Preparation method and application of lithium ion sieve particles
Through extrusion granulation and surface oxidation treatment of carbon fiber filaments, the adsorption efficiency and cycle performance of lithium ion screen particles are improved, solving the problems of poor fluidity and low adsorption performance of existing lithium ion screen materials, and achieving more efficient lithium Application of ion sieve particles in salt lake brine.
Patent Information
- Application Number
- CN202380010020.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-06-16
AI Technical Summary
Existing lithium ion screen materials have poor fluidity and low cycle efficiency in industrial applications, and their powdery state results in high pressure drop. They cannot be effectively used to extract lithium from salt lake brine, and commonly used binders reduce the diffusion capacity and adsorption performance of lithium ions. .
The lithium ion sieve powder is mixed with a binder and a pore-forming agent for extrusion granulation to form porous particles, and a strong oxidizing solution is used to oxidize the carbon fiber filaments, which are then grafted onto the surface of the lithium ion sieve particles and combined with a silane coupling agent. , enhance interface strength and diffusion capacity, and improve adsorption efficiency.
It improves the adsorption efficiency and circulation performance of lithium ion screen particles, enhances the convective mass transfer effect, and improves the diffusion capacity and permeability of lithium ions, making it suitable for long-term recycling.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium extraction from salt lakes, and in particular relates to a preparation method of lithium ion sieve particles and application thereof. Background Art
[0002] Salt lake lithium resources account for more than 69% of the world's industrial lithium reserves. The world's salt lake lithium resources are mainly distributed in South America, North America and Asia. Salt lake areas are often sparsely populated, with incomplete infrastructure and insufficient energy supply, which has brought serious constraints to the development and utilization of these lithium resources. The main methods for extracting lithium from brine include evaporation crystallization, precipitation, extraction, adsorption, calcination, membrane separation and other methods.
[0003] Among them, the adsorption method uses lithium-selective adsorbents to separate and extract lithium. It is especially suitable for salt lake brine with high Mg / Li. The key to this method lies in the selection of adsorbent materials. Generally, adsorbent materials can be divided into two categories: organic adsorbents and inorganic adsorbents. Organic adsorbents usually use strong acidic cation exchange resins to selectively collect and recover lithium from lithium-containing solutions. They mainly rely on Coulomb force to adsorb lithium ions into the resin. However, this type of adsorbent has a low affinity for lithium ions and is not highly selective for lithium ions, making it unsuitable for lithium extraction and recovery. The working principle of inorganic lithium adsorbents mainly relies on the inorganic lithium ion adsorbents for Li + The unique memory effect and selectivity of inorganic lithium ion adsorbents have the advantages of low cost, good cycle stability and high selectivity, and have become the most promising adsorbent for adsorbing lithium ions from lithium-containing solutions. According to the classification of the main elements in inorganic lithium ion adsorbent materials, they mainly include aluminum salt adsorbents, antimony acid adsorbents, titanium oxide adsorbents and manganese oxide adsorbents.
[0004] Although these lithium ion sieve materials have the advantages of large adsorption capacity, high selectivity, and good cycle stability, they usually exist in powder form. They have poor fluidity, low cycle efficiency, and are easy to lose in industrial applications. In addition, powdered ion sieve materials can cause large pressure drops, resulting in high energy consumption in column operations, and cannot be directly used for lithium extraction in salt lake brine. These shortcomings are currently mainly overcome by the granulation molding technology of powder lithium ion sieve. The granulation method is to evenly mix lithium ion sieve powder and adhesive polymers together, and then form spherical particles through the polymerization reaction of the binder itself. Through granulation, the powder ion sieve can have good mechanical strength, so that it can adapt to industrial column operations, and effectively improve the recycling and permeability of lithium ion sieve powder. Materials with PVC, PVDF, etc. as binders have excellent mechanical properties, acid and alkali resistance, easy molding and low cost, but compared with powder adsorbents, the adsorption performance of ion sieve particles after granulation will be significantly reduced. This is because PVC and PVDF binders are hydrophobic materials, which reduce the diffusion capacity of lithium ions. There are also related reports on the use of binders containing hydrophilic groups such as agar, chitosan, polyacrylonitrile, and polyacrylamide to granulate powders, thereby improving the adsorption performance by increasing the permeability and wettability of adsorbed water. However, hydrophilic binders have low stability in water and poor mechanical properties, which reduces the circulation performance of the adsorbent and are not suitable for long-term use. Summary of the invention
[0005] The present disclosure aims to at least solve the technical problems existing in the above-mentioned prior art. To this end, the present disclosure provides a preparation method of lithium ion sieve particles and application thereof.
[0006] According to one aspect of the present disclosure, a method for preparing lithium ion sieve particles is provided, comprising the following steps:
[0007] S1: mixing lithium ion sieve powder, a binder and a pore-forming agent, and then extruding and granulating the mixture to obtain porous particles;
[0008] S2: placing the carbon fiber filaments in a strong oxidizing solution for a first heating treatment, taking out the carbon fiber filaments and washing and drying them to obtain modified carbon fiber filaments;
[0009] S3: placing the modified carbon fiber filaments in a silane coupling agent solution for a second heating treatment to obtain a suspension, adding the porous particles to the suspension and mixing, performing a third heating treatment, filtering and drying to obtain the lithium ion sieve particles.
[0010] In some embodiments of the present disclosure, in step S1, the lithium ion sieve powder is a titanium-based lithium ion sieve, a manganese-based lithium ion sieve, or an aluminum-based lithium ion sieve.
[0011] In some embodiments of the present disclosure, in step S1, the binder is at least one of PVDF, PVC or epoxy resin.
[0012] In some embodiments of the present disclosure, in step S1, the pore-forming agent is at least one of ethanol, isopropanol or n-butanol. The pore-forming agent is a volatile organic compound, and the high temperature environment accompanying the extrusion process allows the pore-forming agent to volatilize quickly and generate gas, so that the extruded particles have a porous structure, and the porous structure has strong liquid absorption.
[0013] In some embodiments of the present disclosure, in step S1, the extrusion granulation is performed using an extruder, and the segmented temperature range of the extruder is 110-250°C.
[0014] In some embodiments of the present disclosure, in step S1, the mass ratio of the lithium ion sieve powder to the pore-forming agent is 1:(0.1-0.2).
[0015] In some embodiments of the present disclosure, in step S1, the mass ratio of the lithium ion sieve powder to the binder is 1:(0.15-0.3).
[0016] In some embodiments of the present disclosure, in step S1, the porous particles have a particle size of 1-5 mm.
[0017] In some embodiments of the present disclosure, in step S2, the strong oxidizing solution is at least one of nitric acid, sodium hypochlorite, hydrogen peroxide, ammonium persulfate, acidic potassium permanganate, acidic potassium dichromate or potassium persulfate.
[0018] In some embodiments of the present disclosure, in step S2, the temperature of the first heating treatment is 70-90° C. and the time is 3-6 hours.
[0019] In some embodiments of the present disclosure, in step S2, the length of the carbon fiber filaments is 0.1-2 mm.
[0020] In some embodiments of the present disclosure, in step S3, the temperature of the second heating treatment is 60-80° C. and the time is 2-4 hours.
[0021] In some embodiments of the present disclosure, in step S3, the temperature of the third heating treatment is 90-110° C., and the time is 1-3 hours.
[0022] In some embodiments of the present disclosure, in step S3, the silane coupling agent is at least one of 3-aminopropyltriethoxysilane or 3-aminopropyltrimethoxysilane.
[0023] In some embodiments of the present disclosure, in step S3, the silane coupling agent solution is prepared by ultrasonic dispersion according to the mass ratio of silane coupling agent: anhydrous ethanol = 1: (4-5).
[0024] In some embodiments of the present disclosure, in step S3, the mass content of carbon fiber filaments in the lithium ion sieve particles is 1%-10%.
[0025] The present disclosure also provides application of the lithium ion sieve particles prepared by the preparation method in extracting lithium from salt lakes.
[0026] According to the embodiments of the present disclosure, there are at least the following beneficial effects:
[0027] The present invention utilizes a strong oxidizing solution to perform surface oxidation etching on carbon fiber filaments, and introduces oxygen-active functional groups (such as hydroxyl and carboxyl groups), which can improve the hydrophilicity of carbon fiber filaments, reduce the surface tension of carbon fiber filaments, and make them easy to disperse evenly in the solution without attracting each other and affecting the processing performance. The oxidized carbon fiber is first combined with a silane coupling agent and then grafted to the surface of lithium ion sieve particles. Silane coupling serves as a bridging agent between carbon fiber filaments and lithium ion sieve particles. The silane alkoxy end reacts with the oxygen-active functional groups of carbon fiber filaments, and the organic functional group end combines with the hydrophobic binder in the lithium ion sieve particles, so that there are multiple interface bonding effects such as covalent bonds and hydrogen bonds in the interface area, which plays a good bridging role, thereby being able to improve the interface strength between the carbon fiber and the lithium ion sieve particles. The present invention connects carbon fiber filaments to the surface of lithium ion sieve particles. The carbon fiber filaments can disturb the solution near the lithium ion sieve particles, enhance the convective mass transfer effect near the lithium ion sieve particles, and make the lithium-containing solution near the lithium ion sieve particles enter the pores of the particles more smoothly and quickly, thereby improving the problem of hydrophobic binders reducing the diffusion capacity of lithium ions. The disturbance of the solution by the carbon fiber filaments on the surface of the particles increases the diffusion capacity of lithium ions in the solution, thereby improving the adsorption efficiency of the lithium ion sieve particles. Compared with hydrophilic binders, hydrophobic binders have higher stability in water and better mechanical properties, and are suitable for the recycling of lithium ion sieve particles. In addition, the polar groups introduced into the carbon fiber after surface treatment enhance the hydrophilicity, which can further improve the permeability and wettability of the lithium ion sieve particles in the solution, thereby improving the adsorption efficiency. DETAILED DESCRIPTION
[0028] The concept of the present disclosure and the technical effects produced will be clearly and completely described below in conjunction with embodiments to fully understand the purpose, features and effects of the present disclosure.
[0029] Example 1
[0030] This embodiment prepares a lithium ion sieve particle, and the specific process is as follows:
[0031] (1) Manganese lithium ion sieve powder MnO2·0.5H2O, PVDF, and ethanol were mixed in a mass ratio of 1:0.2:0.1, and then extruded and granulated using a twin-screw extruder. The first section temperature of the extruder was 130°C, the second section temperature was 170°C, the third section temperature was 190°C, the fourth section temperature was 210°C, and the die head temperature was 230°C. After extrusion, the extruded strips were pelletized using a pelletizer to obtain porous particles with a particle size D50 of 2.3 mm.
[0032] (2) Immerse carbon fiber filaments with a length of about 0.5 mm in a 2 mol / L nitric acid solution and reflux at 85° C. for 4 h to perform surface oxidation treatment on the carbon fiber filaments. Take out the carbon fiber and wash and dry it to obtain improved carbon fiber filaments.
[0033] (3) placing the improved carbon fiber yarn in a 3-aminopropyltriethoxysilane solution (3-aminopropyltriethoxysilane: anhydrous ethanol solution mass ratio = 1:4), reflux at 75°C for 2.5 hours, cool to room temperature, then add the porous particles of step (1) to the above suspension and mix well, reflux at 100°C for 1.5 hours, filter after the reaction is completed, and dry to obtain lithium ion sieve particles with carbon fibers attached to the surface, wherein the mass content of carbon fibers in the product lithium ion sieve particles is 4%.
[0034] Example 2
[0035] This embodiment prepares a lithium ion sieve particle, and the specific process is as follows:
[0036] (1) Manganese lithium ion sieve powder MnO2·0.5H2O, PVDF, and isopropanol were mixed in a mass ratio of 1:0.15:0.15, and then extruded and granulated using a twin-screw extruder. The first section temperature of the extruder was 130°C, the second section temperature was 170°C, the third section temperature was 190°C, the fourth section temperature was 210°C, and the die head temperature was 230°C. After extrusion, the extruded strips were pelletized using a pelletizer to obtain porous particles with a particle size D50 of 4.0 mm.
[0037] (2) Immerse carbon fiber filaments with a length of about 1 mm in a 2 mol / L nitric acid solution and reflux at 90° C. for 3 h to perform surface oxidation treatment on the carbon fiber filaments. Take out the carbon fiber and wash and dry it to obtain improved carbon fiber filaments.
[0038] (3) placing the improved carbon fiber yarn in a 3-aminopropyltrimethoxysilane solution (3-aminopropyltrimethoxysilane: anhydrous ethanol solution mass ratio = 1:5), reflux at 70°C for 5 hours, cool to room temperature, then add the porous particles of step (1) to the above suspension and mix well, reflux at 95°C for 2 hours, filter after the reaction is completed, and dry to obtain lithium ion sieve particles with carbon fibers attached to the surface, wherein the mass content of carbon fibers in the product lithium ion sieve particles is 3%.
[0039] Example 3
[0040] This embodiment prepares a lithium ion sieve particle, and the specific process is as follows:
[0041] (1) Manganese lithium ion sieve powder MnO2·0.5H2O, PVDF, and ethanol were mixed in a mass ratio of 1:0.3:0.1, and then extruded and granulated using a twin-screw extruder. The first section temperature of the extruder was 130°C, the second section temperature was 170°C, the third section temperature was 190°C, the fourth section temperature was 210°C, and the die head temperature was 230°C. After extrusion, the extruded strips were pelletized using a pelletizer to obtain porous particles with a particle size D50 of 5 mm.
[0042] (2) Immerse carbon fiber filaments with a length of about 1.2 mm in a 1 mol / L sodium hypochlorite solution and reflux at 90° C. for 3 h to perform surface oxidation treatment on the carbon fiber filaments. Take out the carbon fiber and wash and dry it to obtain improved carbon fiber filaments.
[0043] (3) placing the improved carbon fiber yarn in a 3-aminopropyltriethoxysilane solution (3-aminopropyltriethoxysilane: anhydrous ethanol solution mass ratio = 1:4), reflux at 80°C for 3 hours, cool to room temperature, then add the porous particles of step (1) to the above suspension and mix well, reflux at 110°C for 3 hours, filter after the reaction is completed, and dry to obtain lithium ion sieve particles with carbon fibers attached to the surface, wherein the mass content of carbon fibers in the product lithium ion sieve particles is 7%.
[0044] Comparative Example
[0045] This comparative example prepares a lithium ion sieve particle. The difference from Example 1 is that only step (1) of Example 1 is performed, and the obtained porous particle is the lithium ion sieve particle of this comparative example.
[0046] Test example
[0047] The adsorption performance of the lithium ion sieve particles prepared in the above embodiments and comparative examples was tested. The test method is as follows: 300 g of the lithium ion sieve particles of the embodiments and comparative examples were weighed and filled into an adsorption column, 10 kg of brine was weighed, and adsorption was performed through the column at a rate of 5 seconds per drop, the lithium content after passing through the column was tested, and the lithium adsorption capacity was calculated. The results are shown in Table 2.
[0048] The calculation formula of adsorption capacity is as follows: adsorption capacity = (lithium content in brine before adsorption - lithium content in brine after adsorption) * mass of brine passing through the column / mass of lithium ion sieve particles.
[0049] Table 1 Chemical composition of salt lake brine
[0050] element Mg Na K Ca Li Content (ppm) 63528.7 2716.6 703.5 276.4 186.2
[0051] Table 2 Lithium adsorption capacity and cyclic adsorption performance of lithium ion sieve particles
[0052] sample Li adsorption capacity (mg / g) 100 cycles adsorption capacity retention rate / % Example 1 53.6 99.6 Example 2 52.7 99.7 Example 3 54.4 99.6 Comparative Example 35.5 99.5
[0053] It can be seen from Table 2 that the lithium adsorption capacity of the embodiment is higher than that of the comparative example, indicating that the lithium ion sieve particles disclosed in the present invention have higher adsorption efficiency after being grafted with carbon fiber filaments.
Claims
1. A method for preparing lithium ion sieve particles, characterized in that: The following steps are involved: S1: mixing lithium ion sieve powder, a binder and a pore-forming agent, and then extruding and granulating the mixture to obtain porous particles; S2: placing the carbon fiber filaments in a strong oxidizing solution for a first heating treatment, taking out the carbon fiber filaments and washing and drying them to obtain modified carbon fiber filaments; S3: placing the modified carbon fiber filaments in a silane coupling agent solution for a second heating treatment to obtain a suspension, adding the porous particles to the suspension and mixing, performing a third heating treatment, filtering and drying to obtain the lithium ion sieve particles; In step S1, the porous particles have a particle size D50 of 1-5 mm; In step S2, the length of the carbon fiber filaments is 0.1-2 mm.
2. The preparation method according to claim 1, characterized in that: In step S1, the lithium ion sieve powder is a titanium-based lithium ion sieve, a manganese-based lithium ion sieve or an aluminum-based lithium ion sieve.
3. The preparation method according to claim 1, characterized in that: In step S1, the adhesive is at least one of PVDF, PVC or epoxy resin.
4. The preparation method according to claim 1, characterized in that: In step S1, the pore-forming agent is at least one of ethanol, isopropanol or n-butanol.
5. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of the lithium ion sieve powder to the pore-forming agent is 1:(0.1-0.2).
6. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of the lithium ion sieve powder to the binder is 1:(0.15-0.3).
7. The preparation method according to claim 1, characterized in that: In step S2, the strong oxidizing solution is at least one of nitric acid, sodium hypochlorite, hydrogen peroxide, ammonium persulfate, acidic potassium permanganate, acidic potassium dichromate or potassium persulfate.
8. The preparation method according to claim 1, characterized in that: In step S2, the temperature of the first heating treatment is 70-90°C and the time is 3-6 hours.
9. The preparation method according to claim 1, characterized in that: In step S3, the temperature of the second heating treatment is 60-80°C and the time is 2-4 hours.
10. The preparation method according to claim 1, characterized in that: In step S3, the temperature of the third heating treatment is 90-110° C. and the time is 1-3 hours.
11. The preparation method according to claim 1, characterized in that: In step S3, the silane coupling agent is at least one of 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane.
12. The preparation method according to claim 1, characterized in that: In step S3, the silane coupling agent solution is prepared by ultrasonic dispersion according to the mass ratio of silane coupling agent to anhydrous ethanol = 1: (4-5).
13. The preparation method according to claim 1, characterized in that: In step S3, the mass content of carbon fiber filaments in the lithium ion sieve particles is 1%-10%.
14. Use of the lithium ion sieve particles obtained by the preparation method according to any one of claims 1 to 13 in extracting lithium from salt lakes.
Citation Information
Patent Citations
Lithium-titanium composite oxide electrode material conjugated with fine carbon fibers
CN103181004A
Preparation of conductive manganese-titanium lithium ion sieve / graphene composite hydrogel and application of conductive manganese-titanium lithium ion sieve / graphene composite hydrogel in extraction of lithium from salt lake brine
CN111250063A