A high-stability transition metal high-entropy oxygen carrier and its preparation method and application

By preparing high-entropy oxides (MnFeCoNiCu)O4-x or (MnFeCoNiCu)O4-x/M as oxygen carriers, the problem of poor stability of oxygen carriers was solved, and the effect of efficient catalytic synthesis of gas in biomass chemical chain reaction was achieved.

CN117019168BActive Publication Date: 2024-11-15SOUTH CHINA AGRICULTURAL UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310785721.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-29
Publication Date
2024-11-15
Estimated Expiration
2043-06-29

AI Technical Summary

Technical Problem

Existing oxygen carriers have poor stability in biomass chemical chain reactions and are difficult to restore to their original state after intense phase transitions, thus failing to meet the requirements for efficient catalytic synthesis gas.

Method used

A highly stable oxygen carrier was prepared by using high-entropy oxides (MnFeCoNiCu)O4-x or (MnFeCoNiCu)O4-x/M, through metal salt preparation, alkaline solution stirring, precipitate drying and calcination, and combined with oxides of Zr, Ce, Mg, Y and Er as the substrate.

Benefits of technology

The prepared highly stable oxygen carrier has a strong oxygen release capacity at low temperatures, can maintain structural stability in chemical looping, is suitable for large-scale production, and has strong oxygen release and recovery capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117019168B_ABST
    Figure CN117019168B_ABST
Patent Text Reader

Abstract

The present invention provides a high-stability transition metal high-entropy oxygen carrier and a preparation method and application thereof. The high-stability transition metal high-entropy oxygen carrier of the present invention is composed of (MnFeCoNiCu)O 4‑x or (MnFeCoNiCu)O 4‑x / M, the oxygen carrier has a strong oxygen release capacity, and can release a large amount of lattice oxygen to supply the chemical chain reaction at a relatively low temperature (400-700°C). At the same time, it has a strong recovery ability, can maintain a certain original crystal structure after a large amount of oxygen release, and restore to its original state after the chemical chain cycle, and has a strong cycle stability. The raw materials used are cheap and easy to obtain, the preparation method is simple, the equipment requirements are low, and it is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of chemical chain materials, and in particular to a high-stability transition metal high-entropy oxygen carrier and a preparation method and application thereof. Background Art

[0002] Biomass chemical chain technology is an efficient technology that can convert biomass into industrial raw materials - synthesis gas. The oxygen carrier transfers lattice oxygen to the biomass in an inert environment, causing the biomass to undergo partial oxidation to produce synthesis gas. The oxygen carrier then regains oxygen from the air and returns to its original state, forming a complete cycle. The raw materials of biomass chemical chain technology come from a wide range of sources. Straw, garden waste, urban domestic waste, etc. can all be used as raw materials; the oxygen carriers of biomass chemical chain technology can be recycled and have low economic costs; biomass chemical chain technology does not come into contact with air during the production of synthesis gas, the concentration of synthesis gas in the product is high, and the cost of separating and extracting the product is low. Therefore, biomass chemical chain technology is environmentally friendly, low-carbon, economical, and efficient.

[0003] Oxygen carriers are the key to biomass chemical chain technology. Excellent oxygen carriers must have the characteristics of good reaction effect, high stability, strong selectivity, and low price. Transition metal oxides have the characteristics of high oxygen carrying capacity and low price, so transition metal oxides are often used as oxygen carriers in biomass chemical chain technology. However, the stability of oxides of a single element is too poor, so composite oxides are often used as oxygen carriers, such as mixtures of metal oxides and inert carriers (such as Al2O3, MgO, SiO2, ZrO2, TiO2), or compounds such as spinel, perovskite, and hydrotalcite. However, since the oxygen carriers in the chemical chain reaction need to undergo strong phase changes and return to their original state after the reaction, most of these oxides still do not meet the demand.

[0004] High entropy oxides are potential new generation oxygen carriers, which are composed of five or more metal or non-metal elements. They are entropy stable and can recover to their original state after a strong phase change. There are almost no reports on the application of high entropy oxides in the field of chemical chaining, and the properties of high entropy oxides are very suitable for use in this field, so the combination of high entropy oxides and chemical chaining is expected. Summary of the invention

[0005] The purpose of the present invention is to overcome the disadvantage of poor stability of existing oxygen carriers and provide a method for preparing a high-stability high-entropy oxygen carrier for biomass chemical chain. The high-entropy oxygen carrier obtained by the preparation method has the characteristics of strong oxygen release capacity, selectivity for synthesis gas, high stability, etc.

[0006] The purpose of the present invention is achieved through the following technical solutions:

[0007] A highly stable transition metal high entropy oxygen carrier, the composition of which is (MnFeCoNiCu)O 4-x or (MnFeCoNiCu)O 4-x / M, wherein M includes at least one metal oxide, x represents the oxygen atom missing from the base transition metal high entropy oxide in the oxygen carrier, and the range of x is 0-4.

[0008] The metal oxide is a non-transition metal oxide; preferably an oxide formed by at least one metal selected from the group consisting of Zr, Ce, Mg, Y and Er; more preferably at least one selected from the group consisting of ZrO2, CeO2, MgO, Y2O3 and Er2O3.

[0009] The highly stable transition metal high entropy oxygen carrier can catalyze the biomass chemical chain to produce synthesis gas.

[0010] The method for preparing the highly stable transition metal high entropy oxygen carrier comprises the following steps:

[0011] (1) preparing a metal salt precursor solution using a metal salt;

[0012] (2) preparing an alkaline solution;

[0013] (3) adding an alkaline solution to a metal salt precursor solution, stirring, filtering, and drying to obtain a precipitate;

[0014] (4) calcining the precipitate obtained in step (3) to obtain a transition metal high entropy oxygen carrier.

[0015] The metal salt in step (1) includes metal salts of at least five transition metals and at least one non-transition metal.

[0016] The metal salt in step (1) is a hydrate of nitrate, acetate or sulfate.

[0017] The ratio of the total molar amount of the metal salt of the transition metal to the molar amount of the metal salt of the non-transition metal is 1-2:1-2; preferably 1:1.

[0018] The metal salt of the transition metal is a metal salt of Mn, Fe, Co, Ni and Cu; preferably manganese acetate tetrahydrate, iron nitrate nonahydrate, cobalt acetate tetrahydrate, nickel nitrate hexahydrate and copper acetate monohydrate.

[0019] The metal salt of the non-transition metal is a metal salt formed by at least one of Zr, Ce, Mg, Y and Er; preferably at least one of ZrO2, CeO2, MgO, Y2O3 and Er2O3.

[0020] The preparation in step (1) is performed by stirring; preferably, the stirring is performed for 20 to 40 minutes.

[0021] The solvent of the solution in step (1) is water, and the amount added is based on the ability to dissolve all solutes.

[0022] The base described in step (2) is anhydrous potassium carbonate.

[0023] The ratio of the molar amount of the base in step (2) to the total molar amount of the metal salt in step (1) is 1-2:1-2; preferably 1:1.

[0024] The preparation in step (2) is performed by stirring; preferably, stirring is performed for 20 to 40 minutes.

[0025] The solvent of the solution in step (2) is water, and the amount added is based on the ability to dissolve all solutes.

[0026] The addition in step (3) is performed dropwise; preferably, the addition is performed dropwise within 2 hours.

[0027] The stirring in step (3) is performed by stirring while adding the alkaline solution and continuing the stirring; preferably, stirring is performed while adding the alkaline solution for 2 hours and then continuing the stirring for 2 hours.

[0028] The filtration in step (3) is suction filtration.

[0029] The drying in step (3) is forced air drying; preferably drying at 105° C. for 12 h.

[0030] The calcination in step (4) is performed at 700-1000° C. in an air atmosphere for 0.5 h to 2 h; preferably, at 900° C. in an air atmosphere for 1 h.

[0031] The application of the highly stable transition metal high entropy oxygen carrier in the production of synthesis gas by biomass chemical chain.

[0032] The highly stable transition metal high entropy oxygen carrier is used in the preparation of a biomass chemical chain synthesis gas catalyst.

[0033] The biomass is bagasse.

[0034] The biomass chemical chain method for producing synthesis gas specifically comprises the following steps:

[0035] The biomass is mixed with an oxygen carrier, placed under a protective atmosphere, heated, and the synthesis gas is collected.

[0036] The protective atmosphere is a nitrogen atmosphere.

[0037] The heating is heating to 600-800°C.

[0038] Compared with the prior art, the present invention has the following advantages and effects:

[0039] The oxygen carrier prepared by the present invention has a strong oxygen release capacity and can release a large amount of lattice oxygen at a relatively low temperature (400-700° C.) to supply the chemical chain reaction. At the same time, it has a strong recovery ability and can maintain a certain original crystal structure after a large amount of oxygen release and restore the original state after the chemical chain cycle, and has a strong cycle stability. The raw materials used are cheap and easy to obtain, the preparation method is simple, the equipment requirements are low, and it is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 is the XRD characterization result diagram of the fresh transition metal high entropy oxygen carrier prepared in Examples 1 to 6; wherein the high entropy oxygen carrier includes: (MnFeCoNiCu)O 4-x / CeO2,(MnFeCoNiCu)O 4-x / ZrO2,(MnFeCoNiCu)O 4-x / MgO,(MnFeCoNiCu)O 4-x / Y2O3,(MnFeCoNiCu)O 4-x / Er2O3,(MnFeCoNiCu)O 4-x .

[0041] Figure 2 This is a diagram showing the results of the biomass chemical chaining reaction to produce synthesis gas using the transition metal high entropy oxygen carrier prepared in Examples 1 to 6.

[0042] Figure 3 This is the XPS characterization result diagram of the transition metal high entropy oxygen carrier prepared in Example 1 and the samples after 5 cycles and 10 cycles.

[0043] Figure 4 It is a SEM photograph of the transition metal high entropy oxygen carrier prepared in Example 1 and the sample after 10 cycles.

[0044] Figure 5 This is the XRD characterization result diagram of the transition metal high entropy oxygen carrier prepared in Example 1 and the sample after 5 cycles and 10 cycles.

[0045] Figure 6 This is a graph showing the results of 10 consecutive biomass chemical chain reactions to produce synthesis gas using the transition metal high entropy oxygen carrier prepared in Example 1. DETAILED DESCRIPTION

[0046] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0047] If no specific experimental conditions are specified in the following embodiments, conventional experimental conditions or experimental conditions recommended by the reagent company are generally followed. The materials and reagents used, unless otherwise specified, are all reagents and materials obtained from commercial sources.

[0048] Example 1 (MnFeCoNiCu)O 4-x Preparation of ZrO2

[0049] (1) 4.90 g of manganese acetate tetrahydrate, 8.08 g of iron nitrate nonahydrate, 4.98 g of cobalt acetate tetrahydrate, 4.98 g of nickel nitrate hexahydrate, 4.00 g of copper acetate monohydrate, and 42.93 g of zirconium nitrate pentahydrate were dissolved in 500 ml of deionized water and stirred for 30 min to form a precursor salt solution.

[0050] (2) Dissolve 0.9 mol of anhydrous potassium carbonate in 1000 ml of deionized water and stir for 30 minutes to form an alkaline solution.

[0051] (3) Add the alkaline solution dropwise to the precursor salt solution within 2 hours, stir, and gradually form a stable suspension. After all the alkaline solution is dripped into the precursor salt solution and stirred for 2 hours, continue stirring for 2 hours. Then use a circulating water vacuum pump to filter, wash the filter residue with 100 ml of deionized water for 3 times, and then put it into a 105°C forced air drying oven to dry for 12 hours to obtain a precipitate;

[0052] (4) The precipitate obtained in step (3) was placed in a muffle furnace and calcined at 900° C. for 1 h to obtain a transition metal high entropy oxygen carrier (MnFeCoNiCu)O 4-x / ZrO2, and then the obtained oxygen carrier was subjected to XRD / XPS characterization test. The results are as follows Figure 1 and Figure 3 shown.

[0053] Example 2 (MnFeCoNiCu)O 4-x Preparation of CeO2

[0054] (1) 4.90 g of manganese acetate tetrahydrate, 8.08 g of iron nitrate nonahydrate, 4.98 g of cobalt acetate tetrahydrate, 4.98 g of nickel nitrate hexahydrate, 4.00 g of copper acetate monohydrate, and 43.42 g of cerium nitrate hexahydrate were dissolved in 500 ml of deionized water and stirred for 30 min to form a precursor salt solution.

[0055] (2) Prepare (MnFeCoNiCu)O by referring to the method of steps (2) to (4) of Example 1 4-x / CeO2.

[0056] Example 3 (MnFeCoNiCu)O 4-x Preparation of MgO

[0057] (1) 4.90 g of manganese acetate tetrahydrate, 8.08 g of iron nitrate nonahydrate, 4.98 g of cobalt acetate tetrahydrate, 4.98 g of nickel nitrate hexahydrate, 4.00 g of copper acetate monohydrate, and 25.64 g of magnesium nitrate hexahydrate were dissolved in 500 ml of deionized water and stirred for 30 min to form a precursor salt solution.

[0058] (2) Prepare (MnFeCoNiCu)O by referring to the method of steps (2) to (4) of Example 1 4-x / MgO.

[0059] Example 4 (MnFeCoNiCu)O 4-x Preparation of Y2O3

[0060] (1) 4.90 g of manganese acetate tetrahydrate, 8.08 g of iron nitrate nonahydrate, 4.98 g of cobalt acetate tetrahydrate, 4.98 g of nickel nitrate hexahydrate, 4.00 g of copper acetate monohydrate, and 26.60 g of yttrium acetate hydrate were dissolved in 500 ml of deionized water and stirred for 30 min to form a precursor salt solution.

[0061] (2) Prepare (MnFeCoNiCu)O by referring to the method of steps (2) to (4) of Example 1 4-x / Y2O3.

[0062] Example 5 (MnFeCoNiCu)O 4-x Preparation of Er2O3

[0063] (1) Dissolve 4.90 g of manganese acetate tetrahydrate, 8.08 g of iron nitrate nonahydrate, 4.98 g of cobalt acetate tetrahydrate, 4.98 g of nickel nitrate hexahydrate, 4.00 g of copper acetate monohydrate, and 46.14 g of erbium nitrate hexahydrate in 500 ml of deionized water and stir for 30 minutes to form a precursor salt solution.

[0064] (2) Prepare (MnFeCoNiCu)O by referring to the method of steps (2) to (4) of Example 1 4-x / Er2O3.

[0065] Example 6 (MnFeCoNiCu)O 4-x Preparation

[0066] (1) Dissolve 4.90 g of manganese acetate tetrahydrate, 8.08 g of iron nitrate nonahydrate, 4.98 g of cobalt acetate tetrahydrate, 4.98 g of nickel nitrate hexahydrate, and 4.00 g of copper acetate monohydrate in 500 ml of deionized water and stir for 30 minutes to form a precursor salt solution.

[0067] (2) Prepare (MnFeCoNiCu)O by referring to the method of steps (2) to (4) of Example 1 4-x .

[0068] Example 7 Test of biomass chemical chaining to synthesis gas using transition metal high entropy oxide carriers

[0069] 1 g of the oxygen carrier prepared in Example 1 and 2 g of biomass (dried bagasse) were added to a straight quartz tube (length 350 mm, inner diameter = 12 mm) and fixed in the middle of the tube with quartz wool. -1 N2 was passed through the reactants at a total flow rate of 10 minutes to ensure that the air in the quartz tube was purged clean, and then the quartz tube was placed in a tube furnace at a constant temperature of 700°C for reaction. The generated gas was collected immediately after the reaction started, and the collection time was 2 minutes each time, and the concentration of the gas product in the reactor effluent was analyzed by GC (Agilent). After 30 minutes of reaction, N2 was switched to air, and the furnace temperature was raised to 900°C, and the reaction residue and Example 1 were calcined for 30 minutes.

[0070] The oxygen carriers prepared in Examples 2 to 6 were subjected to the same test.

[0071] The experimental results are as follows Figure 2 As shown, Example 1 has the highest ratio of synthesis gas (H2 and CO) and the least amount of CO2 produced, and the effect is most outstanding.

[0072] Example 8 (MnFeCoNiCu)O 4-x Study on the Cyclic Stability of ZrO2

[0073] According to the test method of Example 7, the oxygen carrier prepared in Example 1 was subjected to 10 consecutive cycle reaction tests, with 2 g of biomass added in each cycle; samples were taken at the 5th and 10th cycles for XPS characterization and XRD characterization, and the results were as follows: Figure 3 and Figure 5 In addition, SEM characterization was performed before the test and after 10 cycles. The results are shown in Figure 4 The results of the 10 consecutive cycles of the biomass chemical chain synthesis gas reaction in Example 1 are shown in Figure 6 shown.

[0074] The experimental results show that the effects of 1 to 10 cycles fluctuate within a certain range. Generally speaking, the effects of 10 cycles are relatively similar, indicating that the performance of Example 1 does not change much in 10 cycles and has high stability. Figure 3 to Figure 5 As shown in the figure, XRD / XPS / SEM characterization also proves that (MnFeCoNiCu)O 4-x The structure and composition of the / ZrO2 oxygen carrier did not change significantly, which proves that the oxygen carrier prepared in Example 1 has high stability.

[0075] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. Application of a high-stability transition metal high-entropy oxygen carrier in biomass chemical chain synthesis gas, characterized in that: The composition of the highly stable transition metal high entropy oxygen carrier is (MnFeCoNiCu)O 4-x / ZrO2 or (MnFeCoNiCu)O 4-x / Y2O3; The range of x is 0 to 4, but not 4.

2. The use according to claim 1, characterized in that: The preparation method of the highly stable transition metal high entropy oxygen carrier comprises the following steps: (1) preparing a metal salt precursor solution using a metal salt; (2) preparing alkaline solution; (3) adding the alkaline solution to the metal salt precursor solution, stirring, filtering, and drying to obtain a precipitate; (4) calcining the precipitate obtained in step (3) to obtain a transition metal high entropy oxygen carrier; The metal salt described in step (1) is manganese acetate tetrahydrate, iron nitrate nonahydrate, cobalt acetate tetrahydrate, nickel nitrate hexahydrate, copper acetate monohydrate and zirconium nitrate pentahydrate / yttrium acetate hydrate; The ratio of the total molar amount of manganese acetate tetrahydrate, iron nitrate nonahydrate, cobalt acetate tetrahydrate, nickel nitrate hexahydrate, and copper acetate monohydrate to the molar amount of zirconium nitrate pentahydrate / yttrium acetate hydrate is 1-2:1-2; The preparation in step (1) is stirring; The solvent of the solution in step (1) is water, and the amount added is based on the amount that can dissolve all the solutes; The base in step (2) is anhydrous potassium carbonate; The ratio of the molar amount of the base in step (2) to the total molar amount of the metal salt in step (1) is 1-2:1-2; The preparation in step (2) is stirring; The solvent of the solution in step (2) is water, and the amount added is based on the amount that can dissolve all the solutes; The adding in step (3) is performed dropwise; The stirring in step (3) is to stir while adding the alkaline solution, and continue stirring; The filtration in step (3) is suction filtration; The drying in step (3) is air drying; The calcination in step (4) is performed at 700-1000° C. in an air atmosphere for 0.5 h to 2 h.

Citation Information

Cited By

  • An oxygen storage material with enhanced oxygen mass transfer capability, and a preparation method and application thereof

    CN122895001A