A high-stability phosphate blue phosphor and preparation method thereof

By introducing trace amounts of alkali metals and Ge ions into the blue LED chip to replace Sr and P elements, the stability of the phosphate blue phosphor is improved, the problem of the lack of blue-violet light band and thermal quenching of the traditional blue LED chip is solved, and high-performance Improved stability and light decay performance over long periods of use.

CN117004390BActive Publication Date: 2024-10-29JIANGSU BREE OPTRONICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310793859.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-30
Publication Date
2024-10-29
Estimated Expiration
2043-06-30

AI Technical Summary

Technical Problem

Traditional high-color white LEDs based on blue LED chips lack the blue-violet light band of 380-450nm, resulting in the inability to achieve effective full-spectrum emission, and the thermal quenching of Sr5(PO4)3Cl:Eu blue phosphor and long-term use of light The decline is more serious, which limits its application fields.

Method used

By combining trace amounts of alkali metals and Ge ions to replace Sr and P elements in the halophosphate blue powder matrix, the stability of the phosphor crystal is improved, and the crystal field binding force around the activator ions is enhanced to prepare a highly stable phosphate blue. Phosphor powder Sr5-aMaP3-bGebO12Cl:xEu2+, the luminescence stability of this powder is significantly enhanced at high temperatures, and the light attenuation performance is greatly improved.

Benefits of technology

It improves the thermal quenching performance of blue phosphor, improves the brightness maintenance rate after 1000 hours of high temperature and high humidity aging, and significantly extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117004390B_ABST
    Figure CN117004390B_ABST
Patent Text Reader

Abstract

The present invention provides a high-stability phosphate blue phosphor and a preparation method thereof. The high-stability phosphate blue phosphor has a structural formula of Sr 5‑a M a P 3‑b Ge b O 12 Cl:xEu 2+ , wherein M is one or two of Li and Na, 0.0001≤a≤0.02, 0.0001≤b≤0.02, 0.001≤x≤0.5. The high-stability phosphate blue phosphor improves the thermal quenching and long-term light decay problems of the phosphate blue phosphor by combining element substitution. The high-stability phosphate blue phosphor improves the thermal quenching of the blue phosphor by more than 5%, and the 1000-hour high-temperature and high-humidity aging is improved by 15%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of optoelectronic materials, and in particular relates to a high-stability phosphate blue phosphor. Background Art

[0002] General lighting is the main application area of ​​white light LED technology. In the field of general lighting, white light LED is moving from the original medium color rendering index (CRI: 70~80) to high color rendering index (CRI: above 90) and even full spectrum. LED lighting is developing towards healthy, green and high color quality lighting devices. In full spectrum white light LED, the spectrum structure of LED will be closer to the spectrum structure of sunlight, which is beneficial to human visual health.

[0003] In order to improve the light source quality of white light LEDs, the spectrum of white light LEDs needs to cover the entire visible band as effectively as possible, but traditional high-color white light LEDs based on blue light LED chips lack the blue-violet light band of 380-450nm, and thus cannot achieve effective full-spectrum emission. In full-spectrum white light LEDs excited by purple light chips, blue phosphors play an extremely important role. On the one hand, blue phosphors are needed to provide the blue band spectral component in white light LEDs, and on the other hand, the blue light emitted by blue phosphors is also needed to excite green, yellow and red phosphors.

[0004] Sr5(PO4)3Cl:Eu blue phosphor has an emission peak at 450nm. It is a highly efficient blue light emitting material and has been used in the full spectrum of purple LED chips. However, the thermal quenching and long-term light decay of this phosphor are relatively serious, which restricts the application areas of this phosphor. Summary of the invention

[0005] The present invention aims to solve the deficiencies of the prior art and provides a high-stability phosphate blue phosphor. The high-stability phosphate blue phosphor improves the thermal quenching and long-term light decay problems of the phosphate blue phosphor by combining element substitution.

[0006] The high stability phosphate blue phosphor has a structural formula of Sr 5-a M a P 3-b Ge b O 12 Cl:xEu 2+ ,

[0007] Wherein M is one or both of Li and Na, 0.0001≤a≤0.02, 0.0001≤b≤0.02, 0.001≤x≤0.5.

[0008] The high-stability phosphate blue phosphor uses a trace amount of alkali metal and Ge ion combination to replace the Sr and P elements in the halophosphate blue powder matrix in trace amounts, thereby improving the stability of the phosphor crystal, making the crystal field around the activator ions have a stronger binding force on the activator ions, and significantly enhancing the luminous stability of the phosphor at high temperatures. The light decay performance is also greatly improved after long-term use. The introduction of alkali metals replaces the Sr element, and an equal amount of Ge elements are used to replace the P element. The two work together to achieve charge balance after combined substitution.

[0009] The high-stability phosphate blue phosphor is excited by ultraviolet light and blue-violet light in the wavelength range of 350-430 nm, and emits blue light with a wavelength of 450 nm.

[0010] Furthermore, the molar ratio of the alkali metal to Ge in the phosphate is in the range of 0.005-0.02; and the molar ratio of the alkali metal to Ge is alkali metal:Ge=(1±0.15):1.

[0011] The method for preparing the high-stability phosphate blue phosphor is to use SrCO3, SrCl2, M2CO3, NH4H2PO4, GeO2 and Eu2O3 as raw materials, sinter them at 1000-1200° C. in a reducing atmosphere, and then crush and sieve them to obtain the phosphor.

[0012] The preparation method of the high-stability phosphate blue phosphor comprises the following specific steps:

[0013] Step 1: Weigh SrCO3, SrCl2, M2CO3, NH4H2PO4, GeO2, Eu2O according to the stoichiometric ratio. 3;

[0014] Step 2: Mix the above raw materials evenly, put them into a corundum crucible, and cover it;

[0015] Step 3: Place the crucible in a box furnace and heat at 1000-1200°C in a reducing atmosphere for 2-20 hours;

[0016] Step 4: crush the powder obtained in step 3 and pass it through a 200-300 mesh sieve, ball mill, filter, dry and sieve to obtain the target phosphor.

[0017] The high-stability phosphate blue phosphor of the present invention improves the thermal quenching of the blue phosphor by more than 5%, and improves the 1000-hour high-temperature and high-humidity aging by 15%. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Example 1 Emission spectrum of blue phosphor.

[0019] Figure 2 SEM morphology photograph of the blue phosphor of Example 2. DETAILED DESCRIPTION

[0020] Example 1: Step 1, weigh SrCO3 61.99 g, SrCl2 9.51 g, Li2CO3 0.037 g, NH4H2PO4 34.39 g, GeO2 0.10 g, Eu2O3 3.34 g;

[0021] Step 2: Mix the above raw materials evenly and put them into a corundum crucible with an inner diameter of 50 mm and a height of 60 mm, and cover it;

[0022] Step 3: Place the crucible in a box furnace and heat it at 1100°C in an ammonia decomposition atmosphere for 4 hours;

[0023] Step 4: crush the obtained powder block and pass it through a 200-mesh sieve, ball-mill, filter, dry and sieve to obtain the target phosphor;

[0024] The obtained phosphor has the molecular formula Sr 4.8 Li 0.01 P 2.99 Ge 0.01 O 12 Cl: 0.19 Eu 2+ , emission peak wavelength is 450nm.

[0025] Embodiment 2:

[0026] Step 1: Weigh 61.03 g SrCO3, 9.51 g SrCl2, 0.08 g Na2CO3, 34.33 g NH4H2PO4, 0.16 g GeO2, and 4.4 g Eu2O3;

[0027] Step 2: Mix the above raw materials evenly and put them into a corundum crucible with an inner diameter of 50 mm and a height of 60 mm, and cover it;

[0028] Step 3: Place the crucible in a box furnace and heat it at 1150°C in an ammonia decomposition atmosphere for 3 hours;

[0029] Step 4: crush the obtained powder block and pass it through a 300-mesh sieve, ball-mill, filter, dry and sieve to obtain the target phosphor;

[0030] The obtained phosphor has the molecular formula Sr 4.735 Na 0.015 P 2.985 Ge 0.015 O 12 Cl: 0.25 Eu 2+ , emission peak wavelength is 450nm.

[0031] Example 3, Combination of two alkali metal elements

[0032] Step 1: Weigh 61.99 g SrCO3, 9.51 g SrCl2, 0.04 g Na2CO3, 0.009 g Li2CO3, 34.39 g NH4H2PO4, 0.10 g GeO2, and 3.34 g Eu2O3;

[0033] Step 2: Mix the above raw materials evenly and put them into a corundum crucible with an inner diameter of 50 mm and a height of 60 mm, and cover it;

[0034] Step 3: Place the crucible in a box furnace and heat it at 1090°C in an ammonia decomposition atmosphere for 5 hours;

[0035] Step 4: crush the obtained powder block and pass it through a 200-mesh sieve, ball-mill, filter, dry and sieve to obtain the target phosphor;

[0036] The obtained phosphor has the molecular formula Sr 4.8 Li 0.0025 Na 0.0075 P 2.99 Ge 0.01 O 12 Cl: 0.19 Eu 2+ , emission peak wavelength is 450nm.

[0037] Comparative Example 1

[0038] Weigh 62.13 g of SrCO3, 9.51 g of SrCl2, 34.5 g of NH4H2PO4, and 3.34 g of Eu2O3;

[0039] Mix the above raw materials evenly and put them into a corundum crucible with an inner diameter of 50mm and a height of 60mm, and cover it. Put the crucible into a box furnace and keep it at 1100℃ in an atmosphere of ammonia decomposition for 4 hours. Crush the obtained powder block and pass it through a 200-mesh sieve, ball mill, filter, dry and sieve to obtain the target phosphor. The phosphor molecular formula is Sr4.81P3O12Cl:0.19Eu2+, and the emission peak wavelength is 450nm.

[0040] Application test example

[0041] The spectrum and brightness were measured using the Yuanfang HASS-2000 spectrometer, the thermal quenching test was measured using the Yuanfang EX-1000 thermal quenching analyzer, and the aging test was performed using the Dongguan Weihuang Experimental Equipment WHTH-800 LED aging analyzer.

[0042] Emission peak wavelength nm Relative brightness% 150℃ brightness maintenance rate% Brightness maintenance rate after 1000h aging (current 60mA, temperature 85℃, humidity 85%) Example 1 450 100 85.2 97.3 Example 2 450 100.4 84.9 97.7 Example 3 450 99.8 85 97.5 Comparative Example 1 450 99.5 80.2 82.2

[0043] Note: Thermal quenching test: Heat the phosphor sample to the target temperature and test the brightness comparison of the phosphor sample at high temperature and room temperature.

[0044] Aging test: The phosphor and purple LED chips (Sanan Optoelectronics) (peak wavelength 400nm) were packaged into LED devices, which were then lit for 1000 hours in a high temperature and high humidity environment. The brightness and initial brightness after 1000 hours were tested.

Claims

1. A high stability phosphate blue phosphor, It is characterized in that Its structural formula is Sr 5-a-x M a P 3-b Ge b O 12 Cl:xEu 2+ , Wherein M is one or both of Li and Na, 0.0001≤a≤0.02, 0.0001≤b≤0.02, 0.001≤x≤0.

5.

2. The high-stability phosphate blue phosphor according to claim 1, It is characterized in that The high-stability phosphate blue phosphor is excited by ultraviolet light and blue-violet light in the wavelength range of 350-430 nm, and emits blue light with a wavelength of 450 nm.

3. The high-stability phosphate blue phosphor according to claim 1, It is characterized in that The molar ratio of M to Ge in phosphate is in the range of 0.005-0.02; and the molar ratio of M to Ge is M:Ge=(1±0.15):

1.

4. The method for preparing the high-stability phosphate blue phosphor according to claim 1, It is characterized in that SrCO 3 , SrCl 2 , M 2 CO 3 , NH 4 H 2 PO 4 ,GeO 2 ,Eu 2 O 3 The raw material is sintered at 1000-1200℃ in a reducing atmosphere, then crushed and sieved to obtain it.

5. The method according to claim 4, It is characterized in that The preparation method of the high-stability phosphate blue phosphor comprises the following specific steps: Step 1: Weigh SrCO according to the stoichiometric ratio 3 , SrCl 2 , M 2 CO 3 , NH 4 H 2 PO 4 ,GeO 2 ,Eu 2 O 3 ; Step 2: Mix the above raw materials evenly, put them into a corundum crucible, and cover it; Step 3: Place the crucible in a box furnace and heat at 1000-1200°C in a reducing atmosphere for 2-20 hours; Step 4: crush the powder obtained in step 3 and pass it through a 200-300 mesh sieve, ball mill, filter, dry and sieve to obtain the target phosphor.

Citation Information

Patent Citations

  • Fluorescent powder capable of being effectively excited by blue light and preparation method thereof

    CN101812297A

  • Blue fluorescent powder and preparation method thereof

    CN102010710A