Carbon nanodots synthesized from natural dried leaves, preparation method and application
Through high-temperature calcination and ultrasonic vibration treatment of naturally dried camphor tree leaves, carbon nanodots with high fluorescence intensity are prepared, which solves the problems of complex preparation process and non-environmental protection in the existing technology, and realizes low-cost, low-toxicity and high-efficiency nanomaterials. application.
Patent Information
- Application Number
- CN202310975389.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-03
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-08-03
AI Technical Summary
The preparation of existing luminescent carbon nanodots has problems such as cumbersome operations, high raw material costs, insufficient environmental protection, or the need to dope metals and other ingredients, resulting in low fluorescence intensity and limited application scenarios.
Naturally dried camphor tree leaves were used for high-temperature calcination and ultrasonic vibration treatment, and carbon nanodots were obtained through centrifugal separation and purification, achieving the preparation of low-cost, low-toxicity and environmentally friendly fluorescent nanomaterials.
We have realized carbon nanodots with a fluorescence intensity of over 1300, which can be used in fields such as anti-counterfeiting, cell imaging, and Co2+ detection. They have good water solubility and stability, simplifying the preparation process and reducing equipment requirements.
Smart Images

Figure CN117105210B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to carbon nanodots synthesized from natural dried leaves, a preparation method and application thereof, and belongs to the technical fields of new materials and energy conservation and environmental protection. Background Art
[0002] With the rapid development of science and technology, the materials studied in the past were at most micrometer-level, but in recent decades, they have shifted to the nanoscale, which has become an important direction of current scientific and technological development. Nano-sized materials are widely used in medicine, biosensor development, energy research, reaction catalysts and other related fields. Among them, fluorescent nanomaterials, because they can emit fluorescence, have great potential in the application of bio-labeling technology or optoelectronic materials. For example, semiconductor quantum dots such as cadmium sulfide (CdS) or cadmium selenide (CdSe) have been widely studied due to their high fluorescence stability.
[0003] Most of the materials with high quantum yield (QY) on the market contain heavy metal components, which increases the risk of biotoxicity and cytotoxicity. Not only are they prone to pollution during the synthesis process, but if they are not properly recycled after use, the harm to the environment cannot be underestimated. The above disadvantages limit the application scope of semiconductor quantum dots. In recent years, luminescent carbon nanodots have become a novel material with advantages such as easy preparation, low cost, low cytotoxicity, photostability and quantum size effect (Zhang. et al., 2010). Recently, some literature has also pointed out that carbon nanodots exist in the three-in-one coffee powder we drink daily (Jiang et al., 2014), which can be inferred that carbon nanodots should have higher biocompatibility and lower toxicity. So far, many technologies for synthesizing nanocarbon dots have been developed, including: laser ablation, arc discharge, electrochemistry, thermal decomposition, ultrasound and microwave methods. Among them, the thermal decomposition method is simple, safe, fast and effective. In the study of Wang, Liu, Zhang, and Lv (2012), it was found that this method has good optical properties, stability and biocompatibility.
[0004] There are some reports on the use of biomass materials to prepare luminescent carbon nanodots. For example, CN 114044511 A discloses a method for preparing beer-based nitrogen and phosphorus co-doped biomass carbon dots and their application, which can be used for Fe 3+ A new method for detecting ascorbic acid; CN 109734073 A uses wormwood leaves as a carbon source for carbon quantum dots. The prepared carbon quantum dot solution is yellow and transparent under natural light, and bright blue fluorescence can be seen under 365nm ultraviolet light excitation; CN 110373185 A uses paper mulberry leaves as a carbon source to synthesize fluorescent carbon dots, which can selectively detect Bi 3+, the detection limit is 2.0μmol / L; CN 110308126 A uses neem leaves to synthesize fluorescent nanocarbon dots through a hydrothermal method, which can be used for cell imaging; CN 113023708 A dissolves the smoke from the burning of sugarcane bagasse in a sugarcane sugar factory into pure water, and separates and extracts nanocarbon dots from the particulate matter contained in the smoke through multi-stage membrane filtration, centrifugation and dialysis.
[0005] The current preparation of luminescent carbon nanodots has problems such as complicated operation, high raw material cost, the need to use chemicals such as organic solvents, which is not environmentally friendly, the need to dope with metals and other components, or high requirements for preparation equipment. The prepared luminescent carbon nanodots also have problems such as low fluorescence intensity, doping with metals, or limited functions, resulting in limited application scenarios. Summary of the invention
[0006] In order to solve at least one of the above problems, the inventors used naturally dried camphor tree fallen leaves as materials, dried them, calcined them at high temperature, and then subjected them to ultrasonic vibration and centrifugal separation and purification to obtain carbon nanodots. This method has the advantages of simple and safe operation, and the materials are widely available. At the same time, the production process does not require the use of any chemicals and the requirements for the preparation equipment are simple; the fluorescent nanomaterials prepared by the method of the present invention are low in cost, low in toxicity and environmentally friendly, and the fluorescence intensity can reach more than 1300, which can be used for anti-counterfeiting, cell imaging, Co 2+ Detection and other fields.
[0007] The first object of the present invention is to provide a method for preparing carbon nanodots by using naturally dried fallen leaves, comprising the following steps:
[0008] (1) Pre-treating naturally dried camphor tree leaves and grinding them into powder;
[0009] (5) placing the powder obtained in step (1) into a high-temperature furnace for calcining to obtain carbonized leaf powder, and then grinding the powder into fine powder;
[0010] (6) adding the fine powder obtained in step (2) into water and subjecting it to ultrasonic treatment to obtain a solution;
[0011] (7) Centrifuge the solution in step (3) and take out the supernatant to obtain a carbon nanodot solution.
[0012] In one embodiment, the pretreatment in step (1) refers to oven drying of the naturally dried leaves.
[0013] In one embodiment, the oven drying is drying in an oven at 80-85° C. for 20-28 hours;
[0014] Optionally, the oven drying is drying at 82° C. for 24 hours.
[0015] In one embodiment, the temperature of the high temperature furnace calcination in step (2) is controlled at 230-260°C.
[0016] Optionally, the temperature of the high-temperature furnace calcination in step (2) is controlled at 280°C.
[0017] In one embodiment, the calcination time in step (2) is 3-6 hours.
[0018] Optionally, the calcination time in step (2) is 3.5-4h
[0019] Optionally, the calcination time in step (2) is 4 hours.
[0020] In one embodiment, the uniform grinding time in step (2) can be determined according to actual conditions; optionally, 30-60 minutes; further, 30 minutes.
[0021] In one embodiment, the ratio of fine powder to water in step (3) is 5-30 ml of water per gram of fine powder.
[0022] In one embodiment, the ratio of fine powder to water in step (3) is 10 ml of water per gram of fine powder.
[0023] In one embodiment, the water in step (3) refers to distilled water or ultrapure water.
[0024] In one embodiment, the ultrasonic treatment shaking time in step (3) can be determined according to actual conditions; ultrasonic shaking can effectively break up agglomerated or large particles of carbon blocks, so that the fluorescent substance is effectively dissolved in water. Optionally, it is 2 hours.
[0025] In one embodiment, the number of revolutions of the centrifugation in step (4) is 5000 rpm / min.
[0026] In one embodiment, the centrifugation time in step (4) is 10 minutes.
[0027] The second object of the present invention is to provide a carbon nanodot solution prepared according to the above method.
[0028] In one embodiment, the carbon nanodot solution can be further dried to obtain solid or semi-solid carbon nanodots.
[0029] The third object of the present invention is to provide fluorescent ink containing the carbon nanodots.
[0030] The fourth object of the present invention is to provide an anti-counterfeiting material, which uses the carbon nanodots of the present invention or fluorescent ink containing the carbon nanodots of the present invention.
[0031] In one embodiment, the anti-counterfeiting material is an anti-counterfeiting film material, and the carbon nanodots of the present invention are added during the preparation process of the film.
[0032] The fifth object of the present invention is to provide applications of the carbon nanodots.
[0033] In one embodiment, the application includes use in the field of detection of cobalt ions.
[0034] In one embodiment, the detection of the cobalt ions is qualitative detection or quantitative detection.
[0035] In one embodiment, the application is for detecting cobalt ions in soil systems, water systems, and organisms.
[0036] In one embodiment, the application includes use in the field of cell imaging.
[0037] In one embodiment, the application is for preparing fluorescent ink for printing anti-counterfeiting marks.
[0038] Advantages and effects of the present invention:
[0039] (1) The method for preparing the synthetic carbon nanodots of the present invention uses naturally dried camphor tree fallen leaves as raw materials and does not require the use of any chemicals. The materials are widely available, low in cost, can achieve the recycling of waste, are environmentally friendly and safe, and have good economic value and practicality.
[0040] (2) The method for preparing the synthetic carbon nanodots of the present invention is simple to operate, has simple requirements on the preparation equipment, has a fast synthesis speed, and is easy to realize industrial application.
[0041] (3) The synthetic carbon nanodots prepared by the present invention have no cytotoxicity, a fluorescence intensity of more than 1300, good water solubility, fluorescence properties, and stability, and can achieve Co 2+ Selective detection.
[0042] (4) The carbon nanodots synthesized by the present invention can be used for anti-counterfeiting, cell imaging, Co 2+ In areas such as detection, for example, invisible ink or test strips can be developed. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a flow chart of drying, grinding, calcining and crushing of naturally dried leaves in Example 1 of the present invention; wherein 1 is an oven uamato DX-400, 2 is a mortar, 3 is a high-temperature furnace A-550, 4 is powder, 5 is fine powder, and 6 is a solution;
[0044] Figure 2The figure is a diagram of the experimental steps of ultrasound and centrifugation in Example 1 of the present invention; wherein 7 is an ultrasonic oscillator DC-200H, 8 is a centrifuge E-centrifuge, and 9 is a sample bottle;
[0045] Figure 3 This is a UV-visible spectrum diagram of the carbon nanodots synthesized from plants when diluted 400 times in Example 1 of the present invention;
[0046] Figure 4 The fluorescence spectra of carbon nanodots synthesized by plants at different excitation wavelengths in Example 1 of the present invention;
[0047] Figure 5 The fluorescence spectra of carbon nanodots synthesized by plants at different dilution ratios in Example 1 of the present invention;
[0048] Figure 6 A comparison of carbon nanodots synthesized using plants in Example 1 of the present invention under (1) sunlight and (2) UV light;
[0049] Figure 7 This is a comparison diagram of the Tyndall effect phenomenon of carbon nanodots synthesized by plants and pure water observed under sunlight in Example 1 of the present invention;
[0050] Figure 8 This is a comparison chart of writing NttU under UV light and under sunlight using ink made of plant-synthesized carbon nanodots in Example 1 of the present invention;
[0051] Fig. 9 is log(F0 / F) and Co 2+ Linear relationship graph of concentration;
[0052] Fig.10 This is a test diagram of the selectivity of fluorescent carbon dots to common metal ions. DETAILED DESCRIPTION
[0053] 1. Instruments used in the present invention
[0054] 1. Oven uamato DX-400
[0055] 2. High temperature furnace A-550
[0056] 3. Ultrasonic Oscillator DC-200H
[0057] 4. Centrifuge
[0058] 5.Ultraviolet lamp UVGL-25
[0059] 6. Fluorescence detector F-4500
[0060] 7. Lambda EZ-201 UV / Visible Light Detector
[0061] 2. Experimental Materials Used in the Present Invention
[0062] 1. Centrifuge tube
[0063] 2. Sample bottle
[0064] 3. Plastic Nipple Dropper
[0065] 4. Quartz glass bottle
[0066] 5. Mortar
[0067] 6. Naturally dried camphor leaves
[0068] 7. Distilled water
[0069] Example 1: A method for preparing synthetic carbon nanodots
[0070] A method for preparing carbon nanodots, the specific steps are as follows:
[0071] (1) Figure 1 As shown, the fallen leaves of camphor trees are picked up, dried naturally, and then placed in an oven 1 at about 82°C for 24 hours. 2g of the dried leaves are taken and ground into powder 4 using a mortar 2, and then placed in a high-temperature furnace 3 for calcination at 280°C for 4 hours. After burning, the carbonized leaf powder is taken and evenly ground into a fine powder using a mortar for 30 minutes.
[0072] (2) Figure 2 As shown, the carbonized leaf powder 5 ground into fine powder in the previous step is placed in a sample bottle 9, 20 mL of distilled water is added, and then placed in an ultrasonic oscillator 7. After oscillation for 2 hours, the solution is poured into a centrifuge tube, placed in a centrifuge 8, and centrifuged at a speed of 5000 rpm for 10 minutes. After centrifugation, the supernatant is taken to obtain a carbon nanodot solution. The carbon nanodot solution is placed in a sample bottle and stored in aluminum foil to avoid light.
[0073] The obtained carbon nanodot solution is analyzed, specifically including:
[0074] (1) UV-Visible spectroscopy and fluorescence spectroscopy analysis
[0075] The carbon nanodot solution was diluted with distilled water to the required concentration for the experiment, and after uniform mixing, UV-visible light spectrum and fluorescence spectrum tests were performed. The optical properties of the synthetic fluorescent substance were analyzed using absorption spectrum and fluorescence spectrum.
[0076] Figure 3 This is the absorption spectrum of the carbon nanodot solution after diluting it 400 times. Figure 3 It can be seen that in the wavelength range of 265nm-290nm, the absorbance is linearly related to the wavelength.
[0077] Figure 4 To utilize the emission spectra of different excitation wavelengths in fluorescence spectroscopy. Figure 4 It can be found that when the incident light is 320nm, the strongest fluorescence emission can be obtained at 455nm; at the same time, as the incident light increases from 300nm to 340nm, the position of the strongest emission spectrum also moves toward the long-wave direction; different emission wavelengths under different excitation wavelengths also illustrate the existence of carbon nanodots.
[0078] Figure 5 Fluorescence spectra at different dilution ratios. The carbon nanodot solution obtained in the experiment was used to measure the fluorescence intensity at different dilution ratios using an excitation wavelength of 320 nm; Figure 5 As shown in the figure, when the sample solution is diluted with distilled water, the fluorescence intensity increases with the dilution. When the sample solution is diluted 100 times, the fluorescence intensity is the highest, reaching 1325. Then, the fluorescence intensity gradually decreases with further dilution. This may be because the sample is prone to self-absorption at high concentrations, and dilution reduces the impact of this phenomenon.
[0079] (2) Analysis of the fluorescence characteristics of UV lamps
[0080] By using the fact that fluorescent substances can be affected by short wavelengths (such as UV light) and produce fluorescence, it is observed whether the carbon nanodot solution obtained in the experiment has fluorescent properties.
[0081] Figure 6 The left and right figures are the fluorescence of the carbon nanodot solution obtained in this embodiment after being diluted 100 times under ordinary fluorescent lamps and ultraviolet lamps (i.e., UV lamps). The results show that the diluted sample is transparent and colorless under ordinary fluorescent lamps, and produces blue fluorescence under UV lamps. It can be seen that the carbon nanomaterial obtained in this embodiment cannot produce fluorescence under sunlight.
[0082] (3) Analysis of the Tyndall effect
[0083] When a beam of laser light is transmitted through a colloid, another beam of light can be observed to be scattered from the colloid in the perpendicular direction of the incident light. This phenomenon is called the Tyndall effect. The Tyndall effect can distinguish between a true solution and a colloidal solution. When the particle size of a sol is between 1 and 100 nm, the light path can be observed due to light scattering, but the light path cannot be observed in a true solution.
[0084] Figure 7 This is the situation after a 100-fold diluted carbon nanodot solution and pure water were irradiated with laser light. Figure 7It can be clearly found that the diluted carbon nanodot solution has a light beam, which proves that the synthesized carbon nanodot solution is a colloidal solution, but the pure water on the right does not have this phenomenon. From this result, it can be seen that the carbon nanodots synthesized in this example contain fluorescent substances, which contain particles of 1 to 100 nm.
[0085] (4) Fluorescence stability analysis
[0086] A. Storage stability
[0087] The carbon nanodot solution was placed in a sample bottle with aluminum foil to protect it from light, stored at room temperature for different periods of time, and then diluted 100 times. The fluorescence intensity at an excitation wavelength of 320nm was measured to analyze the change in fluorescence intensity over time. The results are shown in Table 1. After being stored at room temperature for 2 months, the fluorescence intensity can still be maintained at more than 97%.
[0088] Table 1
[0089] Save time Fluorescence intensity Day 0 1325 15 days 1318 1 month 1302 2 months 1288
[0090] B. Ionic Strength Stability
[0091] The obtained carbon nanodot solution was diluted 100 times with NaCl solution of different concentrations, and the fluorescence intensity at an excitation wavelength of 320 nm was measured to analyze the change of fluorescence intensity with ion strength. The results are shown in Table 2, which are basically not affected by the concentration of NaCl solution.
[0092] Table 2
[0093] Concentration of NaCl solution (mol / L) Fluorescence intensity 0 1325 2 1321 4 1328 6 1322
[0094] Example 2: A method for preparing synthetic carbon nanodots
[0095] A method for preparing carbon nanodots, the specific steps are as follows:
[0096] (1) Pick up fallen leaves of camphor trees, dry them naturally, put them in an oven at about 85℃ for 20 hours, take 2g of dried leaves, grind them into powder with a mortar, and then put them into a high-temperature furnace at 260℃ for 3.6 hours. After burning, take the carbonized leaf powder and grind it evenly with a mortar for 50 minutes into a fine powder.
[0097] (2) The carbonized leaf powder ground into fine powder in the previous step was placed in a sample bottle, 20 mL of distilled water was added, and then placed in an ultrasonic oscillator. After oscillation for 3 hours, the solution was poured into a centrifuge tube, placed in a centrifuge, and centrifuged at 6000 rpm for 12 minutes. After centrifugation, the supernatant was taken to obtain a carbon nanodot solution. The carbon nanodot solution was placed in a sample bottle and stored in an aluminum foil paper to avoid light.
[0098] The obtained carbon nanodot solution has a fluorescence intensity of 1321 at an excitation wavelength of 320 nm after being diluted 100 times, and can maintain more than 97% of the fluorescence intensity after being stored at room temperature for 2 months, and can also maintain a fluorescence intensity of 1319 in a 6M NaCl solution.
[0099] Example 3: A method for preparing synthetic carbon nanodots
[0100] A method for preparing carbon nanodots, the specific steps are as follows:
[0101] (1) Pick up fallen leaves of camphor trees, dry them naturally, put them in an oven at about 80℃ and dry them for 28 hours, take 2g of the dried leaves, grind them into powder with a mortar, and then put them into a high-temperature furnace at 230℃ for 3.8 hours. After burning, take the carbonized leaf powder and grind it evenly with a mortar for 40 minutes into a fine powder.
[0102] (2) The carbonized leaf powder ground into fine powder in the previous step was placed in a sample bottle, 20 mL of distilled water was added, and then placed in an ultrasonic oscillator. After oscillation for 4 hours, the solution was poured into a centrifuge tube, placed in a centrifuge, and centrifuged at 8000 rpm for 16 minutes. After centrifugation, the supernatant was taken to obtain a carbon nanodot solution. The carbon nanodot solution was placed in a sample bottle and stored in an aluminum foil paper to avoid light.
[0103] The obtained carbon nanodot solution has a fluorescence intensity of 1319 at an excitation wavelength of 320 nm after being diluted 100 times, and can maintain 98% of the fluorescence intensity after being stored at room temperature for 2 months, and has a fluorescence intensity of 1320 in a 6M NaCl solution. Optimization Example 4: Effect of Calcination Time on Carbon Nanodots
[0104] The calcination time of Example 1 was adjusted, and the other steps and parameters were the same as those of Example 1. The fluorescence intensity of the carbon nanodots obtained at different calcination times at an excitation wavelength of 320 nm after dilution by 100 times was compared. The results showed that the fluorescence intensity was higher within 3.5-4 hours.
[0105] Table 3
[0106] Calcination time (h) Fluorescence intensity 4 (i.e. embodiment 1) 1325 3 1123 3.5 1322 4.5 1093 5 1083 6 1088
[0107] Application Example 1: Preparation of fluorescent ink using carbon nanodot solution
[0108] Figure 5 The results show that the carbon nanodot solution has the strongest fluorescence when it is diluted 100 times. Figure 8 As shown. Under UV light ( Figure 8 The words written on the picture above are clearly visible, but under fluorescent light ( Figure 8There is no fluorescence when illuminated by
[0109] Therefore, the carbon nanodot solution prepared in Example 1 can be further made into invisible ink for use and developed into a special anti-counterfeiting mark.
[0110] Application Example 2: Application of Carbon Nanodots in Biological Imaging
[0111] (1) Analysis of the toxicity of fluorescent carbon nanodot solution to cells
[0112] In order to determine the toxic effect of the fluorescent carbon nanodots prepared in Example 1 on cells, the cytotoxicity test was performed using mouse mononuclear macrophage RAW264.7 cells by MTT method. Specifically:
[0113] Mouse mononuclear macrophage RAW264.7 cells were cultured at 8×10 3 / well inoculated in a 96-well plate, after the cells adhered, a phosphate buffered saline solution (PBS) containing the fluorescent carbon nanodot solution prepared in Example 1 was added (the concentrations of the fluorescent carbon nanodot solution were 0, 50, 100, 200, 400, and 800 μL / mL, respectively), and incubated in a 37°C, 5% (volume fraction) CO2 incubator for 24 hours, and then 20 μL of thiazole blue solution (MTT, 5 mg / mL) was added to each well. After 4 hours of incubation in the incubator, the original culture solution was discarded, and 150 μL of DMSO solution was added to each well. The absorbance value of each well at 490 nm was measured by an enzyme marker, and the parallel experiment was repeated 3 times. The MTT results in the following table show that the fluorescent carbon nanodots prepared in Example 1 have almost no cytotoxicity to cells, and when the concentration reaches 800 μL / mL, it still has no effect on cell proliferation, indicating that the carbon nanodot solution prepared in Example 1 has almost no toxicity to cells, good biocompatibility, and can be used for cell imaging.
[0114] Table 4
[0115] Concentration of fluorescent carbon nanodot solution (μL / mL) Cell viability 0 100% 50 108% 100 121% 200 112% 400 109% 800 101%
[0116] (2) Application of fluorescent carbon nanodots in cell imaging
[0117] The fluorescent carbon nanodot solution prepared in Example 1 was used to perform imaging analysis on cells. Specifically:
[0118] RAW264.7 cells were inoculated in a multi-well plate at 150,000 cells / well, and incubated in a CO2 incubator at 37°C and 8% (volume fraction) for 24 hours. The original culture medium was discarded, and a PBS solution containing the fluorescent carbon nanodot solution prepared in Example 1 was added (the addition amount was 100 μL / mL). After overnight culture, the original culture solution was discarded, and the cells were washed three times with PBS buffer solution to wash away the residual fluorescent carbon nanodots on the cell surface. The excitation wavelength was set to 320nm, and the cell imaging was taken. The results showed that green fluorescence was emitted from the inside of the cell, and the cell structure could be clearly seen, indicating that the fluorescent carbon nanodots were able to enter the cell and effectively mark the cell.
[0119] Application Example 3: Carbon nanodots in metal ion Co 2+ Application in detection
[0120] Cobalt is an important industrial metal material for the production of heat-resistant alloys, hard alloys, anti-corrosion alloys, and magnetic alloys. Cobalt-based compounds (such as cobalt oxide, cobalt hydroxide, lithium cobalt oxide, etc.) are increasingly used in lithium-ion batteries, supercapacitors, and electrocatalytic oxidation. However, long-term exposure to a high-concentration cobalt environment will lead to excessive intake of cobalt and produce toxic effects, causing pneumonia, asthma, cardiomyopathy, contact dermatitis, goiter, gastrointestinal disorders and other diseases. In addition, cobalt and cobalt compounds are listed as Class 2A possible human carcinogens by the International Agency for Cancer.
[0121] Cobalt ions have the common properties of heavy metal ions: they are not biodegradable, and can be enriched hundreds or thousands of times through the food chain and eventually enter the human body. Therefore, environmental and biological monitoring of cobalt ions has gradually attracted people's attention and become the focus of research, especially the effective detection of cobalt ions in relevant water bodies.
[0122] This example analyzes the carbon nanodots in Example 1 on Co 2+ Application effect in detection.
[0123] (1) Qualitative and quantitative test analysis
[0124] With different concentrations of Co 2+ Solution (cobalt chloride) dilute the carbon nanodot solution obtained in Example 1 by 100 times to make Co 2+ The final concentrations were 0, 0.02, 0.04, 0.08, 0.2, 0.4, 0.80, 2, 4, 8, 10, 20, 40, 60, 80, 100, 120, 150, and 200 μM, respectively. After 5 min, the fluorescence intensity at 455 nm was measured at an excitation wavelength of 320 nm. 2+ The concentration is taken as the horizontal axis, and the concentration without Co 2+ Concentration (i.e. adding Co 2+ Before joining Co 2+The ratio of the fluorescence intensity of the solution after the test is taken as the logarithm log (F0 / F) as the ordinate, and a standard curve is drawn, such as Fig. 9 shown.
[0125] The results show that the fluorescence intensity of the system increases with the Co 2+ The solubility of Co 2+ The concentration is 2×10 -8 ~2×10 - 4 In the range of M, the logarithm of relative fluorescence intensity log(F0 / F) and Co 2+ The concentration has a good linear relationship, and its linear regression equation is log(F0 / F)=0.0046C(Co 2+ )+0.0137,R 2 Greater than 0.99, the minimum detection limit is 2×10 -8 M.
[0126] (2) Anti-interference capability test analysis
[0127] The carbon nanodots obtained in Example 1 were used to detect various metal ions in water, and the specific method was as follows:
[0128] The solutions containing different metal ions were diluted 100 times respectively to make the final concentration of metal ions in each solution 2×10 -4 M; 5 min later, the samples containing different metal ions (Mg 2+ 、Ni 2+ , Ca 2+ 、Al 3+ 、Na + , Li + , K + , Sr 2+ , Ba 2+ , Mn 2+ , Pb 2+ 、Ag + , Fe 2+ 、Cd 2+ 、Zn 2+ Cr 3+ , Cu 2+ , Fe 3+ , Hg 2+ 、Bi 3+ Cr 6+ ) at 455 nm, and then compared with F0 in Example 1 to calculate the F / F0 value of solutions containing different metal ions. The results are as follows Fig.10 Display. Combine Fig. 9 It can be seen that only when Co 2+When the carbon nanodots in Example 1 were present, the fluorescence intensity of the system was significantly weakened, and its F / F0 value was significantly reduced, indicating that the carbon nanodots in Example 1 had an 2+ There is good selectivity.
[0129] (3) Co 2+ Analysis of spike recovery
[0130] About Co 2+ The spike recovery was analyzed and the results showed that the spike recovery was 105%.
[0131] Application Example 4: Carbon nanodots in metal ion Co 2+ Application in detection
[0132] On the basis of Example 1, some preparation processes were changed to obtain carbon nanodots (other processes or parameters remained the same), and then the obtained carbon nanodot solution was subjected to the method in Example 3. 2+ The detection effect was analyzed, including the logarithm of the relative fluorescence intensity log(F0 / F) and Co 2+ concentration, and through the common metal ions (Pb 2+ , Fe 2+ 、Cd 2+ Cr 3+ , Cu 2+ , Hg 2+ 、Bi 3+ ) to determine whether the anti-interference test is effective for Co 2+ Be selective.
[0133] Table 5 Carbon nanodots obtained from different raw materials
[0134]
[0135] Table 6 Carbon nanodots obtained by different processes
[0136] Technology <![CDATA[Whether the relative fluorescence intensity is linearly correlated with the Co 2+ concentration]]> <![CDATA[Regarding Co 2+ With or without selectivity]]> Example 1 Related have Example 2 Related have Example 3 Related have Comparative Example 1 Not relevant none
[0137] Wherein, the process of comparative example 1 is:
[0138] (1) Pick up fallen leaves of camphor trees, dry them naturally, and then put them in an oven at about 82°C for 24 h. Take 2 g of the dried leaves, grind them into powder with a mortar, add 20 mL of distilled water, and then put them into a high-temperature furnace for calcination at 280°C for 4 h.
[0139] (2) Place the solution in an ultrasonic oscillator and shake for 2 hours, then pour the solution into a centrifuge tube, place the tube in a centrifuge, and centrifuge at 5000 rpm for 10 minutes. After centrifugation, take the supernatant to obtain the carbon nanodot solution.
[0140] Application Example 5: Carbon Nanodots in Soil Co2+ Application in detection
[0141] Distilled water was added to the soil sample to be tested, ultrasonically treated for a period of time, and the supernatant was centrifuged. The carbon nanodot solution obtained in Example 1 was diluted 100 times with the supernatant as solvent, and the fluorescence intensity at 455 nm was detected under an excitation wavelength of 320 nm. The logarithm of the relative fluorescence intensity log(F0 / F) was calculated and substituted into the linear regression equation to calculate the Co in the soil sample. 2+ Qualitative and quantitative detection.
[0142] Application Example 6: Fluorescent Anti-Counterfeiting Film
[0143] A fluorescent anti-counterfeiting film comprises a base layer, a visible and invisible layer and a surface coating layer which are sequentially arranged and stacked, wherein the base layer is made of polyvinyl pyrrolidone, the visible and invisible layer is drawn with fluorescent nano-carbon dots prepared in Example 1, and the surface coating layer is made of acrylic resin and epoxy acrylic resin.
[0144] Optionally, the preparation steps include:
[0145] S1, adding polyvinyl pyrrolidone to dichloromethane to prepare a solution, then spreading the solution on a glass sheet, and air-drying to obtain a base layer;
[0146] S2, drawing a pattern on the base layer with the fluorescent nano-carbon dot solution prepared in Example 1, and air-drying it to form a visible and invisible layer;
[0147] S3, coating the mixture of acrylic resin and epoxy acrylic resin on the visible and invisible layer so that it covers the visible and invisible layer, and air-drying to form a surface coating layer to obtain the anti-counterfeiting film.
Claims
1. A method for specific detection of cobalt ions, characterized in that: The method described uses carbon nanodots synthesized from naturally dried fallen leaves; the detection is used for the detection of cobalt ions in a water system; The preparation of carbon nanodots is as follows: (1) Pick up fallen leaves of camphor trees, dry them naturally, and then put them into an oven at 82°C for 24 hours; (2) Take 2 g of dry leaves, grind them into powder with a mortar, and then calcine them in a high-temperature furnace at 280°C for 4 h. After burning, take the carbonized leaf powder and grind it evenly with a mortar for 30 min into a fine powder. (3) The carbonized leaf powder ground into fine powder in the previous step was placed in a sample bottle, 20 mL of distilled water was added, and then placed in an ultrasonic oscillator. After oscillation for 2 hours, the solution was poured into a centrifuge tube, placed in a centrifuge, and centrifuged at 5000 rpm for 10 min. After centrifugation, the supernatant was taken to obtain a carbon nanodot solution.