thickness is the composite plate; when the original substrate is a dissimilar metal, the high-strength substrate is used as the substrate, and the low-strength substrate is used as the composite plate.

[0017] The thickness of the selected substrate is greater than 5 mm, preferably 5 mm to 200 mm; the thickness of the composite plate is greater than or equal to 5 mm, preferably 5 mm to 20 mm.

[0018] The composite plate and its filling metal are supported by gap columns; a buffer layer and an explosive layer are placed above the composite plate; the detonation point of explosive welding cannot be located at the thinnest position of the cavity wall, but should be located far away from the cavity to reduce damage to the cavity during the explosion and improve the welding process accuracy.

[0019] As a preferred embodiment, in the explosion welding method of the present invention for a complex cavity component, the heating temperature in the fifth step should be 50°C higher than the melting point of the filling alloy, and more preferably 50-100°C. This temperature ensures that the internal filling metal melts and flows out, thereby eliminating the residual stress of the device welding and avoiding the oxidation of the component.

[0020] As a preferred embodiment, the present invention provides an explosion welding method for a complex cavity component. In the sixth step, when discharging the low-melting-point alloy melt, an inert gas is continuously blown in from the upper inlet to promote the complete discharge of the melt and avoid the melt remaining in the cavity.

[0021] As a preferred solution, the present invention provides an explosive welding method for a complex cavity component, wherein the minimum distance from the cavity to the outer surface of the substrate is greater than or equal to 2 mm. The present invention realizes efficient and high-quality welding of thin-walled complex cavity components for the first time.

[0022] The advantages or beneficial effects of the present invention are:

[0023] The present invention overcomes the technical difficulties of welding large and complex cavity components by traditional methods (such as brazing and resistance welding) and the disadvantages of low interface bonding strength, and realizes high-strength bonding of large and complex cavity components by explosion welding. By casting a metal mold core in the cavity before explosion welding, it is ensured that the cavity is not damaged under the severe impact of explosion welding, and the mold core is remelted and discharged after explosion welding, thereby ensuring the integrity of the cavity.

[0024] The present invention appropriately selects a eutectic alloy with a temperature of more than 150°C (preferably more than 200°C) below its melting point as the filler metal according to the different materials of the base component. Compared with other alloys, the eutectic alloy has better fluidity and a lower melting temperature, which can ensure good filling properties and easy remelting and discharge. Although pure metals have the same excellent fluidity, the higher compressive strength of the eutectic alloy ensures that the cavity has a better bearing capacity during explosion welding. After explosion welding, the component is heated as a whole to above the melting point of the filler alloy, which not only discharges the filler metal in the cavity, but also eliminates the residual stress generated by the explosion welding, thereby enhancing the dimensional stability of the component. When the component is made of dissimilar metals, heat preservation promotes the cross-interface diffusion of atoms, further enhancing the interface strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The figure is a schematic diagram of the preparation process of the double-sided cavity component;

[0026] Figure 2 Schematic diagram of the preparation process of a single-sided cavity component. DETAILED DESCRIPTION

[0027] Example 1

[0028] Two pieces of 316L stainless steel were selected as the main material of the component, with the size of 600mm×300mm×20mm. After milling, the following Figure 1 The internal cavity (double-sided non-uniform serpentine channel) shown in the figure is milled and the surface burrs are polished. The Al-12wt.%Si alloy with good fluidity is used as a filler material and is melted at 740℃ and poured into the cavity. After natural cooling, the filler material is processed flat to ensure that the filler material and the substrate are in the same plane. Take out the filler, and put it back into the cavity after coating the contact surface with the substrate with dry graphite powder. The substrate and filler are transferred as a whole to the explosive welding site and placed horizontally on the anvil (the anvil is made of cast iron and has a size of 2000mm×1000mm×40mm). The same height support gap column (the height of the gap column is 5mm and the material of the gap column is pure aluminum) is placed between the upper and lower substrates. Rock ammonium nitrate mixed explosives are placed on the upper side, and the thickness of the explosive layer is 60mm. The detonation point is located away from the cavity. The two substrates are composited by explosive welding. After welding, the components are placed at an angle and heated to 650℃ as a whole to completely melt and discharge the Al-12wt.%Si filler alloy in the cavity. The same metal cavity component prepared by this method has an effective interface bonding rate of 99.5%, and the internal cavity is complete without deformation. In the obtained product, the minimum distance from the cavity to the outer surface of the substrate is 5mm.

[0029] Example 2

[0030] 316L stainless steel and T2 copper plate were selected as the main materials of the components. The dimensions of 316L stainless steel were 800mm×500mm×20mm, and the dimensions of T2 copper were 800mm×500mm×10mm. The following Figure 2 The internal cavity shown (unilateral non-uniform serpentine channel). The surface burrs were polished after milling. Al-9wt.%Mg-5wt.%Si alloy with good fluidity was used as a filler material and poured into the cavity after melting at 760℃. After natural cooling, the filler material was processed flat to ensure that the filler material was in the same plane as the 316L stainless steel substrate. The filler was taken out and put back into the cavity after coating the contact surface with the substrate with dry alumina powder. The substrate and filler were transferred to the explosive welding site as a whole and placed horizontally on the anvil (the material of the anvil was cast iron and the size was 2000mm×1000mm×40mm). The 316L stainless steel with filler was used as the substrate and T2 copper was used as the composite plate for explosive welding. The equal-height support gap column (the height of the gap column was 5mm and the material of the gap column was pure aluminum) was placed between the substrate and the composite plate. Rock ammonium nitrate mixed explosives were placed on the upper side of the composite plate. The thickness of the explosive layer was 30mm. The detonation point was located far away from the cavity. The two materials were composited by explosive welding. After welding, the component is tilted and heated to 660°C as a whole, and the Al-9wt.%Mg-5wt.%Si filler alloy in the cavity is completely melted and discharged. The interface bonding rate of the heterogeneous metal cavity component prepared by this method is 99.4%, and the internal cavity is complete without deformation. In the obtained product, the minimum distance from the cavity to the outer surface of the substrate is 10mm.

[0031] Example 3

[0032] TC4 titanium alloy plate and 45# steel were selected as the main materials of the components, with the dimensions of 500mm×500mm×10mm. Figure 1The internal cavity (double-sided non-uniform serpentine channel) shown in the figure is milled and the surface burrs are polished. The Al-33.2wt.%Cu alloy with good fluidity is used as a filler material and is melted at 650℃ and poured into the cavity. After natural cooling, the filler material is processed flat to ensure that the filler material and the substrate are in the same plane. Take out the filler, and put it back into the cavity after coating the contact surface with the substrate with dry boron nitride powder. The substrate and filler are transferred as a whole to the explosive welding site and placed horizontally on the anvil (the anvil is made of cast iron and has a size of 2000mm×1000mm×40mm). The same height support gap column (the height of the gap column is 3mm and the material of the gap column is pure aluminum) is placed between the upper and lower substrates. Rock ammonium nitrate mixed explosives are placed on the upper side, and the thickness of the explosive layer is 35mm. The detonation point is located away from the cavity. The two substrates are composited by explosive welding. After welding, the components are placed at an angle and heated to 600℃ as a whole to completely melt and discharge the Al-33.2wt.%Cu filler alloy in the cavity. The same metal cavity component prepared by this method has an interface bonding rate of 99.6%, an internal cavity is complete and has no deformation. In the obtained product, the minimum distance from the cavity to the outer surface of the substrate is 3 mm.

[0033] Example 4

[0034] H65 brass with dimensions of 600mm×400mm×15mm and 600mm×400mm×2mm were selected as the main material of the components. The following parts were milled on the brass with a thickness of 15mm. Figure 2 The internal cavity shown (unilateral non-uniform serpentine channel). The surface burrs are polished after milling. Al-12wt.% Si alloy with good fluidity is used as a filler material and poured into the cavity after melting at 740℃. After natural cooling, the filler material is processed flat to ensure that the filler material and the brass substrate are in the same plane. Take out the filler, and put it back into the cavity after coating the contact surface with the substrate with dry magnesium oxide powder. The substrate and filler are transferred to the explosive welding site as a whole and placed horizontally on the anvil (the material of the anvil is cast iron and the size is 2000mm×1000mm×40mm). The brass with filler is used as the substrate and the 2mm thick brass is used as the double plate for explosion welding. The equal height support gap column (the height of the gap column is 1.5mm and the material of the gap column is pure aluminum) is placed between the substrate and the double plate. Rock ammonium nitrate mixed explosives are placed on the upper side of the double plate. The thickness of the explosive layer is 18mm. The detonation point is located far away from the cavity. The two materials are composited by explosive welding. After welding, the component is tilted and heated to 650°C as a whole, so that the Al-12wt.%Si filler alloy in the cavity is completely melted and discharged. The interface bonding rate of the same metal cavity component prepared by this method is 99.6%, and the internal cavity is complete without deformation. In the obtained product, the minimum distance from the cavity to the outer surface of the substrate is 2mm.

[0035] Example 5

[0036] Pure aluminum and T2 copper plates are selected as the main materials of the components. The dimensions of the pure aluminum plates are 800mm×500mm×20mm, and the dimensions of the T2 copper plates are 800mm×500mm×5mm. The following are milled on the pure aluminum substrate. Figure 2 The internal cavity shown (unilateral non-uniform serpentine channel). The surface burrs were polished after milling. The ZA8 zinc alloy with good fluidity was used as the filling material and poured into the cavity after being melted at 450℃. After natural cooling, the filling material was processed flat to ensure that the filling material and the pure aluminum substrate were in the same plane. The filler was taken out and the contact surface with the substrate was coated with dry zinc oxide powder and then put back into the cavity. The substrate and the filler were transferred to the explosive welding site as a whole and placed horizontally on the anvil (the material of the anvil was cast iron and the size was 2000mm×1000mm×40mm). Pure aluminum with fillers was used as the substrate and 5mm thick T2 copper was used as the composite plate for explosive welding. The equal height support gap column (the height of the gap column was 2mm and the material of the gap column was pure aluminum) was placed between the substrate and the composite plate. Rock ammonium nitrate mixed explosives were placed on the upper side of the composite plate. The thickness of the explosive layer was 60mm. The detonation point was located far away from the cavity. The two materials were composited by explosive welding. After welding, the component is placed at an angle and heated to 420°C as a whole, and the ZA8 zinc alloy filled in the cavity is completely melted and discharged. The interface bonding rate of the heterogeneous metal cavity component prepared by this method is 99.5%, and the internal cavity is complete without deformation. In the obtained product, the minimum distance from the cavity to the outer surface of the substrate is 5mm.

[0037] Comparative Example 1

[0038] 316L stainless steel with the same size as in Example 1 was selected as the main material of the component, and the components were milled to obtain the following Figure 1 The internal cavity shown in the figure is milled and the surface burrs are polished. No other materials are filled in the cavity, and the substrate is directly transferred to the explosion welding site for explosion compounding. The explosion compounding process is the same as that of implementation 1. The same metal cavity component prepared by this method has no internal casting as support, and the internal cavity is severely deformed, the outer surface corresponding to the cavity position is severely sunken, and the interface bonding rate is 64%.

[0039] Comparative Example 2

[0040] The material with the same size as in Example 2 was selected as the main material of the component, and the 316L stainless steel was milled to obtain the following Figure 2The internal cavity shown is milled and the surface burrs are polished. An Al-2wt.% Si alloy (melting temperature is 650°C) with poor fluidity is selected to fill the cavity, and then explosive compounding is carried out using the same process as Example 2. After welding, the component is placed at an angle and heated to 700°C as a whole to discharge the filler. When this process is used, due to the poor fluidity of the filler metal, the filling body obtained by casting does not completely fit the cavity, resulting in severe deformation of part of the cavity during explosion welding, and the interface bonding rate is 92%. In addition, even if the component is heated to 700°C after welding, some of the filler cannot be discharged due to poor fluidity. The increase in temperature will also lead to a decrease in the strength of the substrate.

[0041] Comparative Example 3

[0042] The material with the same size as that in Example 5 was selected as the main material of the component, and the components were milled on the pure aluminum substrate as shown in the attached figure. Figure 2 The internal cavity is shown. The surface burrs are ground after milling. Al-12wt.%Si alloy (melting temperature is 577℃) with good fluidity is selected to fill the cavity, and then explosive compounding is carried out using the same process as Example 5. After welding, the component is placed at an angle, and the whole is heated to 660℃ and the filler is discharged. When using this process, since the melting point of pure aluminum is 660℃, part of the base material melts during the process of discharging the filler after welding, and the component is scrapped.

[0043] The above description is only a preferred embodiment of the present invention. Without departing from the principle of the present process innovation, any equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, shall be deemed as the patent protection scope of the present invention.

Claims

1. An explosive welding method for components with complex cavities, Features: The explosion welding method comprises the following steps: Step 1: Select two substrates and machine the cavity on them; The substrate in the first step is one or two of carbon steel, stainless steel, aluminum and aluminum alloys, titanium and titanium alloys, copper and copper alloys, nickel and nickel alloys; Step 2: Select a filling alloy, melt it and cast it into the mold cavity of the substrate, and process it flat; the low melting point alloy filled in the second step has a melting temperature lower than the melting point of the substrate by more than 200°C, and the low melting point alloy is a eutectic alloy; The third step is to take out the solidified filler alloy, coat the contact surface with the substrate with an isolation powder, and then put it back into the cavity; the isolation powder in the third step is one of dry graphite powder, boron nitride powder, aluminum oxide powder, magnesium oxide powder, zinc oxide powder or molybdenum disulfide powder; Step 4: Use the base material with the filler alloy as the base plate and the double plate for explosion welding; In the fourth step, the explosive welding is placed horizontally. When the base plate and the double plate are made of the same material, the base material with a larger thickness is the base plate, and the base material with a smaller thickness is the double plate; When the original base materials are dissimilar metals, the base material with a higher strength is used as the base plate, and the base material with a lower strength is used as the double plate; In the fourth step, the detonation point of the explosive welding is located on the side away from the cavity; Step 5: Heat the entire component after explosion welding to above the melting point of the filling alloy until the filling alloy is completely melted; the heating temperature in the fifth step is 50~100℃ higher than the melting point of the filling alloy; Step 6: Continuously blow inert gas from the upper inlet to expel the molten filler alloy from the cavity.

2. The method for explosive welding of a component with a complex cavity according to claim 1, Features: The cavity machined in the first step is located on one substrate or on two substrates at the same time.

3. The explosion welding method for a component with a complex cavity according to claim 1, Features: The minimum distance from the cavity to the outer surface of the substrate is greater than or equal to 2 mm.

4. The method for explosive welding of a component with a complex cavity according to claim 1, Features: The thickness of the selected base material is 5mm~200mm; the thickness of the composite plate is 5mm~20mm.

Citation Information

Patent Citations

  • Production of composite articles with internal cavities by blast welding

    RU2574178C1