Preparation of modified zeolite catalyst, modified zeolite catalyst and ozone purification method

By mixing a metal salt solution with zeolite and using microwave drying technology, the distribution of metal clusters within the zeolite framework is adjusted, which solves the problems of complex preparation and low catalytic activity of modified zeolite catalysts in the existing technology, and achieves efficient and stable ozone production. Purifying effect.

CN117000232BActive Publication Date: 2024-10-22UNIV OF SCI & TECH BEIJING
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311019990.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-14
Publication Date
2024-10-22
Estimated Expiration
2043-08-14

AI Technical Summary

Technical Problem

The preparation method of existing modified zeolite catalysts is complicated, the amount of waste liquid is large, which leads to environmental pollution, and the catalytic activity is low, making it difficult to ensure long-term stability and high efficiency. Especially under low temperature conditions, the catalytic activity is insufficient and the uniformity of metal ion clusters is lacking. dispersion.

Method used

The metal salt solution is mixed with zeolite to form a non-Newtonian fluid mixture, which is dried and calcined by microwave to adjust the distribution of metal clusters in the zeolite framework to ensure the uniform distribution and stability of metal ions in the pores and improve the catalytic activity.

Benefits of technology

It achieves efficient ozone purification, maintains O3 removal rate ≥90% for up to 2000 minutes, has good low-temperature catalytic activity and stability, and reduces the energy consumption and time of catalyst preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117000232B_ABST
    Figure CN117000232B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of modified zeolite preparation, and specifically relates to the preparation of modified zeolite catalysts, modified zeolite catalysts and ozone purification methods. The preparation method comprises mixing a metal salt solution with a zeolite to form a non-Newtonian fluid mixture, drying the mixture with microwaves, and finally calcining to obtain the zeolite catalyst. The preparation method uses microwaves to dry the mixture of the metal salt solution and the zeolite, with a short drying time and fast water evaporation, and can retain the state of metal cations in the zeolite framework, thereby preventing catalyst particles (metal clusters) from escaping from the zeolite framework and aggregating. The zeolite catalyst prepared by the preparation method contains metal clusters and the metal clusters are evenly dispersed, and has active components composed of multiple metal cations. The metal clusters of the zeolite catalyst have higher catalytic activity, play a vital role in the catalytic decomposition process of ozone (O3), and improve the low-temperature catalytic oxidation efficiency of O3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of modified zeolite preparation, and in particular relates to the preparation of a modified zeolite catalyst, a modified zeolite catalyst and an ozone purification method. Background Art

[0002] Ozone (O3) is a strong oxidizing gas composed of three oxygen atoms, which exists in the Earth's stratosphere (about 15-30 kilometers from the surface) and troposphere (within about 15 kilometers from the surface). Stratospheric O3 is mainly formed by the interaction between oxygen molecules (O2) under ultraviolet radiation. Stratospheric O3 can absorb ultraviolet rays in the range of 200-300nm, reducing the amount of harmful ultraviolet radiation reaching the Earth's surface, thereby protecting the Earth's creatures. O3 in the troposphere is mainly formed by photochemical reactions between volatile organic compounds (VOCs) and nitrogen oxides (NOx). Tropospheric O3 is a greenhouse gas that causes global warming and affects air quality and the Earth's ecosystem. Long-term exposure to O3 can have adverse effects on human health, causing cardiopulmonary and respiratory diseases, including changes in blood pressure and peripheral white blood cell counts, respiratory deterioration, lung dysfunction, asthma and chronic obstructive pulmonary disease.

[0003] Common ozone catalytic purification materials include activated carbon, precious metal-loaded catalysts, transition metal oxides and zeolite molecular sieves. Activated carbon is low-cost and easy to obtain, but there are safety hazards of explosion and explosion, and the structure is easily corroded by ozone after long-term use; precious metal-loaded catalysts have high purification efficiency, but are expensive; transition metal oxides are cheap and highly active under dry conditions, but there is a problem of catalytic site deactivation under long-term operation conditions. Zeolite is a typical microporous inorganic material composed of AlO4 and SiO4 tetrahedrons, with micro-mesoporous channels and sufficient catalytic active sites. It is gradually regarded as a suitable material for ozone catalytic purification and has attracted widespread attention.

[0004] Unlike transition metal oxides, in high specific surface area (up to 800m 2 / g), large pore volume, and zeolites with special acid sites include both physical adsorption on the pores and catalytic decomposition on Lewis acid sites (LAS). The tiny pore size similar to that of ozone molecules promotes the interaction between ozone molecules and LAS. According to adsorption theory, this effect is more significant at lower temperatures. Studies have found that the content and dispersion of LAS are related to the framework structure, silicon-aluminum ratio, cation type, and ion exchange method of the zeolite, among which the type and distribution of metal cations are the main factors affecting catalytic activity. Therefore, by ion-modifying the zeolite and controlling the state of cations on the zeolite exchange sites, the ozone conversion efficiency can be adjusted and selected to a large extent.

[0005] The salt solution stirring and impregnation method is a traditional liquid phase zeolite modification method. The zeolite is immersed in a prepared metal salt solution, and ion exchange is promoted by heating and stirring. Then, it is repeatedly washed with deionized water, and the modified zeolite powder is obtained after drying and calcination. This technology has the following disadvantages: ① The modification process is complicated, the amount of waste liquid is large, it is easy to cause environmental pollution, and it is not suitable for industrial applications; ② The degree of ion exchange is low, it is difficult to ensure the content of catalytically active components, and the metal in the modified zeolite framework is a single ion with low catalytic activity; ③ The slow evaporation of water vapor during the drying process will cause the metal ions to detach from the zeolite framework with water molecules and agglomerate on the zeolite surface.

[0006] In addition, in the prior art, the low-temperature catalytic activity of traditional ozone catalysts is low, and they are easily irreversibly deactivated in long-term use, and have poor regeneration performance. The existing modified zeolites have low metal ion exchange rates and use single metal ions as active components, resulting in low catalytic activity. There is currently no O3 zeolite catalyst with uniform and highly dispersed metal ion clusters. Summary of the invention

[0007] In order to solve the above problems, the present invention proposes a preparation method of a modified zeolite catalyst, a modified zeolite catalyst and an ozone purification method. The zeolite catalyst prepared by the preparation method

[0008] The present invention is achieved through the following technical solutions:

[0009] The first aspect of the present invention is to provide a method for preparing a modified zeolite catalyst, which adjusts the metal clusters in the modified zeolite framework, including mixing a metal salt solution with zeolite to form a non-Newtonian fluid mixture, drying the mixture with microwaves, and finally calcining to obtain the zeolite catalyst.

[0010] Furthermore, the preparation method specifically comprises the following steps:

[0011] The metal salt solution and the zeolite are respectively prepared in a specified ratio;

[0012] Preparing a non-Newtonian fluid mixture: mixing the metal salt solution and the zeolite with stirring to obtain the non-Newtonian fluid mixture;

[0013] Microwave drying the non-Newtonian fluid mixture;

[0014] The non-Newtonian fluid mixture after drying is calcined to obtain the zeolite catalyst.

[0015] Further, configuring the metal salt solution specifically includes:

[0016] Determine the amount of metal salt: Calculate the mass of the metal salt based on the silicon-aluminum ratio and the theoretical ion exchange degree;

[0017] Determine the amount of water required to prepare the metal salt solution: add deionized water dropwise to an equal amount of the zeolite, stir evenly until it becomes a non-Newtonian fluid state, and the amount of water added is the amount of water required to prepare the metal salt solution;

[0018] mixing the metal salt with the amount of water to obtain the metal salt solution;

[0019] Furthermore, the molar ratio of the metal salt to the zeolite is in the range of 0 to 5, excluding 0.

[0020] Furthermore, the metal salt includes nitrate and / or acetate.

[0021] Furthermore, the metal clusters include: Mn 2+ 、Mn2O 2+ 、Mn3O3 2+ 、[AlO2] + , [MnCuO] 2+ 、[Mn2CuO3] 2+ and [FeCoO] 2+ One, two or more of the following.

[0022] Further, microwave drying the non-Newtonian fluid mixture specifically comprises:

[0023] The mixture is evenly spread into a crucible, an evaporating dish or a stainless steel beaker, and then quickly heated for 30s-30min using a microwave reactor at a power of 100-1000w; water of the mixture will evaporate quickly during microwave heating, and the polymer of metal salt ions will be locked in the zeolite pores to prevent them from adhering to the zeolite surface due to evaporation of water; at this time, at least one initial cluster is evenly distributed in the pores of the zeolite powder, and the initial cluster includes metal ions and nitrate ions.

[0024] The second aspect of the present invention is to provide a modified zeolite catalyst, wherein the zeolite catalyst is prepared by the above-mentioned preparation method of the modified zeolite catalyst, wherein a plurality of metal clusters are evenly distributed in the pores of the zeolite powder in the zeolite catalyst; the metal clusters include metal ions and compatible oxygen atoms;

[0025] The number of the metal ions is at least 1; preferably, the number of the metal ions is 1-5.

[0026] The third aspect of the present invention is to provide an ozone purification method, wherein the ozone purification method uses the above-mentioned zeolite catalyst to purify ozone; the zeolite catalyst is at -10 to 300°C and the air velocity is 1×10 4 ~2×10 6 h -1Ozone is removed under the conditions of , and the O3 removal rate is maintained at ≥ 90% for up to 2000min.

[0027] Furthermore, the zeolite catalyst is at room temperature and the flow rate is 1.0 L min -1 Under the conditions, the O3 removal rate is maintained at ≥90% for up to 2000 min.

[0028] Furthermore, the scope of the ozone purification includes low-temperature, large-flow aircraft cabin ozone removal, factory ozone waste gas treatment, and indoor ozone purification.

[0029] Furthermore, the zeolite catalyst forms include but are not limited to powder catalysts, granular catalysts (made by mixing with an adhesive) and monolithic catalysts (extruded or coated).

[0030] The preparation method of the modified zeolite catalyst provided in the first aspect of the present invention comprises mixing a metal salt solution with a zeolite to form a non-Newtonian fluid mixture, drying the mixture by microwaves, and finally calcining to obtain the zeolite catalyst. The preparation method adjusts the metal clusters in the modified zeolite framework, calculates the amount of metal salt according to the silicon-aluminum ratio and the theoretical ion exchange degree, and then calculates the amount of water in the metal salt solution according to the target exchange state, so that the polymer formed by the metal cation and the water molecule is evenly distributed in the zeolite pores, and the metal ion exchange degree is adjustable and controllable. The preparation method uses microwaves to dry the mixture of the metal salt solution and the zeolite, the drying time is short, the water evaporates quickly, and the state of the metal cations in the zeolite framework can be retained, and the catalyst particles (metal clusters) are prevented from escaping from the zeolite framework and aggregating. In addition, the preparation method adopts a simple process of mixing and stirring, avoiding a long-term heating and stirring process. The catalyst preparation time is greatly shortened, and the energy consumption of the catalyst preparation process is greatly reduced.

[0031] The second aspect of the present invention provides a modified zeolite catalyst, wherein the zeolite catalyst has a cluster composed of multiple metal cations as catalytically active components, and the clusters are evenly distributed. Compared with the conventional modified zeolite catalyst with a single cation exchange, the metal clusters of the zeolite catalyst have higher catalytic activity, play a vital role in the catalytic decomposition of ozone (O3), and improve the catalyst's O3 low-temperature catalytic oxidation efficiency. The zeolite catalyst has good low-temperature catalytic activity and stability, and can be used at room temperature with a flow rate of 1.0 L min -1 Under the condition of , the removal rate of O3 can be maintained at ≥ 90% for up to 2000 min. In addition, the catalyst has good regeneration performance and can restore the catalytic activity well after low-temperature regeneration at 150°C.

[0032] The ozone purification method provided by the third aspect of the present invention can maintain an O3 removal rate of ≥ 90% for up to 2000 min; it is suitable for ozone removal in low-temperature, large-flow aircraft cabins, factory ozone waste gas treatment, indoor ozone purification, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The zeolite catalysts (D1-Mn-FAU and D2-Mn-FAU) prepared by a preparation method of a modified zeolite catalyst in the embodiment of the present invention and the catalysts (T1-Mn-FAU and T2-Mn-FAU) prepared by an existing conventional liquid phase modification method were tested at an ozone concentration of 20 ppm, room temperature, and a flow rate of 1.0 L min -1 Schematic diagram of ozone conversion performance test results under conditions.

[0034] Figure 2 The zeolite catalyst D2-Mn-FAU prepared by the preparation method of a modified zeolite catalyst in the embodiment of the present invention is subjected to an ozone concentration of 20 ppm, room temperature, and a flow rate of 1.0 L·min -1 Regeneration performance test curve under conditions.

[0035] Figure 3 Schematic diagram comparing XRD characterization results of zeolite catalysts (D1-Mn-FAU and D2-Mn-FAU) prepared by a method for preparing a modified zeolite catalyst in an embodiment of the present invention and zeolite raw powder (FAU zeolite).

[0036] Figure 4 The single metal cluster catalyst (D1-Mn-FAU) and the multi-metal cluster catalyst (D1-Mn2Cu-FAU) of the zeolite catalyst prepared by the preparation method of the embodiment of the present invention were subjected to ozone concentration of 20 ppm, room temperature and flow rate of 1.0 L min -1 Schematic diagram of efficiency curve under different conditions.

[0037] Figure 5 This is a schematic diagram showing that polyatomic metal clusters in a zeolite catalyst prepared by a method for preparing a modified zeolite catalyst in an embodiment of the present invention are located in a zeolite framework structure.

[0038] Figure 6 The figure is a schematic diagram of the calculation results of the reaction energy and transition state energy barrier of the modified catalyst obtained by the preparation method described in this embodiment using the CASTEP (plane wave pseudopotential method) module in Materials studio (material simulation calculation software). DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0040] On the contrary, the present invention covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present invention as defined by the claims. Further, in order to make the public have a better understanding of the present invention, some specific details are described in detail in the following detailed description of the present invention. Those skilled in the art can fully understand the present invention without the description of these details.

[0041] The following examples serve to illustrate the present invention. In the examples, unless otherwise indicated, parts are by weight, percentages are by weight, and temperatures are in degrees Celsius. The relationship between parts by weight and parts by volume is the same as the relationship between grams and cubic centimeters.

[0042] The term "MFI" stands for "Mobil five Instructure" in English, and both MFI and FUA are types of zeolite topological structures.

[0043] The first aspect of the embodiment of the present invention provides a method for preparing a modified zeolite catalyst, which adjusts the metal clusters in the modified zeolite framework, including mixing a metal salt solution with zeolite to form a non-Newtonian fluid mixture, using microwaves to dry the mixture, and finally calcining to obtain the modified zeolite catalyst.

[0044] A method for preparing a modified zeolite catalyst proposed in the first aspect of an embodiment of the present invention includes mixing a metal salt solution with a zeolite to form a non-Newtonian fluid mixture, drying the mixture with microwaves, and finally calcining to obtain a modified zeolite. The preparation method adjusts the metal clusters in the modified zeolite framework, calculates the amount of metal salt according to the silicon-aluminum ratio and the theoretical ion exchange degree, and then calculates the amount of water in the metal salt solution according to the target exchange state, so that the polymer formed by the metal cation and the water molecule is evenly distributed in the zeolite pores, and the metal ion exchange degree is adjustable and controllable. The preparation method uses microwaves to dry the mixture of the metal salt solution and the zeolite, the drying time is short, the water evaporates quickly, and the state of the metal cations in the zeolite framework can be retained, and the catalyst particles (metal clusters) are prevented from escaping from the zeolite framework and aggregating. In addition, the preparation method adopts a simple process of mixing and stirring, which avoids long-term heating and stirring processes. The catalyst preparation time is greatly shortened, and the energy consumption of the catalyst preparation process is greatly reduced.

[0045] In some embodiments of the present invention, a method for preparing a modified zeolite catalyst is provided, and the preparation method specifically comprises the following steps:

[0046] S1, preparing metal salt solution and zeolite in a specified ratio;

[0047] S2: preparing a non-Newtonian fluid mixture: mixing and stirring the metal salt solution prepared in S1 with the zeolite to obtain a non-Newtonian fluid mixture;

[0048] S3 microwave drying of non-Newtonian fluid mixture;

[0049] S4 calcines the dried non-Newtonian fluid mixture to obtain a modified zeolite catalyst.

[0050] In some embodiments of the present invention, in the above step S1, preparing the metal salt solution specifically includes:

[0051] S1.1 Determine the amount of metal salt used: calculate the mass of the metal salt based on the silicon-aluminum ratio and the theoretical ion exchange degree; the amount of metal salt added is calculated from the silicon-aluminum ratio of the zeolite and the theoretical exchange rate; the silicon-aluminum ratio of the zeolite is any number greater than 1, and the target exchange state is a metal cluster with 1-5 metal ions; the amount of metal salt used is small, the cost is low, and no waste liquid is generated, which is environmentally friendly.

[0052] S1.2 Determine the amount of water required in the metal salt solution: add deionized water dropwise to the same amount of zeolite as in S2, and stir evenly to make it in a non-Newtonian fluid state; the amount of deionized water added at this time is the amount of metal salt solution prepared;

[0053] S1.3 Mix the metal salt in S1.1 with the water in S1.2 to obtain a metal salt solution. The calculated metal salt solution is mixed with the zeolite, which not only ensures the metal ion loading of the zeolite, but also makes the ion exchange degree adjustable and controllable. The type and aggregation state of the metal ions in the zeolite pores are determined by the calculated dosage.

[0054] In some embodiments of the present invention, in the above step S2, the specific contents include adding the prepared metal salt solution dropwise into the zeolite, and stirring evenly at the same time, so that the mixture is in a non-Newtonian fluid state; the purpose of this operation is to make the metal salt ions and water form charged ionic polymers, which are evenly distributed in the zeolite pores.

[0055] In some embodiments of the present invention, taking a single metal cation exchange, nitrate, as an example, the calculation method of the required amount of metal salt is as follows:

[0056] The molecular formula of the zeolite molecular sieve used is H(AlO2)(SiO2) n , n is an arbitrary number not less than 1; the theoretical exchange of metal clusters is [M x O y ] z+ , M is metal, 0<x≤5、0≤y≤5、z> 0, x, y, z are all integers;

[0057] To modify 1 mol of zeolite molecular sieve, (x / z) mol of metal cations are required, (x / z) mol of nitrate (or (x / z) mol of acetate) are required;

[0058] The mass of nitrate was calculated based on the molar masses of zeolite molecular sieve and nitrate.

[0059] In some embodiments of the present invention, the molar ratio of the metal salt to the zeolite is in the range of 0 to 5, excluding 0.

[0060] In some embodiments of the present invention, the metal salt is nitrate and / or acetate. Both types of salts are easily soluble in water, and the metals in the metal salt solution after being dissolved in water are all free metal ions, which is convenient for subsequent ion exchange.

[0061] In some embodiments of the invention, the nitrates include nitrates of manganese, cobalt, copper, cerium, tin, lanthanum, praseodymium, samarium, europium, gadolinium, potassium, calcium, zinc, magnesium, and nickel.

[0062] In some embodiments of the invention, the acetate salts include acetate salts of manganese, cobalt, copper, cerium, tin, lanthanum, praseodymium, samarium, europium, gadolinium, potassium, calcium, zinc, magnesium, and nickel.

[0063] In some embodiments of the present invention, the concentration of the metal salt solution is within the saturation concentration range.

[0064] In some embodiments of the present invention, in the above step S3, microwave drying the non-Newtonian fluid mixture specifically includes:

[0065] The non-Newtonian fluid mixture is evenly spread into a crucible, an evaporating dish or a stainless steel beaker, and then rapidly heated in a microwave reactor at a power of 100-1000W for 30s-30min;

[0066] The mixture will evaporate water quickly during microwave heating, locking the polymer of metal salt ions in the zeolite pores to prevent them from adhering to the zeolite surface due to evaporation of water; at this time, 1-5 initial clusters are evenly distributed in the pores of the zeolite powder, and the initial clusters include metal ions and nitrate ions. The microwave drying method is used to quickly evaporate water under high temperature and high pressure conditions, locking the metal ion polymer in the zeolite pores, preventing the metal ions from moving with water molecules, and retaining the polymerization state and position of the metal ions. A specific number of metal polymers have higher catalytic activity and can improve the low-temperature ozone conversion performance of the zeolite catalyst.

[0067] In some embodiments of the present invention, in the above step S4, the non-Newtonian fluid mixture after calcining and drying specifically includes:

[0068] The powder obtained by drying is calcined in an oven, hot plate, heating mantle, muffle furnace or tubular furnace at a temperature of 300-1200°C for 1-12h; calcination can remove nitrate ions in the zeolite pores (the product of nitrate and H ion exchange in zeolite is HNO3, which is decomposed and removed during calcination) and remaining water molecules to obtain metal clusters formed by metal ions and oxygen atoms; the zeolite catalyst powder obtained after calcination has high catalytic activity.

[0069] A second aspect of an embodiment of the present invention provides a modified zeolite catalyst, wherein the zeolite catalyst is prepared by the above-mentioned preparation method of the modified zeolite catalyst, wherein a plurality of metal clusters are evenly distributed in the pores of the zeolite powder in the zeolite catalyst; the metal clusters include metal ions and compatible oxygen atoms;

[0070] The number of metal ions is at least 1; preferably, the number of metal ions is 1-5.

[0071] The modified zeolite catalyst provided in the second aspect of the embodiment of the present invention has a cluster of metal cations as catalytically active components, and the clusters are evenly distributed. Compared with the traditional modified zeolite catalyst with a single cation exchange, the metal clusters of the zeolite catalyst have higher catalytic activity, which plays a vital role in the catalytic decomposition of ozone (O3), and improves the catalyst's O3 low-temperature catalytic oxidation efficiency. The zeolite catalyst has good low-temperature catalytic activity and stability, and can be used at room temperature with a flow rate of 1.0L·min -1 Under the condition of , the removal rate of O3 can be maintained at ≥ 90% for up to 2000min. In addition, the catalyst has good regeneration performance and can restore catalytic activity well after low-temperature regeneration at 150℃.

[0072] The third aspect of the embodiment of the present invention provides an ozone purification method, which uses the above-mentioned zeolite catalyst to purify ozone; the zeolite catalyst is at -10 to 300 ° C and the air velocity is 1×10 4 ~2×10 6 h -1 Ozone is removed under the conditions of , and the O3 removal rate is maintained at ≥ 90% for up to 2000min.

[0073] The ozone purification method provided in the third aspect of the embodiment of the present invention can maintain an O3 removal rate of ≥ 90% for up to 2000 min; it is suitable for ozone removal in low-temperature, large-flow aircraft cabins, factory ozone waste gas treatment, indoor ozone purification, etc.

[0074] In some specific embodiments of the present invention, the zeolite catalyst is heated at room temperature and the flow rate is 1.0 L min -1 Under the conditions, the O3 removal rate is maintained at ≥90% for up to 2000 min.

[0075] In some specific embodiments of the present invention, the scope of ozone purification includes low-temperature, large-flow aircraft cabin ozone removal, factory ozone waste gas treatment, and indoor ozone purification.

[0076] In some specific embodiments of the present invention, the zeolite catalyst forms include but are not limited to powder catalysts, granular catalysts (made by mixing with a binder) and monolithic catalysts (extruded or coated).

[0077] The technical solution of the present invention is further described below in conjunction with embodiments.

[0078] Example 1

[0079] A method for preparing a modified zeolite catalyst comprises the following steps:

[0080] ① Measure FAU zeolite and 50wt% manganese nitrate solution;

[0081] ② Determine the amount of water required for modification: Weigh 10g of zeolite, add deionized water dropwise to the zeolite powder while stirring evenly until the mixture is in a non-Newtonian fluid state, then add 10.0ml of deionized water and record the required amount of water.

[0082] ③ Calculate the amount of zeolite and manganese nitrate solution: According to the silicon-aluminum ratio of the zeolite used and the theoretical exchange rate, weigh 10g of zeolite and 4.26g of 50wt.% manganese nitrate solution to prepare 10ml of solution.

[0083] ④ Add the prepared manganese nitrate solution dropwise into the zeolite powder while stirring evenly to make it into a non-Newtonian fluid state.

[0084] ⑤ Spread the mixture evenly into an evaporating dish and quickly dry it using a microwave reactor at 800 W power for 4 minutes.

[0085] ⑥ The dried powder was calcined in a muffle furnace at 350°C for 3 hours at a heating rate of 2°C / min to obtain a modified zeolite catalyst powder.

[0086] Example 2

[0087] A method for preparing a modified zeolite catalyst. The method for preparing a modified zeolite catalyst in this embodiment is basically the same as that in Example 1, except that the theoretical exchange rate of metal ions in this embodiment is 3.0, and the theoretical exchanged metal cluster is [Mn3O3] 2+ .

[0088] Example 3

[0089] A method for preparing a modified zeolite catalyst. The method for preparing a modified zeolite catalyst in this embodiment is basically the same as that in Example 1, except that the zeolite powder used is tZSM-5 with a topological structure of MFI.

[0090] Example 4

[0091] A method for preparing a modified zeolite catalyst. The method for preparing a modified zeolite catalyst in this embodiment is basically the same as that in Example 1, except that the drying power of the microwave reactor is 600 W and the drying time is 8 min.

[0092] Example 5

[0093] A method for preparing a modified zeolite catalyst. The method for preparing a modified zeolite catalyst in this embodiment is basically the same as that in Embodiment 1, except that the mixture is placed in an oven and dried at 160° C. for 2 hours.

[0094] Example 6

[0095] A method for preparing a modified zeolite catalyst. The method for preparing a modified zeolite catalyst in this embodiment is substantially the same as that in Embodiment 1, except that the dried powder is calcined at 450° C. for 3 h in a muffle furnace.

[0096] Example 7

[0097] A method for preparing a modified zeolite catalyst. The method for preparing a modified zeolite catalyst in this embodiment is basically the same as that in embodiment 1, except that: the theoretical exchange cluster is [Mn2CuO3] 2+ .

[0098] Example 8

[0099] A method for preparing a modified zeolite catalyst. The method for preparing a modified zeolite catalyst in this embodiment is basically the same as that in Example 1, except that:

[0100] The preparation method also includes step ⑦ of grinding the zeolite catalyst powder, mixing the obtained zeolite fine powder with an adhesive, an additive, and deionized water in a certain proportion, forming a spherical or cylindrical shape, and drying and calcining to obtain a granular zeolite catalyst.

[0101] Example 9

[0102] A method for preparing a modified zeolite catalyst. The method for preparing a modified zeolite catalyst in this embodiment is basically the same as that in Example 1, except that:

[0103] The preparation method also includes step ⑦ grinding the zeolite catalyst powder, mixing the zeolite fine powder with an adhesive, an additive, and deionized water in a certain proportion, extruding it into a honeycomb shape using a mold under a certain pressure, and obtaining an extruded honeycomb zeolite catalyst after drying and calcining.

[0104] Example 10

[0105] A method for preparing a modified zeolite catalyst. The method for preparing a modified zeolite catalyst in this embodiment is basically the same as that in Example 1, except that:

[0106] The preparation method also includes step ⑦ grinding the zeolite catalyst powder, mixing the zeolite fine powder with an adhesive, an additive, and deionized water in a certain proportion to prepare a slurry with a suitable viscosity, immersing the pre-prepared carrier in the slurry for 10s-30min, taking it out, drying, and calcining to obtain a coated monolithic catalyst. The carrier includes a metal carrier, a cordierite carrier, a glass or ceramic fiber carrier.

[0107] Comparative Example 1

[0108] The catalyst samples (T1-Mn-FAU and T2-Mn-FAU) were obtained by salt solution stirring impregnation method (the existing traditional liquid phase modification method).

[0109] Next, the modified zeolite catalysts prepared in Examples 1 to 10 and Comparative Example 1 were analyzed.

[0110] like Figure 1 As shown, the catalyst samples (T1-Mn-FAU and T2-Mn-FAU) obtained by the salt solution stirring impregnation method (the existing traditional liquid phase modification method) in Comparative Example 1 and the zeolite catalysts (D1-Mn-FAU and D2-Mn-FAU) prepared by the preparation method of Example 1 were subjected to an ozone concentration of 20 ppm, room temperature, and a flow rate of 1.0 L·min -1 Schematic diagram of ozone conversion performance test results under different conditions. Figure 1 It can be seen that the modified sample is tableted with a tablet press, then ground into broken particles, and the 40-60 mesh granular catalyst is screened out by the screen; 30-1000 mg of granular catalyst is filled into the reactor; the ozone concentration at the reactor inlet is maintained at 20ppm, and the ozone concentration C of the reactor outlet gas is monitored and recorded in real time. The ozone conversion efficiency curve is plotted with time as the x-axis and 1-C / 20 as the y-axis as shown in the figure. By comparing the ozone purification efficiency of zeolite catalysts obtained by different methods (salt solution stirring and impregnation method and DT method), it can be seen that the sample obtained by the salt solution stirring and impregnation method is rapidly deactivated after a period of testing, and the catalytic activity is much lower than that of D1-Mn-FAU and D2-Mn-FAU.

[0111] like Figure 2As shown, the zeolite catalyst D2-Mn-FAU prepared by the preparation method of a modified zeolite catalyst in Example 1 has an ozone concentration of 20 ppm, room temperature, and a flow rate of 1.0 L·min -1 Regeneration performance test curve under the conditions of Figure 2 It can be seen that the modified zeolite material can be regenerated under heating conditions at 150°C and the catalytic activity can be well restored.

[0112] like Figure 3 FIG. 1 is a schematic diagram showing the comparison of XRD characterization results of zeolite catalysts (D1-Mn-FAU and D2-Mn-FAU) prepared by the preparation method of a modified zeolite catalyst in an embodiment of the present invention and zeolite raw powder (FAU zeolite). Figure 3 It can be seen that there is no obvious difference in the XRD curves of the samples before and after modification, and the modification process will not destroy the framework structure of the zeolite.

[0113] like Figure 4 As shown, the single metal cluster catalyst (D1-Mn-FAU) and the multi-metal cluster catalyst (D1-Mn2Cu-FAU) prepared by the preparation method of a modified zeolite catalyst of Example 1 and Example 7 were subjected to an ozone concentration of 20 ppm, room temperature, and a flow rate of 1.0 L·min -1 Ozone conversion performance test results under conditions. Figure 4 It can be seen that the synergistic effect between multiple elements in the catalyst can improve its catalytic performance.

[0114] like Figure 5 FIG. 2 is a schematic diagram showing that the polyatomic metal clusters in the zeolite catalyst prepared by the preparation method of Example 2 are located in the zeolite framework structure. Figure 5 It can be seen that in the zeolite framework structure, [AlO2] - It can attract ion clusters composed of metal ions and oxygen atoms and become the location site of metal clusters.

[0115] refer to Figure 6 , a schematic diagram of the calculation results of reaction energy and transition state energy barrier using the CASTEP (plane wave pseudopotential method) module in Materialsstudio (material simulation calculation software) for the modified zeolite catalysts prepared in Example 1 and Example 2. Figure 6 It can be seen that in different metal ion clusters (Mn 2+ 、Mn2O 2+ 、Mn3O3 2+In the zeolite catalyst model with ) exchange, the adsorption energy of ozone molecules increases with the increase of the number of Mn atoms, and the transition state energy barrier of the rate-limiting step of the reaction decreases with the increase of the number of Mn atoms. The metal cluster model composed of three Mn atoms in the zeolite pore has higher ozone adsorption energy and lower rate-limiting step energy barrier, so it has higher catalytic activity than single-atom catalytic active sites.

[0116] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a modified zeolite catalyst for ozone purification, characterized in that: The preparation method adjusts the metal clusters in the modified zeolite framework, including mixing a metal salt solution with zeolite to form a non-Newtonian fluid mixture, drying the mixture with microwaves, and finally calcining to obtain the zeolite catalyst; The metal cluster is: Mn2O 2+ 、Mn3O3 2+ or [Mn2CuO3] 2+ .

2. The method for preparing a modified zeolite catalyst for ozone purification according to claim 1, characterized in that: The preparation method specifically comprises the following steps: The metal salt solution and the zeolite are respectively prepared in a specified ratio; Preparing a non-Newtonian fluid mixture: mixing the metal salt solution and the zeolite with stirring to obtain the non-Newtonian fluid mixture; Microwave drying the non-Newtonian fluid mixture; The non-Newtonian fluid mixture after drying is calcined to obtain the zeolite catalyst.

3. The method for preparing a modified zeolite catalyst for ozone purification according to claim 2, characterized in that: The metal salt solution is configured to specifically include: Determine the amount of metal salt: Calculate the mass of the metal salt based on the silicon-aluminum ratio and the theoretical ion exchange degree; Determine the amount of water required to prepare the metal salt solution: add deionized water dropwise to an equal amount of the zeolite, stir evenly until it becomes a non-Newtonian fluid state, and the amount of water added is the amount of water required to prepare the metal salt solution; The metal salt is mixed with the required amount of water to obtain the metal salt solution.

4. The method for preparing a modified zeolite catalyst for ozone purification according to claim 2, characterized in that: The metal salt includes nitrate and / or acetate.

5. The method for preparing a modified zeolite catalyst according to claim 2, characterized in that: Microwave drying of the non-Newtonian fluid mixture specifically comprises: The non-Newtonian fluid mixture is evenly spread into a crucible, an evaporating dish or a stainless steel beaker, and rapidly heated with a microwave reactor at a power of 100-1000 W for 30 s-30 min.

6. A modified zeolite catalyst for ozone purification, characterized in that: The zeolite catalyst is prepared by the preparation method according to any one of claims 1 to 5, and a plurality of metal clusters are evenly distributed in the pores of the zeolite powder in the zeolite catalyst; The metal clusters include metal ions and compatible oxygen atoms.

7. An ozone purification method, characterized in that: The ozone purification method uses the zeolite catalyst as claimed in claim 6 to purify ozone; The zeolite catalyst is heated at -10-300°C with a space velocity of 1×10 4 -2×10 6 h -1 The ozone is removed under the conditions of 8. The ozone purification method according to claim 7, characterized in that: The zeolite catalyst forms include but are not limited to powder catalyst, granular catalyst and monolithic catalyst.

Citation Information

Patent Citations

  • Multi-component zeolite material as well as preparation method and application thereof in ozone purification and removal

    CN111054299A

  • Metal ion modified molecular sieve, preparation method thereof and blast furnace gas desulfurization method

    CN114618426A

  • Method for modifying zeolite adsorbent

    CN114618428A

  • Ketone VOCs adsorbent as well as preparation method and application thereof

    CN115487776A

  • Adsorbent for purifying alcohol VOCs (Volatile Organic Compounds) and preparation method thereof