A processing aid containing PTFE and preparation method thereof

By using processing aids containing PTFE in engineering plastics and using low molecular weight polytetrafluoroethylene to react with functional monomers and hard monomers to form a core-shell structure, the problem of mold release expansion during the injection molding process is solved and the size of the product is increased. Stability and mechanical properties, suitable for large-scale production.

CN117003949BActive Publication Date: 2024-10-22EVERSUN POLYCARBON SCI&TECH CORP LTD
0 Cites 0 Cited by

Patent Information

Application Number
CN202311006180.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-10
Publication Date
2024-10-22
Estimated Expiration
2043-08-10

AI Technical Summary

Technical Problem

During the injection molding process, engineering plastic products are prone to mold expansion, resulting in unstable product edges, warping of film product edges, and reduced product mechanical properties.

Method used

Processing aids containing PTFE are used to form a core-shell structure through the reaction of low molecular weight polytetrafluoroethylene with functional monomers and hard monomers, which improves the melt tension and film-forming properties of the polymer, reduces the mold release expansion ratio, and improves engineering Processing properties of plastics.

Benefits of technology

It effectively reduces the mold-leaving expansion ratio of engineering plastic products, improves the dimensional stability and mechanical properties of the product, and makes the injection molded products more in line with expected requirements and suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004388380520000081
    Figure BDA0004388380520000081
  • Figure BDA0004388380520000091
    Figure BDA0004388380520000091
  • Figure BDA0004388380520000101
    Figure BDA0004388380520000101
Patent Text Reader

Abstract

The present invention relates to the technical field of modified processing aids for engineering plastics, and in particular to a processing aid containing PTFE and a preparation method thereof, the preparation method comprising the following steps: (S1), adding a low molecular weight polytetrafluoroethylene dispersion to water under stirring conditions and mixing evenly to obtain a diluted dispersion; (S2), adding functional monomers, hard monomers, emulsifiers and initiators to water for homogenization to obtain a pre-emulsion; (S3), at a certain temperature, dripping the pre-emulsion and the reducing agent-water solution into the diluted dispersion, after the dropwise addition is completed, heat preservation, and a finished emulsion is obtained; (S4), the finished emulsion is spray-dried to obtain a processing aid containing PTFE. The processing aid is used to reduce the mold expansion ratio of engineering plastic products as a whole, improve the processing performance of engineering plastics, make injection molded products more in line with expected requirements, and also ensure the mechanical properties of its products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of modified processing aids for engineering plastics, and in particular to a processing aid containing PTFE and a preparation method thereof. Background Art

[0002] Plastic products, such as polycarbonate products, usually have mold expansion during the injection molding process, poor edge stability of plastic products, and warping at the edges of film products.

[0003] When the polymer melt leaves the runner, the diameter of the melt flow is larger than the diameter of the runner outlet. This phenomenon is called die expansion. Die expansion is common, but reducing the expansion ratio is more conducive to the dimensional stability of the product. For example, during the injection molding process, when the mold size is constant, if die expansion occurs, the polymer that expands more will have less corresponding material entering than the material that does not expand. When the material cools, it is not enough to meet the expected size, reducing the dimensional stability of the product, and may introduce internal stress in the product, reducing the mechanical properties of the product. Summary of the invention

[0004] In order to overcome the shortcomings and deficiencies in the prior art, one of the objects of the present invention is to provide a method for preparing a processing aid containing PTFE, which has simple operation, convenient control, high production efficiency, low production cost, and can be used for large-scale production.

[0005] A second object of the present invention is to provide a processing aid containing PTFE.

[0006] One of the purposes of the present invention is achieved by the following technical solution: A method for preparing a processing aid containing PTFE, comprising the following steps:

[0007] (S1), adding a low molecular weight polytetrafluoroethylene dispersion into water and mixing evenly to obtain a diluted dispersion;

[0008] (S2), adding functional monomer, hard monomer, emulsifier and initiator to water and homogenizing for 20-25 minutes to obtain a pre-emulsion;

[0009] (S3), at a temperature of 40-80° C., adding the pre-emulsion to the diluted dispersion, and adding the reducing agent-water solution 8-12 minutes after the pre-emulsion is added, and after the addition is completed, keeping the temperature for 1.5-3 hours to obtain a finished emulsion;

[0010] (S4), spray drying the finished emulsion to obtain a white powder, i.e., a processing aid containing PTFE.

[0011] The preparation method of the processing aid containing PTFE comprises the following steps: a low molecular weight polytetrafluoroethylene dispersion is reacted with a pre-emulsion to form a core-shell structure, wherein the core layer is low molecular weight polytetrafluoroethylene, and the shell layer is a copolymer composed of a functional monomer and a hard monomer. The core layer component can effectively improve the melt tension, and the shell layer copolymer composed of the functional monomer and the hard monomer is better compatible with engineering plastics (for example, polycarbonate). Meanwhile, the adopted functional monomer can improve the film-forming property of the polymer after polymerization, so that the processing aid can reduce the demoulding expansion ratio of the engineering plastic product as a whole, improve the processing property of the engineering plastic, make the injection molded product more in line with the expected requirements, and also ensure the mechanical property of the product.

[0012] Preferably, the solid content of the low molecular weight polytetrafluoroethylene dispersion is 28-40 wt %; the number average molecular weight of the low molecular weight polytetrafluoroethylene is 30,000-300,000.

[0013] By adopting the above technical scheme, the main effective component, low molecular weight polytetrafluoroethylene, can increase the melt tension, so that the polymer molecules provide shrinkage force from the surface to the inside during processing, and reduce the mold expansion ratio of the engineering plastic product.

[0014] Preferably, the functional monomer is lauryl methacrylate; and the hard monomer is methyl methacrylate.

[0015] By adopting the above technical scheme, the copolymer of lauryl methacrylate and methyl methacrylate is better compatible with engineering plastics (for example, polycarbonate); at the same time, after the lauryl methacrylate is polymerized, the melt fluidity is effectively improved and the film-forming performance of the polymer is improved; after the methyl methacrylate is polymerized, it effectively provides good impact strength, and the two coat low molecular weight polytetrafluoroethylene to improve the dispersibility of PTFE in engineering plastics.

[0016] Preferably, the emulsifier is at least one of fatty alcohol polyoxyethylene ether, isomeric decanol polyoxyethylene ether, oleic acid polyoxyethylene ether, lauric acid polyoxyethylene ether, hydrogenated castor oil polyoxyethylene ether, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, alkylphenol polyoxyethylene ether and nonylphenol polyoxyethylene ether; the initiator is at least one of benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide and dicumyl peroxide.

[0017] More preferably, the emulsifier is a mixture of sodium dodecylbenzene sulfonate and isomeric decanol polyoxyethylene ether in a weight ratio of 1.2-1.5:3-4. The emulsification effect of the compounded system is better. The selected sodium dodecylbenzene sulfonate and isomeric decanol polyoxyethylene ether work together to make the emulsion more uniform and stable when the emulsion is added dropwise. If the emulsifier does not disperse the system well, the pre-emulsified system is prone to stratification, and uneven subsequent addition is likely to lead to uneven reaction.

[0018] Preferably, the mass concentration of the reducing agent-water solution is 2.5-4.0wt%; the reducing agent is sodium sulfite, sodium bisulfite or sodium formaldehyde sulfoxylate.

[0019] Preferably, in the step (S1), the volume ratio of water to the low molecular weight polytetrafluoroethylene dispersion is 2-3:1.

[0020] Preferably, in the step (S2), the weight ratio of the functional monomer, the hard monomer, the emulsifier, the initiator and the water is 15-50:30-70:4-6:1-2:200.

[0021] Preferably, in the step (S3), the volume ratio of the diluted dispersion, the pre-emulsion and the reducing agent-water solution is 300-400:250-350:150-200.

[0022] Preferably, in the step (S3), the pre-emulsion is added dropwise for 2-2.5 hours, and the reducing agent-water solution is added dropwise for 2-3 hours.

[0023] The second object of the present invention is achieved by the following technical solution: a processing aid containing PTFE is prepared by the above-mentioned preparation method of the processing aid containing PTFE.

[0024] The beneficial effects of the present invention are as follows: the preparation method of the processing aid containing PTFE of the present invention is to react a low molecular weight polytetrafluoroethylene dispersion with a pre-emulsion to form a core-shell structure, the core layer is a low molecular weight polytetrafluoroethylene, the shell layer is a copolymer composed of a functional monomer and a hard monomer, the core layer component can effectively improve the melt tension, and the shell layer is a copolymer composed of a functional monomer and a hard monomer, which is better compatible with engineering plastics (e.g., polycarbonate), and at the same time, the functional monomer used can improve the film-forming properties of the polymer after polymerization, so that the processing aid can reduce the mold expansion ratio of the engineering plastic product as a whole, improve the processing performance of the engineering plastic, make the injection molded product more in line with the expected requirements, and also ensure the mechanical properties of the product. The preparation method is simple to operate, easy to control, high in production efficiency, low in production cost, and can be used for large-scale production.

[0025] The processing aid containing PTFE of the present invention can reduce the mold release expansion ratio when the mold size is constant during injection molding, so that more materials enter than materials with a large expansion ratio. After cooling and opening the mold, the product size is closer to the expected size. DETAILED DESCRIPTION

[0026] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.

[0027] Example 1

[0028] A method for preparing a processing aid containing PTFE comprises the following steps:

[0029] (S1), adding 100 ml of low molecular weight polytetrafluoroethylene dispersion to 250 ml of water under stirring and mixing evenly to obtain a diluted dispersion;

[0030] (S2), adding 20 g of functional monomer, 50 g of hard monomer, 4.6 g of emulsifier and 2 g of initiator to 200 ml of water and homogenizing for 23 min to obtain a pre-emulsion;

[0031] (S3), at a temperature of 50° C., adding the pre-emulsified liquid of step (S2) to the diluted dispersion of step (S1), and 10 minutes after the pre-emulsified liquid was added, simultaneously adding 180 ml of a reducing agent-water solution with a mass concentration of 3.2 wt %, and after the addition was completed, keeping the temperature for 2 hours to obtain a finished emulsion;

[0032] (S4), spray drying the finished emulsion to obtain a white powder, i.e., a processing aid containing PTFE.

[0033] The solid content of the low molecular weight polytetrafluoroethylene dispersion is 30 wt %; the number average molecular weight of the low molecular weight polytetrafluoroethylene is 60,000.

[0034] The functional monomer is lauryl methacrylate; and the hard monomer is methyl methacrylate.

[0035] The emulsifier is a mixture of sodium dodecylbenzene sulfonate and isomeric decanol polyoxyethylene ether in a weight ratio of 1.3:3.5; the initiator is cumene hydroperoxide.

[0036] The reducing agent is sodium bisulfite.

[0037] In the step (S3), the pre-emulsion is added dropwise for 2.2 hours, and the reducing agent-water solution is added dropwise for 2.5 hours.

[0038] Example 2

[0039] A method for preparing a processing aid containing PTFE comprises the following steps:

[0040] (S1), adding 100 ml of low molecular weight polytetrafluoroethylene dispersion to 200 ml of water under stirring and mixing evenly to obtain a diluted dispersion;

[0041] (S2), adding 15 g of functional monomer, 30 g of hard monomer, 4 g of emulsifier and 1 g of initiator to 200 ml of water and homogenizing for 20 min to obtain a pre-emulsion;

[0042] (S3), at a temperature of 48° C., adding the pre-emulsified liquid of step (S2) to the diluted dispersion of step (S1), and 12 minutes after the pre-emulsified liquid was added, simultaneously adding 150 ml of a reducing agent-water solution with a mass concentration of 2.5 wt %, and after the addition was completed, keeping the temperature for 1.5 hours to obtain a finished emulsion;

[0043] (S4), spray drying the finished emulsion to obtain a white powder, i.e., a processing aid containing PTFE.

[0044] The solid content of the low molecular weight polytetrafluoroethylene dispersion is 28 wt %; the number average molecular weight of the low molecular weight polytetrafluoroethylene is 30,000.

[0045] The functional monomer is lauryl methacrylate; and the hard monomer is methyl methacrylate.

[0046] The emulsifier is a mixture of sodium dodecylbenzene sulfonate and isomeric decanol polyoxyethylene ether in a weight ratio of 1.2:3; the initiator is cumene hydroperoxide.

[0047] The reducing agent is sodium bisulfite.

[0048] In the step (S3), the pre-emulsion is added dropwise for 2 hours, and the reducing agent-water solution is added dropwise for 2 hours.

[0049] Example 3

[0050] A method for preparing a processing aid containing PTFE comprises the following steps:

[0051] (S1), adding 100 ml of low molecular weight polytetrafluoroethylene dispersion to 300 ml of water under stirring and mixing evenly to obtain a diluted dispersion;

[0052] (S2), adding 50 g of functional monomer, 70 g of hard monomer, 6 g of emulsifier and 2 g of initiator to 200 ml of water and homogenizing for 25 min to obtain a pre-emulsion;

[0053] (S3), at a temperature of 80° C., adding the pre-emulsified liquid of step (S2) to the diluted dispersion of step (S1), and 8 minutes after the pre-emulsified liquid was added, simultaneously adding 200 ml of a reducing agent-water solution with a mass concentration of 4.0 wt %, and after the addition was completed, keeping the temperature for 3 hours to obtain a finished emulsion;

[0054] (S4), spray drying the finished emulsion to obtain a white powder, i.e., a processing aid containing PTFE.

[0055] The solid content of the low molecular weight polytetrafluoroethylene dispersion is 40 wt %; the number average molecular weight of the low molecular weight polytetrafluoroethylene is 100,000.

[0056] The functional monomer is lauryl methacrylate; and the hard monomer is methyl methacrylate.

[0057] The emulsifier is a mixture of sodium dodecylbenzene sulfonate and isomeric decanol polyoxyethylene ether in a weight ratio of 1.5:4; the initiator is cumene hydroperoxide.

[0058] The reducing agent is sodium bisulfite.

[0059] In the step (S3), the pre-emulsion is added dropwise for 2.5 hours, and the reducing agent-water solution is added dropwise for 3 hours.

[0060] Example 4

[0061] A method for preparing a processing aid containing PTFE comprises the following steps:

[0062] (S1), adding 100 ml of low molecular weight polytetrafluoroethylene dispersion to 230 ml of water under stirring and mixing evenly to obtain a diluted dispersion;

[0063] (S2), adding 30 g of functional monomer, 60 g of hard monomer, 5 g of emulsifier and 2 g of initiator to 200 ml of water and homogenizing for 23 min to obtain a pre-emulsion;

[0064] (S3), at a temperature of 70° C., the pre-emulsified liquid of step (S2) was added dropwise to the diluted dispersion of step (S1), and 9 minutes after the pre-emulsified liquid was added dropwise, 180 ml of a reducing agent-water solution with a mass concentration of 3.5 wt % was added dropwise at the same time. After the addition was completed, the mixture was kept warm for 2.2 hours to obtain a finished emulsion;

[0065] (S4), spray drying the finished emulsion to obtain a white powder, i.e., a processing aid containing PTFE.

[0066] The solid content of the low molecular weight polytetrafluoroethylene dispersion is 35 wt %; the number average molecular weight of the low molecular weight polytetrafluoroethylene is 50,000.

[0067] The functional monomer is lauryl methacrylate; and the hard monomer is methyl methacrylate.

[0068] The emulsifier is a mixture of sodium dodecylbenzene sulfonate and isomeric decanol polyoxyethylene ether in a weight ratio of 1.3:3.6; the initiator is cumene hydroperoxide.

[0069] The reducing agent is sodium bisulfite.

[0070] In the step (S3), the pre-emulsion is added dropwise for 2.3 hours, and the reducing agent-water solution is added dropwise for 2.5 hours.

[0071] Comparative Example 1

[0072] The difference between this comparative example and Example 1 is:

[0073] The emulsifier is sodium lauryl sulfate.

[0074] Comparative Example 2

[0075] The difference between this comparative example and Example 1 is:

[0076] The hard monomer is a mixture of styrene and acrylonitrile in a weight ratio of 3:1.

[0077] Comparative Example 3

[0078] A method for preparing a processing aid containing PTFE comprises the following steps:

[0079] (S1), adding 20 g of lauryl methacrylate, 50 g of methyl methacrylate, 4.6 g of emulsifier and 2 g of cumene hydroperoxide to 200 ml of water and homogenizing for 23 min to obtain a pre-emulsion;

[0080] (S2), at a temperature of 50° C., 180 ml of a reducing agent-water solution having a mass concentration of 3.2 wt % was added dropwise to the pre-emulsified liquid for 2.5 h. After the addition was completed, the mixture was kept warm for 2 h to obtain a finished emulsion;

[0081] (S3), under stirring conditions, add 100 ml of low molecular weight polytetrafluoroethylene dispersion and the finished emulsion of step (S2) into 250 ml of water, mix them evenly, and spray dry them to obtain a processing aid.

[0082] The solid content of the low molecular weight polytetrafluoroethylene dispersion is 30 wt %; the number average molecular weight of the low molecular weight polytetrafluoroethylene is 60,000.

[0083] The emulsifier is a mixture of sodium dodecylbenzene sulfonate and isomeric decanol polyoxyethylene ether in a weight ratio of 1.3:3.5.

[0084] The reducing agent is sodium bisulfite.

[0085] Performance Testing

[0086] The processing aids of Examples 1-4 and Comparative Examples 1-3 were used in polycarbonate processing modified materials to prepare implementation samples and comparative samples. The weight amounts of each component are shown in Table 1 below:

[0087]

[0088] The preparation method comprises the following steps: mixing the raw materials of various components, adding them into a twin-screw extruder for melt extrusion, cooling and granulating to obtain a polycarbonate processing modified material; the processing temperatures of the twin-screw extruder starting from the feeding section are 230°C, 240°C, 250°C, 260°C, 260°C, 260°C, respectively, the head temperature is 250°C, and the screw speed is 360r / min.

[0089] I. Mold expansion test:

[0090] The polycarbonate processed modified material is injection molded by an injection molding machine. After cooling, a vernier caliper is used to test its length and width in mm; an electronic micrometer is used to test its thickness in mm; and its shrinkage rate is tested; wherein, the mold size is 125*15*1.6mm;

[0091] Shrinkage = (L 模 -L 样 )÷L 模 ×100%

[0092] Among them, L 模 Indicates the length, width or thickness of the mold, L 样 Indicates the length, width or thickness of the specimen.

[0093] The test results are shown in Table 2 below:

[0094]

[0095] As can be seen from Table 2 above, from the comparison of 1.6 mm thick samples, when the mold size remains unchanged, the same mold size is used for injection molding. By measuring the spline size and the mold size for comparison, we found that the size of the PC modified sample with the processing aid of the present invention is closer to the mold size, the shrinkage rate is lower than that of the control group and the blank control group, and the dimensional stability is better.

[0096] II. Mechanical properties test:

[0097] The polycarbonate processed modified materials of the experimental groups 1-4, the comparative groups 1-3 and the blank control group were tested for melt index (300°C, 1.2kg), Izod notched impact strength, tensile strength and elongation at break. The test results are shown in Table 3 below:

[0098]

[0099] It is not difficult to see from the data in Table 3 above that after adding the processing aid, the melt index of the product is increased accordingly, and the physical properties are also improved, thereby improving the corresponding processing performance of the product.

[0100] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A method for preparing a processing aid containing PTFE, characterized in that: The steps include: (S1), adding a low molecular weight polytetrafluoroethylene dispersion into water and mixing the mixture evenly to obtain a diluted dispersion; (S2), adding functional monomer, hard monomer, emulsifier and initiator into water and homogenizing for 20-25 minutes to obtain a pre-emulsion; (S3), at a temperature of 40-80°C, adding the pre-emulsified liquid to the diluted dispersion, and adding the reducing agent-water solution 8-12 minutes after the pre-emulsified liquid is added, and after the addition is completed, the temperature is kept for 1.5-3 hours to obtain a finished emulsion; (S4), spray drying the finished emulsion to obtain a white powder, i.e., a processing aid containing PTFE; The emulsifier is sodium dodecylbenzene sulfonate and isomeric decanol polyoxyethylene ether; the initiator is at least one of benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide and dicumyl peroxide; The mass concentration of the reducing agent-water solution is 2.5-4.0wt%; the reducing agent is sodium sulfite, sodium bisulfite or sodium formaldehyde sulfoxylate; In the step (S3), the pre-emulsion is added dropwise for 2-2.5 hours, and the reducing agent-water solution is added dropwise for 2-3 hours; the functional monomer is lauryl methacrylate; and the hard monomer is methyl methacrylate.

2. The method for preparing a processing aid containing PTFE according to claim 1, characterized in that: The solid content of the low molecular weight polytetrafluoroethylene dispersion is 28-40wt%; the number average molecular weight of the low molecular weight polytetrafluoroethylene is 30000-300000.

3. The method for preparing a processing aid containing PTFE according to claim 1, characterized in that: In the step (S1), the volume ratio of water to the low molecular weight polytetrafluoroethylene dispersion is 2-3:

1.

4. The method for preparing a processing aid containing PTFE according to claim 1, characterized in that: In the step (S2), the weight ratio of the functional monomer, the hard monomer, the emulsifier, the initiator and the water is 15-50:30-70:4-6:1-2:

200.

5. The method for preparing a processing aid containing PTFE according to claim 1, characterized in that: In the step (S3), the volume ratio of the diluted dispersion, the pre-emulsion and the reducing agent-water solution is 300-400:250-350:150-200.

6. A processing aid containing PTFE, characterized in that: The invention is prepared by the preparation method of the processing aid containing PTFE as claimed in any one of claims 1 to 5.