A high burst volume waterborne polyurethane condom and its preparation method
By employing a multiple impregnation and drying process using low-modulus, high-elongation anionic waterborne polyurethane resin, the problems of insufficient thickness and softness in natural latex rubber condoms were solved, resulting in the production of polyurethane condoms with high burst volume, thus improving the product's softness and safety.
Patent Information
- Application Number
- CN202310982110.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-21
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2040-09-21
AI Technical Summary
Existing natural latex rubber condoms are difficult to make thinner than 0.04mm, posing a risk of protein allergies. Polyurethane condoms lack softness and burst volume, failing to meet consumer demand.
Waterborne polyurethane condoms are prepared using low-modulus, high-elongation anionic waterborne polyurethane resin through multiple impregnation and drying processes, with the thickness controlled at 0.02-0.06 mm, tensile modulus ≤2.0 MPa, burst volume ≥12 liters, and elongation at break ≥650%.
A polyurethane condom with low modulus and high burst volume was prepared. It has uniform thickness, few defects, good softness and high burst volume, thus improving the user experience.
Smart Images

Figure CN116970192B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of waterborne polyurethane technology applications, specifically to a high burst volume waterborne polyurethane condom and its preparation method. Background Technology
[0002] Condoms are currently the most widely used and simple contraceptive and sexually transmitted disease prevention device in the world. Existing products mainly include natural latex rubber condoms and water-based polyurethane condoms.
[0003] Due to the material properties of natural latex, it's difficult to achieve a thickness of less than 0.04mm for natural latex condoms. Furthermore, natural latex contains various proteins, posing a safety risk to individuals with protein allergies. However, after decades of market development, natural latex condoms have a wide market appeal, and their soft texture has gained consumer acceptance.
[0004] Currently, most polyurethane condoms on the market have a high modulus and a burst volume of about 7-11 liters. Compared with latex, their softness and burst volume are inferior. Therefore, a low-modulus, high-elongation waterborne polyurethane condom has been developed. It retains the advantages of polyurethane, such as non-protein allergy, high strength, high pressure, and high thermal conductivity, while also possessing softness and a high burst volume close to latex products. This further enhances the user experience of polyurethane condoms and has significant market implications. Summary of the Invention
[0005] To address the problems existing in the prior art, the present invention provides a high burst volume waterborne polyurethane condom and its preparation method.
[0006] This invention first provides a high burst volume waterborne polyurethane condom and its preparation method. The method includes at least the following steps: providing a waterborne polyurethane; impregnating the waterborne polyurethane and drying it, and repeating the impregnation and drying process N times to obtain a waterborne polyurethane film; curling the waterborne polyurethane film and drying it; impregnating it with a release agent, and then drying, demolding, and electrical testing to obtain the waterborne polyurethane condom; wherein, N = 1-5, the waterborne polyurethane is anionic waterborne polyurethane, the 100% tensile modulus of the waterborne polyurethane is less than or equal to 2.0 MPa, and the elongation at break is greater than or equal to 650%.
[0007] In one embodiment, drying the waterborne polyurethane film after edge rolling is called molding drying, and drying the film after impregnation with the waterborne polyurethane is called setting drying. The setting drying time and the molding drying time have a time interval t. 成 =90·Φ-1.8·(N+2)t 定 The relationship between t 成 For molding and drying time, t 定Φ represents the shaping and drying time, N represents the number of impregnation repetitions, Φ = 2.7 - 0.015·T, T represents the temperature for shaping and drying, and the unit of T is degrees Celsius. 定 and t 成 The unit is minutes.
[0008] In one embodiment, the shaping and drying time is 2-10 minutes, the molding and drying time is 10-65 minutes, and the release agent drying time is 2-30 minutes.
[0009] In one embodiment, the drying temperature is 80-140°C.
[0010] In one embodiment, the solid content of the waterborne polyurethane is 15-30%.
[0011] In one embodiment, the macromolecular polyol accounts for 60-85% of all solid raw material components in the waterborne polyurethane, and among the macromolecular polyols, the proportion of macromolecular polyols having three or more functions is 10-40%.
[0012] In one embodiment, the macromolecular polyol is composed of a difunctional macromolecular polyol with a molecular weight of 500-4000 and a trifunctional macromolecular polyol with a molecular weight of 650-6000 in a mass ratio of 4:(0.2-1.5).
[0013] The present invention also provides an aqueous polyurethane condom prepared by the method described above.
[0014] In one embodiment, the thickness of the waterborne polyurethane condom is 0.02mm-0.06mm.
[0015] In one embodiment, the aqueous polyurethane condom includes any one or more of the following features:
[0016] 100% tensile modulus less than or equal to 2.0 MPa;
[0017] The explosive volume is greater than or equal to 12 liters;
[0018] The burst pressure is greater than or equal to 1 kPa;
[0019] Elongation at break is greater than or equal to 650%;
[0020] Tensile strength is greater than or equal to 20 MPa.
[0021] As described above, the present invention provides a low-modulus, high-burst-volume polyurethane condom and its preparation method, which has the following beneficial effects: By using a low-modulus, high-elongation waterborne polyurethane resin and a multiple impregnation and drying molding process, the present invention enables the prepared low-modulus, high-burst-volume polyurethane condom to achieve the following performance indicators: product thickness 0.02-0.06 mm, 100% tensile modulus ≤ 2.0 MPa, burst volume ≥ 12 liters, and burst pressure ≥ 1 kPa. Attached Figure Description
[0022] Figure 1 The diagram shown is a flowchart of the preparation method of the present invention. Detailed Implementation
[0023] The following specific examples illustrate the embodiments of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. Note that the performance tests of the polyurethane resin and the condom described in this invention were conducted in accordance with national standards GB / T1040.1-2006 and GB7544-2009, respectively. Unless otherwise specified, "%" and "parts" as used herein refer to "mass %" and "parts by mass," respectively.
[0024] Please see Figure 1 This invention first provides a method for preparing a high burst volume waterborne polyurethane condom, the method comprising multiple impregnations with waterborne polyurethane resin, and the method comprising at least steps S1-S4:
[0025] S1: Provides water-based polyurethane;
[0026] S2: After impregnation with the waterborne polyurethane, dry it, and repeat the impregnation and drying process N times to obtain a waterborne polyurethane.
[0027] Polyurethane film;
[0028] S3: After curling the edges of the water-based polyurethane film, dry it;
[0029] S4: The water-based polyurethane condom is obtained by impregnating the release agent, followed by drying, demolding, and electrical testing.
[0030] Wherein, N = 1-5, the waterborne polyurethane is anionic waterborne polyurethane, the 100% tensile modulus of the waterborne polyurethane is less than or equal to 2.0 MPa, and the elongation at break is greater than or equal to 650%.
[0031] In step S1, to prepare the waterborne polyurethane condom, the present invention provides an anionic waterborne polyurethane with good tensile modulus and elongation at break. The 100% tensile modulus of the anionic polyurethane can be less than or equal to 2.0 MPa, for example, 1.8 MPa, 1.5 MPa, 1.4 MPa, or 1.3 MPa. The elongation at break of the anionic waterborne polyurethane can be greater than or equal to 650%, for example, 720%, 730%, or 750%. The waterborne polyurethane provided by the present invention enables the final waterborne polyurethane condom to have an excellent burst volume greater than 12 liters. The anionic waterborne polyurethane resin used in the present invention has a mature process and has the advantage of a large molecular weight under the premise of low modulus. The solid content of the waterborne polyurethane resin can be between 15-30%, for example, 20% or 25%. The waterborne polyurethane resin in the above solid content range has the advantages of good resin leveling, small uniformity difference of the prepared condom, large burst volume, and few defects.
[0032] The waterborne polyurethane of this invention can be synthesized using a stepwise method. The waterborne polyurethane can be prepared from solid raw materials and dispersed in water. The stepwise method may include processes such as polymerization, chain extension, and emulsification. The solid raw materials of the waterborne polyurethane may include soft segments and hard segments. The soft segments may be macromolecular polyols or compositions of macromolecular polyols, and the hard segments may be polyisocyanates or compositions of polyisocyanates. The macromolecular polyols may include macromolecular diols and macromolecular triols, such as polytetrahydrofuran glycol (PTMEG), polypropylene glycol (PPG), and propylene oxide triol. Specifically, the molecular weight of the polytetrahydrofuran glycol may be 500-4000, the molecular weight of the polypropylene glycol may be 1000-5000, and the molecular weight of the propylene oxide triol may be 650-6000.
[0033] In one embodiment, the waterborne polyurethane is composed of the following solid raw materials in parts by weight: 23-38 parts of macromolecular diol, 3-5 parts of macromolecular triol, 6.5-10 parts of polyisocyanate, 1.3-1.6 parts of hydrophilic chain extender, 0.05-0.08 parts of small molecule polyol chain extender, 1-1.3 parts of neutralizer, 0.2-0.3 parts of small molecule amine chain extender, and 0.05-0.08 parts of catalyst.
[0034] The hydrophilic chain extender may be one or more of dimethylolpropionic acid, dimethylolbutyric acid, and sodium ethylenediamine ethanesulfonate; the small molecule polyol chain extender may include one or more of trimethylolpropane, glycerol, butanediol, ethylene glycol, and cyclohexanediol; the neutralizing agent may include one or more of triethylamine and sodium bicarbonate; and the small molecule post-amine chain extender may be one or more of ethylenediamine, hexamethylenediamine, isofluranediamine, toluenediamine, and diaminodicyclohexylmethane. The polyisocyanate may be one or more of TDI, MDI, IPDI, HDI, and HMDI.
[0035] In one embodiment, the waterborne polyurethane is composed of the following solid raw materials in parts by weight: 8-13 parts PTMEG, 15-25 parts PPG, 3-5 parts propylene oxide triol, 5.5-8 parts IPDI, 1-2 parts HDI, 1.3-1.6 parts DMPA and 0.5-0.8 parts DEG, 0.05-0.08 parts catalyst, 1-1.3 parts triethylamine, and 0.2-0.3 parts isophorone diamine.
[0036] In one embodiment, the macromolecular polyol is composed of a difunctional macromolecular polyol with a molecular weight of 500-4000 and a trifunctional macromolecular polyol with a molecular weight of 650-6000 in a mass ratio of 4:(0.2-1.5). Further, the macromolecular polyol is composed of polytetrahydrofuran glycol (PTMEG) with a molecular weight of 500-4000, polypropylene glycol (PPG) with a molecular weight of 1000-5000, and propylene oxide triol with a molecular weight of 650-6000 in a mass ratio of 1:3:(0.2-1.5).
[0037] The proportion of soft segments in the waterborne polyurethane resin can be 60-85% of all solid raw materials, for example, 79.5%. The crosslinking ratio of the soft segments can be 10-40%, for example, 25%. The crosslinking ratio of the soft segments can be defined as the mass ratio of macromolecular polyols with three or more functions to the total mass of macromolecular polyols.
[0038] In step S2, the preparation of the waterborne polyurethane condom further includes a process of multiple impregnation and drying to form a waterborne polyurethane film. For example, the mold can be impregnated with the waterborne polyurethane and then dried, and this process can be repeated N times. The number of repetitions N can be 1-5 times, such as 2 times or 3 times. This invention, through a multiple impregnation process, can achieve good uniformity of condom thickness, fewer defects, a large burst volume, and facilitate drying without wrinkles or cracks. The waterborne polyurethane in this invention requires a drying step after each impregnation. The drying after each impregnation can be a shaping drying, and the shaping drying time can be 2-10 minutes.
[0039] In step S3, the waterborne polyurethane film can be dried again after being rolled at the edges. This drying can be a molding drying process, and the molding drying time can be 10-65 minutes. In steps S2-S4, the drying temperature can be 80-140℃, for example, 120℃ or 130℃.
[0040] This invention allows for testing the tensile strength of the polyurethane film after each impregnation with polyurethane. For example, drying can be stopped and the next impregnation can proceed when the tensile strength of the polyurethane film reaches 60% of the predetermined tensile strength. The predetermined tensile strength can be, for example, greater than or equal to 20 MPa. The invention specifies a drying time after each impregnation. For instance, after the first impregnation, the tensile strength of the polyurethane film is tested. If the tensile strength of the polyurethane film reaches 60% of the predetermined tensile strength, the drying time used at this point can be the shaping drying time described in this invention. The shaping drying time used in this invention can be greater than or equal to the drying time used when the tensile strength of the polyurethane film formed by the first impregnation with water-based polyurethane reaches 60% of the predetermined tensile strength. The shaping drying time can follow a specific time interval. 成 =90·Φ-1.8·(N+2)t 定 The relationship between t 成 For molding and drying time, t 定 Where N is the shaping and drying time, Φ is the number of impregnation repetitions, Φ is the temperature influence factor (Φ = 2.7 - 0.015·T), and T is the temperature for shaping and drying (in degrees Celsius). The shaping and drying times are measured in minutes. In one embodiment, the shaping and drying temperatures are the same when using the above relationship. Using the above relationship between the shaping and drying times ensures optimal performance of the final condom, avoiding defects such as brittleness due to excessive drying time or insufficient strength due to insufficient drying time.
[0041] In step S4, the drying time after impregnation with the release agent can be 2-30 minutes.
[0042] This invention also provides a low-modulus, high-burst-volume water-based polyurethane condom. The water-based polyurethane condom can be a thin condom with a thickness between 0.02mm and 0.06mm, for example, 0.03mm. The polyurethane condom has good tensile modulus and burst volume. The 100% tensile modulus of the polyurethane condom can be less than or equal to 2.0MPa, for example, 1.8MPa, 1.3MPa, or 1.4MPa. The burst volume of the polyurethane condom can be greater than 12 liters, for example, 15 liters, 17 liters, 18 liters, or 20 liters. In one embodiment, the polyurethane condom also has good elongation at break, which can be greater than or equal to 650%, for example, 720% or 750%. The burst pressure of the condom can be greater than or equal to 1 kPa, for example, 1.3 kPa or 1.4 kPa. The tensile strength of the polyurethane condom can be greater than or equal to 20 MPa, for example, 30 MPa, 31 MPa, 32 MPa, or 33 MPa. Here, the polyurethane condom can be a male condom, but it should be understood that it can also be made into a female condom, as well as other non-standard condoms.
[0043] The present invention will be described in more detail below with reference to specific embodiments.
[0044] Example
[0045] Example 1
[0046] 4.73 kg of PTMEG 3000, 9.47 kg of PPG 3000, and 4.2 kg of propylene oxide triol with a molecular weight of 5000 were added to a reactor. 2.92 kg of IPDI and 0.75 kg of HDI were also added. The mixture was stirred and heated to 80-120°C, and the reaction was maintained at this temperature for 1-3 hours. Then, 0.72 kg of DMPA, 0.31 kg of DEG, 6.5 kg of acetone, and 0.04 kg of catalyst were added, and the reaction was carried out at 70-90°C for 2-6 hours. The mixture was then cooled, and triethylamine was added for neutralization. Water was then added for high-speed dispersion and emulsification. Finally, 0.15 kg of isophorone diamine was added for post-chain extension, followed by vacuum solvent removal to obtain the desired waterborne polyurethane resin emulsion. The 100% tensile modulus of the prepared polyurethane resin was measured to be 1.69 MPa, and the elongation at break was 811%.
[0047] The glass mold was cleaned and heated to 30-40℃. The mold was then impregnated with the polyurethane resin prepared above five times. After each impregnation, the mold was shaped and dried at 140℃ for 4 minutes. After edge rolling, the mold was shaped and dried at 140℃ for 10.8 minutes. Then, the mold was impregnated with a release agent and dried at 80℃. After demolding, the mold was subjected to electrical testing, inner packaging, and outer packaging to obtain sample 1. The thickness of sample 1 was 0.032 mm. The 100% tensile modulus of sample 1 was 1.7 MPa, the burst volume was 18.9 liters, the elongation at break was 805%, the burst pressure was 2.8 kPa, and the tensile strength was 33 MPa.
[0048] Example 2
[0049] The glass mold was cleaned and heated to 30-40°C. The mold was then impregnated with the polyurethane resin obtained in Example 1 four times. After each impregnation, the mold was shaped and dried at 120°C for 6 minutes. After edge rolling, the mold was shaped and dried at 120°C for 27 minutes. The mold was then impregnated with a release agent and dried at 80°C. After demolding, the mold was subjected to electrical testing, inner packaging, and outer packaging to obtain Sample 2. The thickness of Sample 2 was 0.038 mm. The 100% tensile modulus of Sample 2 was 1.69 MPa. The burst volume was 19.5 liters, the elongation at break was 812%, the burst pressure was 3.7 kPa, and the tensile strength was 32 MPa.
[0050] Example 3
[0051] The glass mold was cleaned and heated to 30-40°C. The mold was then impregnated with the polyurethane resin obtained in Example 1 three times. After each impregnation, the mold was shaped and dried at 80°C for 10 minutes. After edge rolling, the mold was shaped and dried at 80°C for 63 minutes. The mold was then impregnated with a release agent and dried at 80°C. After demolding, the mold was subjected to electrical testing, inner packaging, and outer packaging to obtain Sample 3. The thickness of Sample 3 was 0.026 mm. The 100% tensile modulus of Sample 3 was 1.67 MPa, the burst volume was 18.2 liters, the elongation at break was 801%, the burst pressure was 2.0 kPa, and the tensile strength was 30 MPa.
[0052] Comparative Example 1
[0053] The preparation conditions of Comparative Example 1 and Example 2 were the same. The molding and drying time of Sample 2 in Example 2 was changed to 37 minutes to obtain Comparative Sample 1. The product thickness of Comparative Sample 1 was 0.038 mm, the 100% tensile modulus was 1.9 MPa, the burst volume was 15.4 liters, the elongation at break was 721%, the burst pressure was 2 kPa, and the tensile strength was 25 MPa.
[0054] Comparative Example 2
[0055] The preparation conditions for Comparative Example 2 and Example 2 were the same. The molding and drying time of Sample 2 in Example 2 was changed to 32 minutes to obtain Comparative Sample 2. The product thickness of Comparative Sample 2 was 0.038 mm, the 100% tensile modulus was 1.79 MPa, the burst volume was 16.2 liters, the elongation at break was 761%, the burst pressure was 2.4 kPa, and the tensile strength was 26.5 MPa.
[0056] Comparative Example 3
[0057] The preparation conditions of Comparative Example 3 and Example 2 were the same. The molding and drying time of Sample 2 in Example 2 was changed to 22 minutes to obtain Comparative Sample 3. The product thickness of Comparative Sample 3 was 0.038 mm, the 100% tensile modulus was 1.54 MPa, its burst volume was 21.2 liters, the elongation at break was 856%, the burst pressure was 2.6 kPa, and the tensile strength was 27.3 MPa.
[0058] Comparative Example 4
[0059] The preparation conditions of Comparative Example 4 and Example 2 were the same. The molding and drying time of Sample 2 in Example 2 was changed to 17 minutes to obtain Comparative Sample 4. The product thickness of Comparative Sample 4 was 0.038 mm, the 100% tensile modulus was 1.3 MPa, the burst volume was 24 liters, the elongation at break was 921%, the burst pressure was 1.6 kPa, and the tensile strength was 23.1 MPa.
[0060] Therefore, this invention effectively overcomes the various shortcomings of the prior art and has high industrial applicability. The above embodiments are merely illustrative of the principles and effects of this invention and are not intended to limit the invention. Any person skilled in the art can modify or change the above embodiments without departing from the spirit and scope of this invention. Therefore, all equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical concept disclosed in this invention should still be covered by the claims of this invention.
Claims
1. A method for preparing a high burst volume waterborne polyurethane condom, characterized in that, The method includes at least the following steps: Provides waterborne polyurethane; After impregnation with the waterborne polyurethane, the process is dried, and the process of impregnation with the waterborne polyurethane and drying is repeated N times to obtain a waterborne polyurethane film. After curling the edges of the water-based polyurethane film, it is dried. The water-based polyurethane condom is obtained by impregnating it with a release agent, followed by drying, demolding, and electrical testing. Wherein, N=1-5, the waterborne polyurethane is anionic waterborne polyurethane, the 100% tensile modulus of the waterborne polyurethane condom is less than or equal to 2.0 MPa, and the elongation at break is greater than or equal to 650%; Drying the water-based polyurethane film after edge curling is called molding drying, and drying the water-based polyurethane film after impregnation is called setting drying. The setting drying time and the molding drying time have a relationship t. 成 =90•Φ-1.8•(N+2)•t 定 The relationship between t 成 For molding and drying time, t 定 Φ represents the shaping and drying time, N represents the number of impregnation repetitions, Φ = 2.7 - 0.015•T, T represents the temperature for shaping and drying, and the unit of T is degrees Celsius. 定 and t 成 The unit is minutes.
2. The method according to claim 1, characterized in that: The setting and drying time is 2-10 minutes, the molding and drying time is 10-65 minutes, and the release agent drying time is 2-30 minutes.
3. The method according to claim 1, characterized in that: The drying temperature is 80-140°C. o C.
4. The method according to claim 1, characterized in that: The solid content of the waterborne polyurethane is 15-30%.
5. The method according to claim 1, characterized in that: The proportion of macromolecular polyols in the raw material components other than water in the waterborne polyurethane is 60-85%, and the proportion of macromolecular polyols having three or more functions is 10-40%.
6. The method according to claim 5, characterized in that: The macromolecular polyol is composed of difunctional macromolecular polyols with a molecular weight of 500-4000 and trifunctional macromolecular polyols with a molecular weight of 650-6000 in a mass ratio of 4:(0.2-1.5).
7. A high burst volume waterborne polyurethane condom prepared by the method according to any one of claims 1-6.
8. The waterborne polyurethane condom according to claim 7, characterized in that: The thickness of the water-based polyurethane condom is 0.02mm-0.06mm.
9. The waterborne polyurethane condom according to claim 7, characterized in that: The aqueous polyurethane condom includes any one or more of the following features: 100% tensile modulus less than or equal to 2.0 MPa; The explosive volume is greater than or equal to 12 liters; The burst pressure is greater than or equal to 1 kPa; Elongation at break is greater than or equal to 650%; Tensile strength is greater than or equal to 20 MPa.
Citation Information
Patent Citations
Method for preparing universal or composite waterborne polyurethane condom
CN103640133A
Pure polyurethane condom with adhesive layer, and preparation method of pure polyurethane condom