Preparation process of composite leather adhesive
By combining modified tannin extract with leather collagen fibers and gelatin molecules, combined with end epoxy modified tannin acid and plant fibers, the problem of poor performance of existing leather adhesives is solved and higher adhesive strength is achieved , water resistance and antibacterial and UV resistance.
Patent Information
- Application Number
- CN202310874499.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-17
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-07-17
AI Technical Summary
Existing leather adhesives often contain benzene and aldehyde substances, which will release formaldehyde and harm human health. In addition, gelatin adhesives have poor water resistance and mechanical properties during use, which limits their application.
By extracting tannins from masan peel and modifying them, they carry aldehyde groups to form hydrogen bonds and chemical bonds with leather collagen fibers, combining gelatin molecules to form a stable Schiff base structure, increasing the degree of cross-linking and bonding properties, and Use end epoxy modified tannin and plant fiber to enhance peel strength and water resistance.
It improves the bonding strength and water resistance of the adhesive with leather, enhances antibacterial and UV resistance, extends service life, and improves peel strength and hydrophobic properties.
Smart Images

Figure BDA0004342384380000061 
Figure BDA0004342384380000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, in particular to a preparation process of a composite adhesive for leather. Background Art
[0002] At present, most of the adhesives used in leather products on the market contain substances such as benzene and aldehydes, which will release formaldehyde during use and endanger human health. Gelatin, as a natural waste-recyclable biomass material, has no triple helix structure and is easy to modify its properties to have better performance. The main reason for its limitation in practicality is that there are still a large number of hydrophilic groups in its structural chain segments, which leads to poor water resistance and mechanical properties of gelatin adhesives during use.
[0003] Therefore, it is of great significance to invent a composite leather adhesive. Summary of the invention
[0004] The object of the present invention is to provide a preparation process of a composite leather adhesive to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A preparation process of a composite leather adhesive comprises the following steps:
[0007] S1: adding Coriolus morsultanus bark powder to sodium hydroxide solution, heating to 60-80°C for reaction for 60-80 minutes, filtering, neutralizing, and drying to obtain a tannin extract; adding the tannin extract to trifluoroacetic acid, adding urotropine, heating to 95-105°C for reaction for 1.5-2.0 hours, purifying, and drying to obtain a modified tannin extract;
[0008] S2: Add the modified tannin extract to a mixed solvent of N,N-dimethylformamide and ethyl acetate, add triethylamine and 4-diaminopyridine and stir evenly, add 10-undecenoyl chloride, react at a constant temperature of 30-40°C under a nitrogen atmosphere for 28-36 hours, purify, and dry to obtain terminal olefin-modified tannic acid; add the terminal olefin-modified tannic acid to dichloromethane, add meta-chloroperbenzoic acid and 4,4'-thiobis(6-tert-butyl-meta-cresol), react at 40-45°C for 36-48 hours, purify, and dry to obtain terminal epoxy-modified tannic acid;
[0009] S3: Add the epoxy-terminated tannic acid, sodium chloride, and Tris buffer solution to distilled water, adjust the pH to 8-8.5, add the plant fiber, perform ultrasonic vibration at 20-25°C for 38-46 hours, purify, dry, add to anhydrous ethanol, add N-tert-butyl-2-benzothiazole sulfonamide and KH560, reflux and stir at 90-95°C under nitrogen atmosphere for 6-12 hours, purify, and dry to obtain modified plant fiber;
[0010] S4: Adjust the pH of gelatin solution to 8-10, add sodium dodecyl sulfate, modified tannin extract and terminal epoxy modified tannic acid in sequence, stir and react at 45-60°C for 2-4h, adjust the pH to 7, add modified plant fiber and stir evenly to obtain composite leather adhesive.
[0011] Furthermore, in the tannin extract, the concentration of the sodium hydroxide solution is 0.2-0.3 wt %, and the solid-liquid ratio of the Cortex Morindae powder to the sodium hydroxide solution is 15-25 mL / g.
[0012] Furthermore, in the modified tannin extract, the mass ratio of tannin extract: trifluoroacetic acid: hexamethylenetetramine is 1:(6-8):(1.5-3).
[0013] Furthermore, in the terminal olefin-modified tannic acid, the mass ratio of N,N-dimethylformamide:ethyl acetate is 1:(1-2); the mass ratio of modified tannin extract:10-undecenoyl chloride:triethylamine:4-diaminopyridine is 1:(4.5-5.5):(2.5-3):(0.1-0.12).
[0014] Furthermore, in the terminal epoxy-modified tannic acid, the mass ratio of terminal olefin-modified tannic acid: meta-chloroperbenzoic acid: 4,4'-thiobis(6-tert-butyl-meta-cresol) is (3-4):(15-20):(0.1-0.15).
[0015] Furthermore, the mass ratio of the plant fiber: epoxy-terminated tannic acid: sodium chloride: Tris buffer solution: N-tert-butyl-2-benzothiazole sulfonamide: KH560 is (8-10):(0.6-0.8):2.5:0.4:(0.25-0.3):(0.2-0.25).
[0016] Furthermore, in the composite leather adhesive, the proportions of the components, by mass, are 80-100 parts of gelatin solution, 1-2 parts of sodium dodecyl sulfate, 0.12-0.24 parts of modified tannin extract, 3.6-6.4 parts of terminal epoxy modified tannic acid and 1-2 parts of modified plant fiber.
[0017] Furthermore, the plant fiber is 3-4 mm in length and is kenaf fiber.
[0018] Furthermore, the solvent in the gelatin solution is deionized water, the solute is gelatin, and the mass fraction is 15-20%; the amount of modified tannin extract added is 1-1.2% of the gelatin mass, and the amount of terminal epoxy modified tannic acid added is 30-32% of the gelatin mass.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] The present invention extracts natural tannin from Coriolus mulberry bark, and modifies it so that each benzene ring in the structure carries an aldehyde group on one side. Leather contains a large amount of collagen fibers, and the collagen fibers are rich in a large amount of amino acid active substances and contain a large amount of functional groups. The modified natural tannin extract can not only hydrogen bond with the leather collagen fibers, but the aldehyde groups carried in the structure can also form chemical bonds with the amino groups in the collagen fiber structure, so that the adhesive and the leather are tightly combined, greatly improving the peeling strength. At the same time, the phenolic hydroxyl group and the aldehyde group in the modified tannin extract can hydrogen bond and react with the amino groups in the adhesive matrix gelatin molecules to form a stable Schiff base structure, further enhancing the crosslinking degree and bonding performance of the adhesive, making the structure more compact, and the tannin structure and aromatic ring group of the modified tannin extract itself can improve the antibacterial and anti-ultraviolet properties of the adhesive, reduce the erosion of bacteria and the aging effect of ultraviolet rays during use, and improve the service life.
[0021] The present invention further modifies the modified tannin extract, and grafts a long aliphatic carbon chain and an epoxy group into the tannin structure. The long aliphatic carbon chain can reduce steric hindrance and increase the grafting degree during the grafting process, and on the other hand, it has the function of a flexible hydrophobic segment in the adhesive structure, greatly improving the hydrophobic property and toughness of the adhesive. The active site in the molecular structure of the terminal epoxy-modified tannic acid can react with the amino group in the matrix gelatin to form a CN covalent bond, thereby improving the intermolecular cohesion and further enhancing the peel strength and water resistance of the adhesive.
[0022] The present invention uses terminal epoxy modified tannic acid to modify plant fiber and grafts the terminal epoxy modified tannic acid on the fiber surface, and at the same time anchors N-tert-butyl-2-benzothiazole sulfenamide and KH560 on the fiber surface. On the one hand, the amino group in the structure of N-tert-butyl-2-benzothiazole sulfenamide can react with the epoxy in the terminal epoxy modified tannic acid and KH560 to stabilize the combination, and on the other hand, the -SC=N structure in its structure can accelerate the cross-linking reaction between polymers, shorten the chemical cross-linking reaction time, and improve the bonding performance of the adhesive. The addition of KH560 and terminal epoxy modified tannic acid in the modified plant fiber synergistically improves the interface bonding strength between the fiber and the matrix gelatin, can be evenly dispersed in the adhesive to avoid the occurrence of agglomeration, thereby further enhancing the peel strength and water resistance of the adhesive. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] It should be noted that the purchase manufacturers of all raw materials involved in the present invention are not subject to any special restrictions, and exemplary examples include: trifluoroacetic acid, meta-chloroperbenzoic acid, 4,4'-thiobis(6-tert-butyl-meta-cresol) were purchased from Shanghai McLean Biochemical Technology Co., Ltd., urotropine was purchased from Chengdu Cologne Chemical Co., Ltd., ethyl acetate was purchased from Beijing Chemical Plant, N,N-dimethylformamide, triethylamine, and 4-diaminopyridine were purchased from Aladdin Reagent Company, kenaf fiber specifications were 3mm, and N-tert-butyl-2-benzothiazolesulfonamide was purchased from Shanghai Dingfen Chemical Technology Co., Ltd.
[0025] Example 1: A process for preparing a composite adhesive for leather: S1: Add 10 g of Coriolus mulberry bark powder to 250 mL of a 0.2 wt% sodium hydroxide solution, heat to 60° C. for 80 min, filter, neutralize, and dry to obtain a tannin extract; add 1 g of the tannin extract to 6 g of trifluoroacetic acid, add 1.5 g of urotropine, heat to 95° C. for 2.0 h, purify, and dry to obtain a modified tannin extract;
[0026] S2: Add 1 g of modified tannin extract to a mixed solvent of 10 g of N,N-dimethylformamide and 20 g of ethyl acetate, add 2.5 g of triethylamine and 0.1 g of 4-diaminopyridine, stir evenly, add 4.5 g of 10-undecenoyl chloride, react at 30°C for 36 h under a nitrogen atmosphere, purify, and dry to obtain terminal olefin-modified tannic acid; add 3 g of terminal olefin-modified tannic acid to 50 mL of dichloromethane, add 15 g of meta-chloroperbenzoic acid and 0.1 g of 4,4'-thiobis(6-tert-butyl-meta-cresol), react at 40°C for 48 h, purify, and dry to obtain terminal epoxy-modified tannic acid;
[0027] S3: 0.6 g of epoxy-terminated tannic acid, 2.5 g of sodium chloride, and 0.4 g of Tris buffer solution were added to distilled water, the pH was adjusted to 8, 8 g of plant fiber was added, ultrasonically shaken at 25 ° C for 46 h, purified, dried, added to anhydrous ethanol, 0.25 g of N-tert-butyl-2-benzothiazole sulfonamide and 0.2 g of KH560 were added, refluxed at 95 ° C for 12 h under a nitrogen atmosphere, purified, and dried to obtain modified plant fiber;
[0028] S4: Adjust the pH value of 100g 15wt% gelatin solution to 8.5, add 1g sodium dodecyl sulfate, 0.15g modified tannin extract and 4.5g terminal epoxy modified tannic acid in sequence, stir and react at 45°C for 4h, adjust the pH value to 7, add 1g modified plant fiber and stir evenly to obtain a composite leather adhesive.
[0029] Example 2: A process for preparing a composite adhesive for leather: S1: Add 10 g of Coriolus morsulcata powder to 200 mL of 0.2 wt% sodium hydroxide solution, heat to 60° C. for 80 min, filter, neutralize, and dry to obtain a tannin extract; add 1 g of the tannin extract to 7 g of trifluoroacetic acid, add 2 g of urotropine, heat to 95° C. for 2.0 h, purify, and dry to obtain a modified tannin extract;
[0030] S2: Add 1 g of modified tannin extract to a mixed solvent of 10 g of N,N-dimethylformamide and 20 g of ethyl acetate, add 3 g of triethylamine and 0.11 g of 4-diaminopyridine, stir evenly, add 5 g of 10-undecenoyl chloride, react at 30°C for 36 h under a nitrogen atmosphere, purify, and dry to obtain terminal olefin-modified tannic acid; add 3 g of terminal olefin-modified tannic acid to 50 mL of dichloromethane, add 20 g of meta-chloroperbenzoic acid and 0.15 g of 4,4'-thiobis(6-tert-butyl-m-cresol), react at 40°C for 48 h, purify, and dry to obtain terminal epoxy-modified tannic acid;
[0031] S3: 0.7 g of epoxy-terminated tannic acid, 2.5 g of sodium chloride, and 0.4 g of Tris buffer solution were added to distilled water, the pH was adjusted to 8, 9 g of plant fiber was added, ultrasonically shaken at 25 ° C for 46 h, purified, dried, added to anhydrous ethanol, 0.3 g of N-tert-butyl-2-benzothiazole sulfonamide and 0.25 g of KH560 were added, refluxed at 95 ° C for 12 h under a nitrogen atmosphere, purified, and dried to obtain modified plant fiber;
[0032] S4: Adjust the pH value of 100g 20wt% gelatin solution to 8.5, add 1.5g sodium dodecyl sulfate, 0.2g modified tannin extract and 6g terminal epoxy modified tannic acid in sequence, stir and react at 45°C for 4h, adjust the pH value to 7, add 1.5g modified plant fiber and stir evenly to obtain a composite leather adhesive.
[0033] Example 3: A process for preparing a composite adhesive for leather: S1: Add 10 g of Coriolus mulberry bark powder to 150 mL of a 0.2 wt% sodium hydroxide solution, heat to 60° C. for 80 min, filter, neutralize, and dry to obtain a tannin extract; add 1 g of the tannin extract to 8 g of trifluoroacetic acid, add 3 g of urotropine, heat to 95° C. for 2.0 h, purify, and dry to obtain a modified tannin extract;
[0034] S2: Add 1 g of modified tannin extract to a mixed solvent of 10 g of N,N-dimethylformamide and 20 g of ethyl acetate, add 3 g of triethylamine and 0.12 g of 4-diaminopyridine, stir evenly, add 5.5 g of 10-undecenoyl chloride, react at 30°C for 36 h under a nitrogen atmosphere, purify, and dry to obtain terminal olefin-modified tannic acid; add 4 g of terminal olefin-modified tannic acid to 50 mL of dichloromethane, add 20 g of meta-chloroperbenzoic acid and 0.15 g of 4,4'-thiobis(6-tert-butyl-meta-cresol), react at 40°C for 48 h, purify, and dry to obtain terminal epoxy-modified tannic acid;
[0035] S3: 0.8 g of epoxy-terminated tannic acid, 2.5 g of sodium chloride, and 0.4 g of Tris buffer solution were added to distilled water, the pH was adjusted to 8, 10 g of plant fiber was added, ultrasonically shaken at 25 ° C for 46 h, purified, dried, added to anhydrous ethanol, 0.3 g of N-tert-butyl-2-benzothiazole sulfonamide and 0.25 g of KH560 were added, refluxed at 95 ° C for 12 h under a nitrogen atmosphere, purified, and dried to obtain modified plant fiber;
[0036] S4: Adjust the pH value of 100g 20wt% gelatin solution to 8.5, add 2g sodium dodecyl sulfate, 0.24g modified tannin extract and 6.4g terminal epoxy modified tannic acid in sequence, stir and react at 45°C for 4h, adjust the pH value to 7, add 2g modified plant fiber and stir evenly to obtain a composite leather adhesive.
[0037] Comparative Example 1: Preparation process of a composite adhesive for leather: S1: Add 10g of Coriolus mulberry bark powder to 250mL of 0.2wt% sodium hydroxide solution, heat to 60°C for reaction for 80min, filter, neutralize, and dry to obtain a tannin extract; add 1g of tannin extract to 3g of trifluoroacetic acid, add 1.5g of urotropine, heat to 95°C for reaction for 2.0h, purify, and dry to obtain a modified tannin extract;
[0038] The remaining steps are the same as in Example 1.
[0039] Comparative Example 2: A process for preparing a composite adhesive for leather: S1: Add 10 g of Coriolus mulberry bark powder to 250 mL of a 0.2 wt% sodium hydroxide solution, heat to 60° C. and react for 80 min, filter, neutralize, and dry to obtain a tannin extract; add 1 g of the tannin extract to 6 g of trifluoroacetic acid, add 0.5 g of urotropine, heat to 95° C. and react for 2.0 h, purify, and dry to obtain a modified tannin extract;
[0040] The remaining steps are the same as in Example 1.
[0041] Comparative Example 3: A process for preparing a composite leather adhesive: S4: Adjust the pH of 100g 15wt% gelatin solution to 8.5, add 1g sodium dodecyl sulfate, 0.15g modified tannin extract and 8g terminal epoxy modified tannic acid in sequence, stir and react at 45°C for 4h, adjust the pH to 7, add 4g modified plant fiber and stir evenly to obtain a composite leather adhesive;
[0042] The remaining steps are the same as in Example 1.
[0043] Comparative Example 4: A process for preparing a composite leather adhesive: S4: Adjust the pH of 100g 15wt% gelatin solution to 8.5, add 1g sodium dodecyl sulfate, 0.15g modified tannin extract and 2g terminal epoxy modified tannic acid in sequence, stir and react at 45°C for 4h, adjust the pH to 7, add 0.5g modified plant fiber and stir evenly to obtain a composite leather adhesive;
[0044] The remaining steps are the same as in Example 1.
[0045] Comparative Example 5: Preparation process of a composite leather adhesive:
[0046] The remaining steps are the same as in Example 1.
[0047] Test: Peel strength test: According to GB / T 532-2008, the adhesive prepared in each embodiment and comparative example is evenly coated on the polished cow leather surface, placed at 80°C for activation for 5 minutes and then bonded. The sample size is 100mm×25mm. After pressurization for 15s, the test is performed on a universal testing machine. The peeling angle is 180° and the tensile rate is 50mm / min.
[0048] Wet peel strength test: The test is carried out in accordance with EN15062:2005. The sample in the peel strength test is immersed in water for 4 hours and then subjected to a peel strength test. The sampling specification is 100mm×25mm.
[0049]
[0050]
[0051] Conclusion: The adhesives prepared in Examples 1-3 have excellent bonding properties and water resistance.
[0052] In Comparative Example 1, the amount of trifluoroacetic acid added during the modification of the tannin extract was too low, resulting in a decrease in the modified grafting rate, resulting in a decrease in the peel strength and the wet peel strength.
[0053] In Comparative Example 2, the amount of hexamethylenetetramine added during the modification of the tannin extract was too low, resulting in a decrease in the modified grafting rate, and a decrease in the peel strength and the wet peel strength.
[0054] In Comparative Example 3, excessive amounts of terminal epoxy-modified tannic acid and modified plant fiber were added during the preparation of the adhesive, resulting in an excessive degree of crosslinking between the epoxy groups and gelatin, causing the material to become brittle, resulting in decreased peel strength and wet peel strength.
[0055] In Comparative Example 4, too little epoxy-modified tannic acid and modified plant fiber were added during the preparation of the adhesive, resulting in a reduced degree of crosslinking, a loose crosslinked network structure, and reduced cohesion, leading to decreased peel strength and wet peel strength.
[0056] In Comparative Example 5, 10-undecenoyl chloride was replaced by propylene bromide during the preparation of the epoxy-terminated tannic acid, which lacked a long aliphatic carbon chain, resulting in reduced water resistance and toughness, and reduced peel strength and wet peel strength.
[0057] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for preparing a composite leather adhesive, characterized in that: The following steps are involved: S1: Add the modified tannin extract to a mixed solvent of N,N-dimethylformamide and ethyl acetate, add triethylamine and 4-diaminopyridine and stir evenly, add 10-undecenoyl chloride, react at a constant temperature of 30-40°C under a nitrogen atmosphere for 28-36 hours, purify, and dry to obtain terminal olefin-modified tannic acid; add the terminal olefin-modified tannic acid to dichloromethane, add meta-chloroperbenzoic acid and 4,4'-thiobis(6-tert-butyl-m-cresol), react at 40-45°C for 36-48 hours, purify, and dry to obtain terminal epoxy-modified tannic acid; S2: adjusting the pH of the gelatin solution to 8-10, adding sodium dodecyl sulfonate, modified tannin extract and terminal epoxy modified tannic acid in sequence, stirring and reacting at 45-60° C. for 2-4 hours, adjusting the pH to 7, adding modified plant fiber and stirring evenly to obtain a composite leather adhesive; The modified tannin extract is prepared as follows: adding Cortex Morindae Powder to a sodium hydroxide solution, heating for reaction, filtering, neutralizing, and drying to obtain a tannin extract; adding the tannin extract to trifluoroacetic acid, adding methenamine, heating for reaction, purifying, and drying to obtain a modified tannin extract; In the modified tannin extract, the heating reaction temperature is 95-105° C., and the time is 1.5-2.0 h; the mass ratio of tannin extract: trifluoroacetic acid: hexamethylenetetramine is 1:(6-8):(1.5-3); The modified plant fiber is prepared as follows: add terminal epoxy-modified tannic acid, sodium chloride, and Tris buffer solution to distilled water, adjust the pH to 8-8.5, add plant fiber, ultrasonically shake at 20-25° C. for 38-46 hours, purify, dry, add to anhydrous ethanol, add N-tert-butyl-2-benzothiazole sulfonamide and KH560, reflux and stir at 90-95° C. for 6-12 hours under a nitrogen atmosphere, purify, and dry to obtain the modified plant fiber; The mass ratio of the plant fiber: epoxy-terminated tannic acid: sodium chloride: Tris buffer solution: N-tert-butyl-2-benzothiazole sulfonamide: KH560 is (8-10):(0.6-0.8):2.5:0.4:(0.25-0.3):(0.2-0.25).
2. The process for preparing a composite leather adhesive according to claim 1, characterized in that: In the tannin extract, the heating reaction temperature is 60-80° C., the time is 60-80 min; the concentration of the sodium hydroxide solution is 0.2-0.3 wt %, and the material-liquid ratio of the Cortex Morindae powder to the sodium hydroxide solution is 15-25 mL / g.
3. The process for preparing a composite leather adhesive according to claim 1, characterized in that: In the terminal olefin-modified tannic acid, the mass ratio of N,N-dimethylformamide:ethyl acetate is 1:(1-2); the mass ratio of modified tannin extract:10-undecenoyl chloride:triethylamine:4-diaminopyridine is 1:(4.5-5.5):(2.5-3):(0.1-0.12).
4. The process for preparing a composite leather adhesive according to claim 1, characterized in that: In the terminal epoxy-modified tannic acid, the mass ratio of terminal olefin-modified tannic acid: meta-chloroperbenzoic acid: 4,4'-thiobis(6-tert-butyl-meta-cresol) is (3-4):(15-20):(0.1-0.15).
5. The process for preparing a composite leather adhesive according to claim 1, characterized in that: In the composite leather adhesive, the proportions of various components, by mass, are 80-100 parts of gelatin solution, 1-2 parts of sodium dodecyl sulfonate, 0.12-0.24 parts of modified tannin extract, 3.6-6.4 parts of terminal epoxy modified tannic acid and 1-2 parts of modified plant fiber.
6. The process for preparing a composite adhesive for leather according to claim 5, characterized in that: The solvent in the gelatin solution is deionized water, and the solute is gelatin with a mass fraction of 15-20%; the added amount of the modified tannin extract is 1-1.2% of the mass of the gelatin, and the added amount of the terminal epoxy modified tannic acid is 30-32% of the mass of the gelatin.
Citation Information
Patent Citations
Method for preparing bio-based flame-retardant epoxy resin and prepared bio-based flame-retardant epoxy resin
CN108192078A
Extraction method of Chinese coriaria bark tannin and extract of Chinese coriaria bark tannin
CN109867703A
Tannic acid curing agent as well as preparation method and application thereof
CN110790902A
Environmentally-friendly rubber accelerator modified filling material,, and preparation method and application thereof
CN111303489A
Curable adhesive for bookbinding and method of bookbinding
JP1991239781A