Composite film with magnetic properties and method for preparing conductive electrode sheet using the composite film
By introducing a magnetic layer and an adhesive layer into the composite film, the magnetic adsorption force is used to achieve efficient re-peeling of the conductive electrodes, which solves the problems of insufficient re-peeling performance and unstable heat shrink glue in the existing technology, and improves production efficiency. and product quality.
Patent Information
- Application Number
- CN202311060030.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-08-22
AI Technical Summary
Existing composite films have insufficient re-peelability in the manufacturing of electronic equipment components. The heat shrinkable adhesive is unstable and can easily cause extrusion and deformation of the surrounding coatings, affecting the quality of the pole pieces. Moreover, there is a risk of secondary contamination during the cleaning process.
A composite film with a magnetic layer is used. The magnetic layer is formed by printing, spraying or plating magnetic materials. The magnetic adsorption force reaches more than 0.5Mpa. Combined with the adhesive layer and the high molecular polymer layer, the magnetic adsorption force of the magnetic layer is used to achieve excellent Peeling efficiency and easy sweeping through external stimulation.
It improves the production efficiency and product quality of conductive electrodes, reduces the risk of secondary pollution, avoids peeling failure and residual glue problems, and enhances the cleaning performance of the composite film.
Smart Images

Figure CN117116598B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a magnetic composite film and a preparation method thereof and a preparation method of a conductive electrode sheet using the composite film, belonging to the field of electronic equipment component preparation, in particular, to the field of energy storage electronic equipment component preparation. Background Art
[0002] Re-peelable composite films have been used in the manufacture of various electronic device components (such as semiconductor components, electrode components, etc.). The re-peelable property of the re-peelable composite film can be used to temporarily fix, transfer, and protect the entire or local parts of the components during the manufacturing process of these components.
[0003] Generally, these removable composite films are required to have satisfactory initial adhesive force when bonding to an adherend and to have adhesive force that decays over time or after being subjected to external stimulation so that they can be re-peeled whenever necessary.
[0004] The general requirement for re-peeling is that the composite film can be peeled off from the adherend surface as a whole and quickly under specified conditions, and such peeling should not cause damage to the adherend substrate (e.g., damage to the adherend surface) or contamination (e.g., part of the adhesive layer remains on the adherend surface), nor should the re-peeling quality or efficiency be reduced due to tearing of the composite film base film. In particular, as electronic equipment components become increasingly miniaturized and sophisticated, the requirements for composite film re-peeling are becoming increasingly higher.
[0005] When removing the covering tape after use, it is usually done by mechanical or semi-mechanical methods such as scraper sweeping, mechanical vibration peeling, or even manual peeling, which is a relatively rough process. In order to obtain a good peeling effect, higher performance requirements are put forward for the product to remove the masking, increase the peeling workability, and seek practical methods for peeling, such as using a tape that can automatically curl after heating. When the tape completes the covering function, the tape curls to a higher height so that the scraper can sweep it more easily, that is, the tape can automatically curl for easy removal.
[0006] For example, Reference 1 discloses a pressure-sensitive adhesive sheet comprising a layered structure of an energy-ray-curable pressure-sensitive adhesive layer and a heat-shrinkable film. This pressure-sensitive adhesive sheet can prevent elongation or creases in the sheet under the irradiation of ultraviolet light because the heat-shrinkable sheet shrinks under the irradiation of energy rays. However, although this technical solution utilizes heat shrinkage to shrink the substrate and increase the mechanical properties of the adhesive sheet, thereby preventing the adhesive sheet from breaking, etc., it is also found in actual operation that its overall re-peeling performance is insufficient.
[0007] Furthermore, with the large-scale industrial production of new energy equipment, the manufacturing requirements for electronic equipment components in energy storage devices are also increasing, both in terms of quality and efficiency.
[0008] It is known that when preparing the electrode plate in the energy storage device, it is usually necessary to plan the area for connecting the pole ear on the electrode surface after obtaining the metal electrode plate or electrode sheet. The position is further bonded with a composite film to play a temporary protective role. After that, the pole piece is coated with a composition containing an active substance to form an active layer. While or after the active layer is dried, the composite film is peeled off from the surface of the electrode plate by shrinking due to the heat, thereby exposing the weldable area.
[0009] For example, Reference 2 discloses a method for preparing a lithium-ion battery pole piece, comprising: pasting a heat shrink adhesive at the reserved position of the pole ear of the current collector, then coating the active material on the surface of the current collector and the heat shrink adhesive, and removing the heat shrink adhesive and the active material coated thereon after heating; the heat shrink adhesive comprises a substrate and a foaming adhesive layer. The one-way heat shrinkage rate of the substrate is 60-80%. However, the heat shrink adhesive used in this method is unstable and is prone to extrusion deformation of the surrounding coating during baking, thereby affecting the quality of the pole piece and reducing the product quality rate.
[0010] In addition, none of the above documents mention the final heat shrink adhesive cleaning process. The currently known cleaning method is to use a scraper for cleaning. Because the cleaning direction of the scraper is usually opposite to the direction of electrode production, the cleaning process may sweep the tape back into the furnace, causing secondary pollution in the electrode production. On the other hand, the curl balance requirements for the product are very high. If the curl is not enough, the scraper cannot be touched, and the tape is not swept away, polluting the product. If the curl is too large, the bonding area of the product is too small, resulting in insufficient bonding between the product and the electrode plate. The tape is blown away by the air pressure in the furnace, causing contamination during the drying process of the electrode plate in the furnace (such as Figure 7-9 shown).
[0011] In summary, although various studies have been conducted on the composite films used in the production of electronic components in the prior art, the improvements in the prior art are still not sufficient to provide a composite film with improved easy-to-clean and re-peel performance and improved production efficiency, and there is room for further exploration.
[0012] References:
[0013] Reference 1: Japanese Patent No. 3073239
[0014] Reference 2: CN105742565A Summary of the invention
[0015] Problem that the invention aims to solve
[0016] In view of the technical problems existing in the prior art, such as: the final sweeping efficiency of the tape, reducing the risk of secondary contamination of the tape during the production of the pole piece, insufficient overall re-peeling performance, unstable heat shrink adhesive, easy to cause extrusion deformation of the surrounding coating, affecting the quality of the pole piece, etc., the present invention first provides a composite film with magnetic properties, which is particularly suitable for electronic equipment components, new energy lithium batteries, and especially in the preparation process of conductive pole pieces. The composite film of the present invention has a magnetic layer, and the magnetic adsorption force of the magnetic layer is used to peel the binder from the current collector, which has excellent peeling efficiency and is easy to sweep, and at the same time, it will not cause peeling failure or residual glue problems.
[0017] Furthermore, the present invention also provides a method for preparing a conductive electrode sheet using the composite film, which has improved production efficiency and enhanced product quality.
[0018] Solutions for solving problems
[0019] [1] A composite film comprising a magnetic layer and an adhesive layer formed on one surface of the magnetic layer; wherein:
[0020] At a distance of 1 cm from the magnetic layer, the magnetic adsorption force of the magnetic layer is greater than 0.5 MPa, and preferably greater than 0.7 MPa.
[0021] [2] A composite film according to [1] above, wherein the magnetic layer is a magnetic layer formed by printing, spraying or plating a magnetic material; or, the magnetic layer is a magnetic metal film or a ferrite ceramic film.
[0022] [3] The composite film according to [1] or [2] above, wherein the content of ferrite in the magnetic layer is greater than 50%; and / or
[0023] The thickness of the magnetic layer is 1 μm to 500 μm.
[0024] [4] A composite film according to any one of [1] to [3] above, wherein the adhesive layer is formed by coating or adhering an adhesive composition to the surface of the magnetic layer; preferably, the magnetic adsorption force of the magnetic layer is greater than the peeling stress of the adhesive layer at a temperature of 180°C.
[0025] [5] The composite film according to [4] above, wherein the adhesive layer is distributed continuously or at intervals;
[0026] Preferably, the adhesive layer has an adhesive strength of 0.02-0.5 MPa.
[0027] [6] A composite film according to any one of [1] to [5] above, wherein there is a polymer layer or two or more polymer layers between the adhesive layer and the magnetic layer; preferably, the gel fraction of the polymer layer is 10% to 90%.
[0028] [7] The composite film according to [6] above, wherein the maximum shrinkage stress value of the polymer layer in the MD direction occurs in the temperature range of 60 to 300°C; and the maximum shrinkage stress value in the MD direction is 0.2 to 10 MPa.
[0029] [8] A composite film according to any one of [5] to [7] above, wherein the magnetic layer is bonded to the polymer layer via an adhesive layer; or the magnetic layer is formed on the surface of the polymer layer by printing, spraying or plating a magnetic material.
[0030] [9] A method for preparing a conductive electrode sheet, the method comprising:
[0031] a bonding step, using the composite film according to any one of [1] to [8] above to form a protective region on at least a portion of the current collector; and
[0032] The step of re-peeling is to use a magnetic substance to externally stimulate the composite film so as to re-peel it from the current collector.
[0033]
[10] A method for preparing an electrode sheet for a lithium-ion battery, characterized in that the method comprises the method described in [9] above.
[0034] Effects of the Invention
[0035] The composite film of the present invention has a magnetic layer, and the magnetic adsorption force of the magnetic layer is used to peel the binder from the current collector, which has excellent peeling efficiency and is easy to clean without causing peeling failure or residual adhesive problems.
[0036] Furthermore, the preparation method of the conductive electrode sheet of the present invention is simple and easy, the raw materials are easy to obtain, and it is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 A composite film according to a first embodiment of the present invention is shown;
[0038] Figure 2 A composite film according to a second embodiment of the present invention is shown;
[0039] Figure 3 A composite film according to a third embodiment of the present invention is shown;
[0040] Figure 4 A composite film according to a fourth embodiment of the present invention is shown;
[0041] Figure 5 A composite film according to a fifth embodiment of the present invention is shown;
[0042] Figure 6 A composite film according to a sixth embodiment of the present invention is shown;
[0043] Figure 7 The first method of using the composite film in the prior art is shown;
[0044] Figure 8 A second method of using the composite film in the prior art is shown;
[0045] Fig. 9 A third use of the composite film in the prior art is shown;
[0046] Fig.10 The first use mode of the composite film of the present invention is shown;
[0047] Fig.11 A second way of using the composite film of the present invention is shown. DETAILED DESCRIPTION
[0048] The following is a detailed description of the present invention. The technical features described below are described based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples.
[0049] It should be noted that:
[0050] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values A and B.
[0051] In the present specification, a numerical range expressed using "above" or "below" means a numerical range including the number.
[0052] In this specification, the word "may" means both performing a certain process and not performing a certain process.
[0053] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.
[0054] In this specification, the "room temperature" used means an indoor ambient temperature of "20°C".
[0055] In this specification, the unit names used are all international standard unit names, and unless otherwise stated, the "%" used indicates weight or mass percentage.
[0056] In the present specification, the use of "substantially" means that the standard deviation from a theoretical model or theoretical data is within a range of 5%, preferably 3%, and more preferably 1%.
[0057] In this specification, the “MD” direction is used to indicate a machine direction or a flow line direction, and the “TD” direction is used to indicate a direction perpendicular to the machine direction or the flow line direction.
[0058] In this specification, the "surface" used refers to the main surface of the polymer layer, that is, the two opposite surfaces with the largest area.
[0059] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.
[0060] <First aspect>
[0061] A first aspect of the present invention provides a composite film, comprising a magnetic layer and an adhesive layer formed on one surface of the magnetic layer; wherein:
[0062] At a distance of 1 cm from the magnetic layer, the magnetic adsorption force of the magnetic layer is greater than 0.5 MPa, and preferably greater than 0.7 MPa.
[0063] (Magnetic layer)
[0064] The magnetic layer of the present invention is derived from a magnetic material. The present invention does not specifically limit the magnetic material, as long as it can satisfy the requirement that the magnetic adsorption force of the magnetic layer is greater than 0.5Mpa, preferably greater than 0.7Mpa, for example, 0.5Mpa to 2Mpa, at a distance of 1cm from the magnetic layer.
[0065] Specifically, the magnetic material of the present invention may include one or more of cobalt (Co), iron (Fe) and nickel (Ni). The magnetic material may also include at least one non-magnetic material, such as boron (B), zinc (Zn), aluminum (Al), titanium (Ti), ruthenium (Ru), tantalum (Ta), silicon (Si), silver (Ag), gold (Au), copper (Cu), carbon (C) and nitrogen (N). For example, the magnetic material may include one or more of FePt, FePd, CoCr, CoCu, CoPt, CoTb, CoCrPt, CoFeTb, CoFeGd, CoNi and CoNiFe.
[0066] The magnetic material can be prepared by printing or spraying to form a magnetic layer, or by plating.
[0067] Furthermore, in the present invention, the magnetic layer is a magnetic metal film or a ferrite ceramic film; or, the magnetic layer can be formed by printing, spraying or plating a magnetic material. The magnetic layer of the present invention can have a magnetic function and can be adsorbed by a magnet to achieve peeling. And, if Fig.10 and 11 As shown, the magnetic material can be easily absorbed without peeling failure or residual glue problem. No residue will be generated after absorption and it is easy to clean without the need for a scraper.
[0068] Specifically, the present invention can directly use magnetic paint for printing. For example, using MagnaMagic's colorable Chalkboard Pain coating. The specific operation method may be to print the above magnetic coating on the surface of the polymer layer by gravure printing or screen printing process to form a continuous and dense magnetic layer on the surface of the adhesive layer or the polymer layer.
[0069] In addition, when a polymer layer is used, a plating method can be used to form a magnetic layer. Specifically, the plating method refers to depositing a magnetic material on the surface of the polymer layer to form a magnetic layer. Taking the magnetic material iron or iron alloy as an example: Commonly used process technologies include the following:
[0070] 1. Chemical iron plating: Coat the iron-containing solvent on the surface of the polymer layer, and deposit the iron layer on the polymer layer through chemical reaction.
[0071] 2. Physical iron plating: depositing pure iron or iron alloy layer on the surface of polymer layer by vacuum evaporation or sputtering.
[0072] 3. Electrochemical iron plating: Iron is deposited on the surface of the polymer layer by electrolysis. The polymer layer serves as the cathode, and the iron in the iron salt solution serves as the anode. The current is used to dissolve the iron from the anode and deposit it on the surface of the polymer layer.
[0073] Specifically, in the present invention, the content of ferrite in the magnetic layer is greater than 50%, for example: 60-100%; and / or the thickness of the magnetic layer is 1μm-500μm. Preferably, when magnetic paint is used for spraying, the thickness of the magnetic layer can be 1-10μm, and most preferably 2-5μm; when the plating method is used, the thickness of the magnetic layer can be 1-10μm, and most preferably 2-5μm.
[0074] (Adhesive layer)
[0075] There is no particular limitation on the type of adhesive that can be used in the present invention, and commonly used pressure-sensitive adhesives and hot-melt adhesives in the art can be used.
[0076] The pressure-sensitive adhesive may be selected from cross-linkable adhesives such as acrylic pressure-sensitive adhesives, silicone pressure-sensitive adhesives, polyester pressure-sensitive adhesives, polyurethane pressure-sensitive adhesives, polyamide pressure-sensitive adhesives, and rubber pressure-sensitive adhesives. Among them, acrylic pressure-sensitive adhesives, silicone pressure-sensitive adhesives, and rubber pressure-sensitive adhesives are preferably used in the present invention.
[0077] For specific examples of acrylic pressure-sensitive adhesives, homopolymers or copolymers of alkyl (meth)acrylates may be included, and the alkyl (meth)acrylates may be, for example, C1-C30 alkyl (meth)acrylates, preferably C1-C20 alkyl esters. Specifically, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isopropyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and octyl (meth)acrylate may be included. In addition, other unsaturated monomers that can be copolymerized with the above-mentioned alkyl (meth)acrylates may be another monomer or olefin monomer containing a carboxyl group or anhydride group. Specifically, it can be (meth)acrylic acid, itaconic acid, fumaric acid or maleic anhydride; hydroxyl-containing monomers, such as 2-hydroxyethyl (meth)acrylate; amino-containing monomers, such as morpholyl (meth)acrylate; amide-containing monomers, such as (meth)acrylamide; cyano-containing monomers, such as (meth)acrylonitrile; or (meth)acrylates containing alicyclic hydrocarbon groups, such as isobornyl (meth)acrylate; ethylene, propylene, butadiene, styrene, olefins with alicyclic structures, and other C1 to C20 olefins.
[0078] As the acrylic pressure-sensitive adhesive, particularly preferred are copolymers of one or more C1-C12 alkyl (meth)acrylates such as ethyl acrylate, butyl acrylate or 2-ethylhexyl acrylate, and at least one copolymerizable monomer selected from a hydroxyl group-containing monomer such as 2-hydroxyethyl acrylate and a carboxyl group-containing or anhydride group-containing monomer such as acrylic acid, or copolymers of one or more C1-C12 alkyl (meth)acrylates, alicyclic hydrocarbon group-containing (meth)acrylates, and at least one copolymerizable monomer selected from a hydroxyl group-containing monomer and a carboxyl group-containing or anhydride group-containing monomer.
[0079] For acrylic pressure-sensitive adhesives, they are generally prepared, for example, by photopolymerizing (for example, with ultraviolet light) the above-mentioned monomer components (and a polymerization initiator) in the presence of a solvent, and are liquid prepolymers with high viscosity. A cross-linked pressure-sensitive adhesive composition can be obtained by adding a cross-linking agent to the above-mentioned prepolymer. The cross-linking agent can be added when preparing the prepolymer. A cross-linked acrylic pressure-sensitive adhesive composition can also be obtained by adding a cross-linking agent and a solvent (not necessary in the case of using an acrylic polymer solution) to an acrylic polymer obtained by polymerizing the above-mentioned monomer components or a solution thereof.
[0080] The crosslinking agent is not particularly limited and can be selected from isocyanate type crosslinking agents, melamine type crosslinking agents, epoxy type crosslinking agents, acrylate type crosslinking agents (multifunctional acrylates), (meth)acrylates containing isocyanate groups, etc. Examples of acrylate type crosslinking agents include hexanediol diacrylate, 1,4-butylene glycol diacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate. Examples of (meth)acrylates having isocyanate groups include 2-isocyanate ethyl acrylate and 2-isocyanate ethyl methacrylate. Among them, ultraviolet (UV) reactive crosslinking agents such as acrylate type crosslinking agents (multifunctional acrylates) or (meth)acrylates having isocyanate groups are preferred.
[0081] The polysiloxane-based pressure-sensitive adhesive is not particularly limited and may be a polymer obtained by hydrolysis and condensation of an organic silane monomer, and the polymer may have an unsaturated active group.
[0082] For the rubber-based pressure-sensitive adhesive, a natural rubber component or an artificial synthetic rubber component, or a mixture thereof can be used.
[0083] For acrylic pressure-sensitive adhesives, polysiloxane pressure-sensitive adhesives, and natural or synthetic rubber pressure-sensitive adhesives, in some preferred embodiments, the weight average molecular weight of the soluble portion may be 30×10 4 ~14×10 5 .
[0084] Furthermore, from the perspective of balancing the adhesive properties (adhesive force, viscosity, durability, and retention properties), the gel fraction may be 20 to 95%. If it is less than 20%, insufficient cohesion may occur, resulting in cohesive failure during peeling, and part of the adhesive may remain on the surface of the adhered body, resulting in reduced processability. On the other hand, if it exceeds 95%, insufficient viscosity may occur, failing to meet the bonding requirements, resulting in reduced bonding reliability.
[0085] As the hot melt adhesive that can be used in the present invention, typically, various thermoplastic resins can be used.
[0086] Examples of these thermoplastic resins include homopolymers of olefins such as ethylene, propylene, butene, hexene, and cycloolefins, copolymers of two or more olefins, copolymers of one or more olefins and one or more polymerizable monomers (other than olefins) copolymerizable with the olefins, and other thermoplastic resins. These thermoplastic resins are generally required to produce initial adhesion within a temperature range of 40°C to 100°C, preferably within a temperature range of 40°C to 60°C.
[0087] Examples of the thermoplastic resin include acrylic resins such as ethylene-ethyl acrylate copolymers, butadiene-styrene copolymers, acrylonitrile-styrene copolymers, polystyrene, styrene-butadiene-styrene copolymers, styrene-isoprene-styrene copolymers, styrene-acrylic acid copolymers and other styrene resins.
[0088] In addition, other thermoplastic resins that can also be used include: vinyl chloride resins, polyvinyl fluoride, polyvinylidene fluoride and other vinyl fluoride resins, 6-nylon, 6,6-nylon, 12-nylon and other amide resins, polyethylene terephthalate, polybutylene terephthalate and other saturated ester resins, polycarbonate, polyphenylene ether, polyphenylene sulfide, thermoplastic silicone resin, thermoplastic polyurethane resin, polyetheretherketone, polyetherimide, thermoplastic epoxy resin, phenolic resin and their modified products, etc.
[0089] As the thermoplastic resin, two or more different thermoplastic resins may be mixed and used.
[0090] Among the above-mentioned thermoplastic resins, from the perspective of forming an adhesive layer by coextrusion as described below, polyolefin resins or copolymers of one or more olefins and one or more polymerizable monomers (other than olefins) copolymerizable with the olefins can be preferably used.
[0091] The olefin constituting the polyolefin resin is preferably a homopolymer or copolymer of ethylene, propylene, α-olefins having 4 to 20 carbon atoms, cycloolefins, aromatic vinyl compounds, alicyclic vinyl compounds such as vinylcyclohexane, and polyene compounds.
[0092] Specific examples of the α-olefins having 4 to 20 carbon atoms include 1-butene, 2-methyl-1-propylene, 1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, 1-hexene, 2-ethyl-1-butene, 2,3-dimethyl-1-butene, 3,3-dimethyl-1-butene, 2-methyl-1-pentene, 2,3-dimethyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-heptene, 2-methyl-1-hexene, 2,3-dimethyl-1-pentene, 2-ethyl-1- Pentene, 2-methyl-3-ethylene-1-butene, 1-octene, 2-ethyl-1-hexene, 3,3-dimethyl-1-hexene, 2-propyl-1-heptene, 2-methyl-3-ethyl-1-heptene, 2,3,4-trimethyl-1-pentene, 2-propyl-1-pentene, 2,3-diethyl-1-butene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, etc.
[0093] Examples of the cycloolefins include bicyclo[2.2.1]hept-2-ene, which is generally referred to as norbornene, and norbornene derivatives into which an alkyl group having 1 to 4 carbon atoms, such as methyl, ethyl or butyl, is introduced, such as 6-alkylbicyclo[2.2.1]hept-2-ene, 5,6-dialkylbicyclo[2.2.1]hept-2-ene, 1-alkylbicyclo[2.2.1]hept-2-ene and 7-alkylbicyclo[2.2.1]hept-2-ene.
[0094] Examples of the aromatic vinyl compound include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, o-ethylstyrene, and p-ethylstyrene.
[0095] Examples of the above-mentioned "one or more olefins and one or more polymerizable monomers (other than olefins) copolymerizable with the olefins" include polar vinyl compounds and derivatives of aromatic vinyl compounds. The derivatives are compounds in which other substituents are bonded to aromatic vinyl, and examples thereof include hydroxystyrene, tert-butoxystyrene, vinyl benzoic acid, vinyl benzyl acetate, o-chlorostyrene, p-chlorostyrene and other substituted styrenes in which hydroxyl groups, alkoxy groups, carboxyl groups, acyloxy groups and halogen groups are introduced into the benzene ring of styrene, and vinyl biphenyl compounds such as 4-hydroxy-4'-vinyl biphenyl. Examples of polar vinyl compounds include acrylic compounds such as methyl acrylate, methyl methacrylate and ethyl acrylate, as well as vinyl acetate and vinyl chloride.
[0096] In some preferred embodiments of the present invention, ethylene vinyl acetate (EVA) is preferably used as the thermoplastic resin of the present invention in consideration of convenience of use and recycling and solvent resistance.
[0097] In addition, for the pressure-sensitive adhesive of the present invention, in addition to the above-mentioned main polymer components, other components or auxiliary agents may be used as required, for example, cross-linking catalysts, tackifying resins (such as rosin derivative resins, polyterpene resins, petroleum resins, or oil-soluble phenolic resins), tackifiers, plasticizers, fillers, inorganic fillers, organic fillers, coupling agents, antioxidants, antistatic agents, foaming agents, and antioxidants.
[0098] It should be noted that, for the composition of the adhesive of the present invention, the foaming component is an optional but not absolutely necessary component. In other words, the technical solution of the present invention does not require the use of foaming components in principle, which is a feature different from the previous use of foaming components to assist re-peeling.
[0099] There is no particular limitation on the method for forming the adhesive layer of the present invention, and the adhesive layer may be formed using a conventional method in the art.
[0100] In the present invention, the adhesive layer is formed by coating or sticking the adhesive composition on the surface of the magnetic layer. In some specific embodiments, the adhesive composition can be formed into a coating liquid or a coating slurry with the aid of a solvent, and then formed on at least one surface of the magnetic layer by spraying or spin coating. Preferably, the magnetic adsorption force of the magnetic layer is greater than the 180° peeling stress of the adhesive layer.
[0101] In some preferred embodiments, the adhesive may be bonded to at least one surface of the magnetic layer in a solid or semi-solid form.
[0102] For example, an adhesive layer can be formed by using an adhesive in the form of a "double-sided tape". For such a double-sided tape, a preferred embodiment can be a laminate of two layers of pressure-sensitive adhesive. Among them, one layer of pressure-sensitive adhesive layer can be mainly composed of an acrylic adhesive, and the other layer of pressure-sensitive adhesive layer can be mainly composed of a polysiloxane-based pressure-sensitive adhesive. When used, the acrylic pressure-sensitive adhesive side of the double-sided tape is attached to one surface of the magnetic layer of the present invention, and the polysiloxane-based pressure-sensitive adhesive faces the surface to be bonded.
[0103] It should be noted that when the adhesive layer is used in the form of the above-mentioned “double-sided tape”, it can also be formed using only one type of pressure-sensitive adhesive.
[0104] In addition, the above-mentioned "double-sided adhesive tape" may or may not have a support layer or a protective layer before use. The typical support layer can be a polyester material such as PET, or a fiber such as cotton paper or non-woven fabric. Preferably, the melting point of the support layer is above 120°C. Generally, the use of the support layer is conducive to the preservation of the adhesive layer and is convenient for use. There is no special restriction on the protective layer, and a polymer layer, paper or non-woven fabric commonly used in the art can be used.
[0105] In some other preferred embodiments, the adhesive (especially the hot melt adhesive) can be co-extruded when the original film is formed (or stretched at the same time) by a co-extrusion method. Figure 1 The layered structure shown has two magnetic layers of polymer layers and an adhesive layer formed by hot melt adhesive.
[0106] The thickness of the adhesive layer of the present invention is not particularly limited. From the viewpoint of facilitating re-peeling, the average thickness of the adhesive layer may be 5 to 500 μm, preferably 6 to 50 μm.
[0107] Further, in the present invention, if Figure 1 and Figure 2 As shown, the adhesive layer can be distributed continuously or at intervals. In order to reduce the peeling stress and not affect the bonding and fixation of the adhesive layer, it is preferred that the adhesive layer is distributed at intervals. When the adhesive layer is formed in an at-interval distribution manner, the risk of residual adhesive on the current collector is reduced by reducing the bonding area of the adhesive layer.
[0108] Furthermore, in the present invention, the bonding strength of the adhesive layer is 0.02 to 0.5 MPa, and preferably the bonding strength of the adhesive layer is 0.05 to 0.3 MPa.
[0109] (Polymer layer)
[0110] The polymer layer may be any film layer that is shrinkable or expandable at least in a uniaxial direction. When the polymer layer is a shrinkable film layer, it may be composed of any film such as a heat-shrinkable film, a film that shows light-induced shrinkage, a film that shrinks due to electrical stimulation, etc. From the viewpoint of operating efficiency, the polymer layer is preferably composed of a heat-shrinkable film. The polymer layer may have shrinkage only in a uniaxial direction, or may have a main shrinkage in a certain direction (uniaxial direction) and a secondary shrinkage in a direction different from the direction (e.g., a direction orthogonal to the direction). In addition, the polymer layer may be a single layer or a multilayer composed of two or more layers.
[0111] The polymer layer of the present invention is derived from a polymer. The polymer can be mainly formed of various organic polymer materials. The types of the organic polymer materials that can be used in the present invention can be selected from one or more mixed materials of polyolefins, modified polyolefins, polyesters, polyimides, polyamides, polyaromatic hydrocarbons or polyurethanes, etc., from the perspective of being beneficial to the thermal shrinkage of the composite film and adhesion to the adhesive layer.
[0112] In some specific embodiments, the polyolefin or modified polyolefin may be selected from homopolymers and copolymers of ethylene, propylene, vinyl chloride, vinyl dichloride, vinyl fluoride, styrene, halogenated styrene, olefins with alicyclic structures (norbornene monomers) and their halides. In other specific embodiments, other comonomers that may be used in the above copolymers are not particularly limited in principle, for example, they may be unsaturated monomers formed by acrylic acid esters and esters of vinyl alcohol.
[0113] As for the polyester, it can be selected from polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene terephthalate-1,4-cyclohexanedimethanol (PET-G) or a mixture thereof in any ratio. In some preferred embodiments, a polyester mixture formed by them is preferably used, and, based on the total mass of the two, the content of PET is preferably 50% by mass or more.
[0114] For polyamide and polyimide, aromatic or alicyclic di / polyacids and di / polyamines can be used and obtained only by condensation reaction. In addition, in order to further improve the transparency of these materials (favorable for radiation treatment, etc.), alicyclic structures and / or fluorine-containing groups can be introduced into their structures.
[0115] As the polyurethane, polyester type as well as polyether type polyurethane materials can be used.
[0116] As the polyaromatic hydrocarbon, materials such as polystyrene may be used.
[0117] The high molecular weight polymer can be cross-linked by chemical or radiation processes. The cross-linking process includes but is not limited to chemical cross-linking (peroxide cross-linking), radiation cross-linking, silane cross-linking and ultraviolet light cross-linking. After cross-linking, the organic polymer layer needs to reach a certain degree of cross-linking (gel rate), wherein the gel rate after cross-linking is 10 to 90%, preferably 30 to 70%.
[0118] Furthermore, in order to form a high molecular polymer into a film, in addition to the base resin of the above-mentioned organic polymer material, additional components such as inorganic / metal fillers, leveling agents, antistatic agents, flame retardants, anti-aging agents, etc. may be used according to any other needs.
[0119] The thickness of the polymer layer can be 5 to 300 μm, preferably 10 to 100 μm. When the thickness of the polymer layer is too large, the rigidity increases and it will not be deformed into a cylindrical shape, or separation between the polymer layer and the rigid layer may occur. When the thickness of the polymer layer is too small, the shrinkage stress is small and it will not roll up automatically, or wrinkles are easily generated when it is bonded to the adjacent layer during processing. In order to improve the adhesion and retention of the surface of the polymer layer with the adjacent layer, the polymer layer can be subjected to conventional surface treatment, such as chemical or physical treatment such as chromic acid treatment, ozone exposure, flame exposure, high voltage electric shock exposure or ionizing radiation treatment, coating treatment with a primer (such as an adhesive substance, etc.), etc.
[0120] The formation of the polymer layer can be achieved by subjecting the original resin film formed of the polymer to stress treatment. The stress treatment of the present invention can generally include calendaring treatment, stretching treatment or a combination thereof.
[0121] There is no particular limitation on the calendering treatment, and the original resin film can be mechanically calendered in one direction or multiple (orthogonal) directions at a temperature not higher than 130° C., preferably in the range of 70 to 120° C., and more preferably in the range of 90 to 120° C. There is no particular limitation on the specific calendering method, which mainly depends on the structure of the calender.
[0122] Typically, the original resin film can be placed between two opposing rollers in a calender for calendering. The degree of calendering can be adjusted by adjusting the distance between the two rollers and the running speed of the two rollers to ensure the thickness uniformity of the calendered film. In other specific embodiments, a certain degree of stretching can be assisted while calendering.
[0123] Further, for the elongation of the polymer layer after calendering, in some specific embodiments of the present invention, the elongation in the MD and TD directions can be 30% to 400%, preferably, 50% to 300%, and more preferably 60% to 200%. By controlling the elongation in the MD and / or TD directions, the shrinkage stress of the polymer layer obtained by calendering in the corresponding direction can be regulated. In some preferred embodiments, the shrinkage stress at 70°C in the MD and TD directions can be adjusted to 0.5 to 30 MPa, preferably 1 to 15 MPa, by adjusting the elongation in the MD and TD directions.
[0124] The number of times of calendering treatment is not particularly limited, and unidirectional or multidirectional calendering treatment may be performed once or a plurality of times.
[0125] There are no special restrictions on the stretching treatment. In order to ensure the stretching efficiency and uniformity, it is usually necessary to carry out the stretching treatment at a temperature of 90 to 180°C. In some specific embodiments, the elongation in the MD and / or TD directions is adjusted by uniaxial or biaxial stretching to adjust the shrinkage stress of the stretched polymer layer in the corresponding direction. It should be noted that for the stretching treatment, the temperature can be raised again after the original resin film is obtained, and it can also be carried out by hot stretching while preparing the original film by, for example, extrusion. In some specific embodiments of the present invention, in the stretching treatment, the elongation in the MD and TD directions can be 30% to 700%, respectively, preferably, 50 to 400%, and more preferably 60% to 300%, respectively. Furthermore, in a preferred embodiment, the shrinkage stress at 70°C in the MD and TD directions of the polymer layer can be adjusted to 0.2 to 20 MPa, preferably in the range of 0.5 to 10 MPa. If the shrinkage stress is too low, it will be difficult to re-peel off the adhesive tape due to wrinkles or curling caused by shrinkage; if the shrinkage stress is too large, on the one hand, the processing difficulty will increase from the processing technology of the polymer layer, and on the other hand, excessive shrinkage stress will also cause problems such as splashing of the adhesive tape or residual glue during the re-peeling process of the adhesive tape.
[0126] The number of stretching treatments is not particularly limited, and unidirectional or multidirectional stretching treatments may be performed once or multiple times.
[0127] Furthermore, from the viewpoint of increasing the internal stress of the polymer layer to improve the uniformity of the thickness of the polymer layer, it is preferred to subject the original resin film to stress treatment using at least a calendaring treatment step.
[0128] Furthermore, the high molecular polymer layer obtained through the above stress treatment can be quickly cooled to room temperature to fix the internal stress so as to slow down the stress relaxation existing during storage before use.
[0129] In the present invention, a high molecular polymer layer that meets the requirements of the present invention can be obtained by stress treatment and control or adjustment of elongation in the stress processing direction (such as MD and TD directions).
[0130] In some specific embodiments, the maximum shrinkage stress value of the high molecular polymer layer in the MD direction of the present invention appears above 60°C, preferably appears in the range of 60-300°C, and more preferably appears in the range of 80-160°C, for example, the peak value of shrinkage stress appears at 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C or 160°C. If the maximum stress value in the MD direction appears in the range below 70°C, it is difficult to complete the re-peeling of the adhesive tape using the high molecular polymer layer in the subsequent re-peeling process. This is mainly because the high molecular polymer layer shrinks prematurely during the heating process of the re-peeling process, but because the adhesive layer still has a high peeling stress at this time, it is easy to cause re-peeling failure.
[0131] Furthermore, the maximum shrinkage stress value that can be achieved by the high molecular polymer layer in the temperature range of 70°C or above is 0.2 to 10 MPa, preferably 0.5 to 9 MPa, more preferably 0.8 to 8.5 MPa, and more preferably 1 to 8 MPa. If the maximum shrinkage stress is lower than 0.3 MPa, it is difficult to re-peel off the adhesive tape through wrinkles or curling caused by shrinkage; if the maximum shrinkage stress is too large, on the one hand, the processing difficulty will increase from the processing technology of the resin film, and on the other hand, the excessive shrinkage stress will also cause splashing in the heating furnace to contaminate the undried current collector.
[0132] In some other specific embodiments, there is no particular limitation on the total shrinkage (stable shrinkage) of the polymer layer of the present invention at a temperature above 70°C. In a preferred embodiment, the total shrinkage in the MD direction may be 20% or more, preferably 20% to 80%. If the total shrinkage is too low, even if the shrinkage stress meets the requirements, there is a concern that the re-peeling efficiency of the adhesive tape may be reduced.
[0133] Furthermore, in the case of a multi-layer polymer layer, there may be 2 to 5 layers of polymer layers, preferably 2 or 3 layers of polymer layers. For a multi-layer polymer layer, these film layers may be the same film layer or different film layers. In some preferred embodiments, among these film layers, at least one layer of polymer layer has a shrinkage stress different from that of other layers of polymer layers.
[0134] Due to the difference in shrinkage stress, when the polymer layer generates deformation stress at high temperature, the polymer layer curls toward the layer with higher shrinkage stress, thereby controlling the product to curl in a directional manner toward the magnetic object, making the product easier to be absorbed by the magnetic object. At the same time, the curling of the polymer layer can also reduce the bonding area of the adhesive, making it easier for the product to separate from the current collector surface.
[0135] From the perspective of the morphology formed after the polymer layer shrinks, which is conducive to the re-peeling of the adhesive tape, in a preferred embodiment of the present invention, the polymer layer can be a laminated film formed by two polymer layers. More preferably, at the same temperature, the shrinkage stress of one polymer layer in the double-layer film is greater than that of the other polymer layer, so as to facilitate the formation of a curled structure after shrinkage.
[0136] Furthermore, in order for the polymer layer of the present invention to have the defined shrinkage stress and the required mechanical properties, it is necessary and advantageous for the polymer layer to have a certain total gel fraction. The so-called total gel fraction is the gel fraction calculated based on the entire polymer layer. If the polymer layer is a multi-layer resin film, it is calculated based on the entirety of the multi-layer polymer layer.
[0137] In some specific embodiments of the present invention, the gel fraction of the polymer layer is 10% or more, preferably 20% or more. If the gel fraction is too low, it is difficult to obtain the shrinkage stress defined in the present invention and the mechanical stress of the resin film is too low (easy to tear). There is no particular upper limit on the gel fraction, but it can usually be controlled below 90%, preferably below 80%. If the gel fraction is too high, there is a concern that it may have an adverse effect on the processability of the polymer layer. To obtain the above-mentioned gel fraction, the organic polymer material can usually be cross-linked by chemical or radiation processes. The cross-linking process includes but is not limited to chemical cross-linking (peroxide cross-linking), radiation cross-linking, silane cross-linking, and ultraviolet light cross-linking.
[0138] The overall average thickness of the polymer layer of the present invention is not particularly limited, but from the perspective of convenient re-peeling, it can be 5 to 1000 μm, preferably 8 to 500 μm, more preferably 10 to 300 μm, and further preferably 15 to 100 μm. If the average thickness is too low, there are concerns about insufficient mechanical properties and uneven distribution of the polymer layer; if the average thickness is too high, there are concerns about insufficient shrinkage and curling due to excessive rigidity, and there are also concerns about hindering irradiation efficiency when the polymer layer is used as an adhesive tape later.
[0139] <Second Aspect>
[0140] In a second aspect of the present invention, there is provided a method for preparing an electronic device component, especially an electrode component, by using the composite film of the first aspect.
[0141] In some specific embodiments of the present invention, the present invention provides a method for preparing a conductive electrode sheet for a lithium ion secondary battery.
[0142] Specifically, the conductive electrode sheet generally includes a current collector, an active material composition formed on the surface of the current collector, and an electrode tab electrically connected to the current collector.
[0143] There is no particular limitation on the current collector, and a single metal or its alloy material can be used. In some preferred embodiments, metal copper, aluminum or their alloys can be used, and more preferably, aluminum or aluminum alloys can be used.
[0144] There is no particular restriction on the composition of the active material composition, which may include an electrode active material that can accommodate and precipitate lithium ions, an adhesive component, and other optional conductive components. The electrode active material may be a positive electrode active material, such as a metal oxide, preferably containing one or more metal elements of Li, Co, Ni, Mn, rare earth metal elements, etc.; or a negative electrode active material, such as a carbon-based material (graphite, etc.) or a silicon-based material (silicon dioxide, etc.).
[0145] In some specific embodiments of the present invention, the method for preparing the conductive electrode sheet may include a bonding step and a peeling step.
[0146] The bonding step includes: forming a protective region on at least a portion of the current collector, and then coating the surface of the current collector with a composition containing an active substance;
[0147] The re-peeling step includes: using a magnetic substance to externally stimulate the composite film so as to re-peel it from the current collector.
[0148] Furthermore, the step of forming the protection area may be a pre-designed area reserved for the connection of the tabs, wherein the area is protected by protective measures to prevent the active material composition from entering.
[0149] Regarding the specific method of forming the protective region, when no high molecular polymer layer is included, the present invention can adopt the following method:
[0150] In the first method, the adhesive composition of the present invention can be sprayed continuously or intermittently on the protective area in advance, or one side of the adhesive as a double-sided tape can be continuously or intermittently adhered to the protective area to form an adhesive layer, and then the magnetic material is sprayed or attached to the adhesive layer to form a composite film.
[0151] In the second mode, the adhesive composition of the present invention is used to form an adhesive layer in the protected area, and then the magnetic layer is bonded to the surface of the adhesive layer. Furthermore, there is no particular limitation on the method for forming the adhesive layer. The adhesive composition can be used to continuously or intermittently coat (spray or spin coat) the protective area, or one side of the adhesive as a double-sided tape can be continuously or intermittently bonded to the protective area, and then the magnetic layer is bonded to the surface of the adhesive layer. The magnetic layer should be aligned with the adhesive layer to avoid poor processing of the protective area when the active material is subsequently coated.
[0152] In the third mode, the adhesive composition of the present invention and the magnetic layer are formed into a composite film in advance, and then the optionally cut composite film is attached to the protective area. There is no particular limitation on the method of forming the composite film, and the adhesive composition can be continuously or intermittently coated on the magnetic layer, or the composite film can be directly obtained by coextrusion (for example, hot melt adhesive is continuously or intermittently extruded on the magnetic layer) to obtain the composite film.
[0153] Further, the present invention preferably uses interval coating to form a composite film, specifically as Figure 2 As shown, the composite film can be partially adhesive and partially adhesive-free, and the adhesive coating area on the metal foil can be controlled by controlling the ratio of the closed and glue-discharging areas of the glue coating die, thereby achieving control of the bonding strength. The present invention does not specifically limit the method of intermittent coating, and the adhesive can be sprayed or the glue discharging die can be partially closed and partially glue-discharging by using a mold to achieve intermittent coating of the adhesive.
[0154] Regarding the specific method of forming the protective region, when a high molecular polymer layer is included, the present invention may adopt the following method:
[0155] In the first mode, the adhesive composition of the present invention, the polymer layer and the magnetic layer are formed into a composite film, and then the optionally cut composite film is attached to the protective area. There is no particular limitation on the method of forming the composite film, and the magnetic layer can be sprayed, printed or plated (such as chemical plating, electroplating, physical plating, electrochemical plating, etc.) on the surface of the polymer layer, and then the polymer layer is bonded to the adhesive layer.
[0156] In the second method, after the magnetic layer is sprayed, printed or plated (such as chemical plating, electroplating, physical plating, electrochemical plating, etc.) on the polymer layer, the adhesive composition of the present invention is continuously coated or intermittently coated (sprayed or spin coated) on the polymer layer to form a composite film. One side of the adhesive as a double-sided tape can also be continuously or intermittently adhered to the polymer layer to form a composite film, which is then applied to the protective area.
[0157] In the third method, the adhesive composition of the present invention, the polymer layer and the magnetic layer are formed into a composite film in advance, and then the optionally cut composite film is adhered to the protective area. There is no particular limitation on the method of forming the composite film. The magnetic layer can be coated on or adhered to the surface of the polymer layer, and the adhesive layer can be adhered to the surface of the polymer layer. The present invention does not particularly limit the order of coating or pasting. The magnetic layer can be coated or pasted first, or the adhesive layer can be adhered to the surface of the polymer layer first. For the adhesive layer, it can be coated continuously or coated at intervals. Preferably, the composite film is formed by using interval coating. Specifically, Figure 4 and Figure 6 As shown, the composite film can be partially adhesive and partially adhesive-free, and the adhesive coating area on the metal foil can be controlled by controlling the ratio of die closure and glue discharge area, thereby achieving control of the bonding strength. The present invention does not specifically limit the method of intermittent coating, and the adhesive can be sprayed or the glue discharge die can be partially closed and partially glued by a mold to achieve intermittent coating of the adhesive.
[0158] In addition, the magnetic layer and the polymer can also be attached by using an adhesive layer. However, it should be noted that in order to ensure a tighter connection between the magnetic layer and the polymer, it is recommended to continuously apply an adhesive composition or continuously apply double-sided tape.
[0159] In the above manner, a composite film is formed in the protection area. In some preferred embodiments, the total thickness of the composite film may be 10 to 1000 μm, preferably 10 to 700 μm, and more preferably 20 to 300 μm.
[0160] Furthermore, there is no particular limitation on the method of coating the active material composition on the current collector surface, and the composition may be coated in the form of a slurry. Furthermore, during coating, the composition may be coated on a portion or all of the surface of the composite film in the protected area.
[0161] In the step of peeling off the composite film in the protective region of the present invention, the active material composition slurry is dried, usually accompanied by external stimulation to the conductive electrode sheet, so that the composite film is peeled off.
[0162] By using a magnetic substance to externally stimulate the composite film, the composite film can be easily peeled off from the protection area to expose the protection area not coated with the active material composition. Furthermore, the tabs are connected to the protection area by bonding or welding.
[0163] The conductive electrode sheet obtained by the above method of the present invention can preferably be used for the positive electrode or negative electrode of a lithium ion secondary battery.
[0164] Specifically, the preparation method of the corresponding conductive electrode sheet includes the following steps:
[0165] 1) Fixing the magnetic layer at the position where the collector lug is pre-welded;
[0166] 2) coating the positive and negative electrode slurries on the current collectors respectively to obtain preforms;
[0167] 3) After the preform is dried, the magnetic layer is sucked away from the current collector by a magnetic body (such as a magnetic rod) installed after the drying tunnel, leaving a blank space for welding the pole lugs. After welding the pole lugs, the required conductive electrode sheet is obtained.
[0168] Compared with the existing disclosed technology, the present invention prepares a composite film with magnetic properties, and by placing a magnetic body (such as a magnetic rod) behind the drying tunnel, the magnetic layer is sucked away from the dried current collector to form a blank for welding the pole ear. The currently disclosed technology usually adjusts the curling height and bonding strength of the composite film for the removal of the composite film, and sweeps it by a scraper bar placed behind the drying tunnel, which has a considerable failure rate, causing the composite film to remain on the current collector or fall into the drying tunnel, causing contamination of the pole piece surface. The present invention can better solve the composite film removal failure rate, and at the same time, there is no need to strictly control the curling height of the composite film after shrinkage.
[0169] Example
[0170] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0171] Test Method
[0172] 1. Magnetic adsorption
[0173] The test sample was cut into 10mm×10mm pieces along the water flow direction (MD direction), and the sample was fixed on the lower chuck of the tensile testing machine with the flat surface facing upward. At the same time, a 10mm×10mm standard Ruthenium-Fe-B magnet (model ND35) was fixed on the upper chuck of the tensile testing machine. The upper chuck was slowly brought close to the lower chuck at a speed of 5mm / second until the distance between the ND35 Ruthenium-Fe-B magnet fixed on the upper chuck and the sample fixed on the lower chuck was 5mm, and the tensile testing machine displayed the force value (N).
[0174] The calculation formula of magnetic adsorption force is:
[0175] Magnetic adsorption force (MPa) = test value / (10mm×10mm)
[0176] 2. Shrinkage stress
[0177] The test sample was cut into strips of 25 mm × 200 mm along the water flow direction (MD direction), and then both ends of the sample were clamped on a constant temperature heated tensile testing machine with a distance of 150 mm between the upper and lower clamps.
[0178] The force (N) generated by the test sample at 100°C, the calculation formula for shrinkage stress is:
[0179] Shrinkage stress (MPa) = test value / (sample thickness in millimeters × 25 mm)
[0180] 3. 180° peel stress (hereinafter referred to as "peel stress"):
[0181] The test sample was cut into strips of 25 mm × 200 mm along the production line direction, and then the sample was laminated on an Al plate using a 2 kg roller for two reciprocating cycles, and the peel stress (N) was tested at a temperature of 100°C.
[0182] The calculation formula of sample peeling internal stress is:
[0183] Peel stress (MPa) = test value / (sample thickness in mm x 25 mm).
[0184] 4. Heat resistance evaluation:
[0185] The test samples were cut into strips of 25 mm × 200 mm along the production line direction, and then placed in a 140°C oven for 10 minutes. After cooling, the appearance changes were observed:
[0186] If it melts obviously, it has poor heat resistance and is marked with ×;
[0187] There is a slight tendency to melt, and it is marked with ○;
[0188] There is no melting and the ◎ logo is adopted.
[0189] 5. Gel rate test method:
[0190] The material was wrapped with a tetrafluoroethylene film and then placed in trichloroethylene at 70°C. After 24 hours, it was taken out and weighed before and after. The gel fraction was calculated using the formula:
[0191] Gel ratio = (weight of tetrafluoroethylene and film before immersion - weight of tetrafluoroethylene and film after immersion) / weight of tetrafluoroethylene and film before immersion × 100%.
[0192] 6. Whether curling occurs
[0193] The shrinkage stress is subtracted from the 1.3×180° peeling stress. If the value is greater than 0, curling will occur, otherwise, no curling will occur.
[0194] 7. Curl effect
[0195] The sample was cut into strips of 30 mm × 10 mm, with the long side in the shrinkage direction (MD direction), and then laminated on aluminum foil and heated at 100 ° C × 2 min. The height after curling was tested, and the curling score was calculated according to the following formula:
[0196] Curl score = (product height after curling - product width before curling) / product width before curling (10mm)
[0197] If the curl score is: 0.15-0.4 is ◎, the curl shape is good;
[0198] If the curl score is: 0.05~<0.15 is ○, the curl morphology is general;
[0199] If the curl score is: <0.05 is ×, the curl morphology is poor.
[0200] 8. Residual glue condition:
[0201] The test sample was cut into strips of 100 mm × 50 mm along the production line direction (MD direction), and then the sample was attached to an aluminum foil and placed in an oven at 140° C. for heating for 10 min. After being taken out and cooled, the tape was peeled off.
[0202] If offset printing appears on the aluminum foil surface, it means that the heat resistance is poor and is marked with ×;
[0203] If there is no mark on the surface, it is marked with ○.
[0204] 9. Adsorption effect
[0205] The sample was cut into 30 mm × 10 mm strips along the water flow direction, and then attached to aluminum foil and heated at 140 °C × 2 min. The heated aluminum foil and sample were then taken out.
[0206] Use ND35 neodymium iron boron magnet to absorb the sample at a height of 5 mm. If the sample is adsorbed by the magnet, it is represented by ○, otherwise it is represented by ×.
[0207] <Materials>
[0208] Magnetic layer: metal iron foil, metal iron-plated layer or iron-containing coating.
[0209] The metal iron-plated layer is deposited on the high molecular polymer layer or the adhesive layer by vacuum evaporation or sputtering.
[0210] The ferrous coating is a colorable ChalkboardPain coating. The specific operation method is to print the above magnetic coating on the polymer layer or adhesive layer through gravure printing or screen printing process to form a continuous and dense magnetic layer.
[0211] High molecular polymer layer: single-layer vinyl chloride film, PET-G film and double-layer LDPE / EVA film prepared by calendaring or stretching.
[0212] Adhesives: Commercially available acrylic pressure-sensitive adhesives and polyurethane hot-melt adhesives.
[0213] Examples 1 to 9 and Comparative Examples 1 to 4
[0214] The composite films were prepared according to the compositions in Table 1 and Table 3, and the tests in Table 2 and Table 4 were performed, wherein the high molecular polymer layer was a single-layer high molecular polymer layer prepared by a stretching method.
[0215] Table 1
[0216]
[0217] Table 2
[0218]
[0219] Table 3
[0220]
[0221] Table 4
[0222]
[0223] Industrial Applicability
[0224] The magnetic composite film and the method for preparing a conductive electrode sheet using the composite film of the present invention can be prepared or implemented industrially.
[0225] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.
[0226] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A composite film, characterized in that: The composite film includes a magnetic layer and an adhesive layer formed on one surface of the magnetic layer; wherein, At a distance of 1 cm from the magnetic layer, the magnetic adsorption force of the magnetic layer is greater than 0.5 MPa; The magnetic layer is a magnetic layer formed by printing, spraying or plating a magnetic material; or, the magnetic layer is a magnetic metal film or a ferrite ceramic film; In the magnetic layer, the content of ferrite is greater than 50%, and the thickness of the magnetic layer is 1 μm to 20 μm; the magnetic adsorption force of the magnetic layer is greater than the 180° peeling stress of the adhesive layer.
2. The composite film according to claim 1, characterized in that The magnetic adsorption force of the magnetic layer is greater than 0.7 MPa.
3. The composite film according to claim 1 or 2, characterized in that: The adhesive layer is formed by coating or sticking an adhesive composition on the surface of the magnetic layer.
4. The composite film according to claim 3, characterized in that: The adhesive layer is distributed continuously or at intervals.
5. The composite film according to claim 4, characterized in that The adhesive layer has an adhesive strength of 0.02-0.5 MPa.
6. The composite film according to claim 1 or 2, characterized in that: There is also a polymer layer or two or more polymer layers between the adhesive layer and the magnetic layer.
7. The composite film according to claim 6, characterized in that: The gel fraction of the high molecular polymer layer is 10% to 90%.
8. The composite film according to claim 6, characterized in that: The maximum shrinkage stress value of the high molecular polymer layer in the MD direction appears in the temperature range of 60 to 300° C.; and the maximum shrinkage stress value in the MD direction is 0.2 to 10 MPa.
9. The composite film according to claim 8, characterized in that The magnetic layer is bonded to the high molecular polymer layer via an adhesive layer; Alternatively, the magnetic layer is formed on the surface of the high molecular polymer layer by printing, spraying or plating a magnetic material.
10. A method for preparing a conductive electrode sheet, characterized in that: The method comprises: A bonding step, using the composite film according to any one of claims 1 to 9 to form a protective region on at least a portion of the current collector; and The step of re-peeling is to use a magnetic substance to externally stimulate the composite film so as to re-peel it from the current collector.
11. A method for preparing a pole piece for a lithium ion battery, characterized in that: The method comprises the method according to claim 10.