A process for preparing high-permeability aramid pulp / molecular sieve adsorption paper

Through the preparation process of highly air-permeable aramid pulp/molecular sieve adsorption paper, the deficiencies of existing air filter materials in adsorbing fine particles and toxic and harmful gases are solved, achieving high-efficiency, low-resistance air filtration effects, and expanding the material's use Application scenarios.

CN117127435BActive Publication Date: 2024-10-11SHAANXI KETIAN TESTING TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311140563.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-05
Publication Date
2024-10-11
Estimated Expiration
2043-09-05

AI Technical Summary

Technical Problem

Existing air filter materials are deficient in having high air permeability and adsorbing fine particles and toxic and harmful gases. They have high resistance, low dust holding capacity, and poor filtering effect on fine particles or toxic and harmful gases.

Method used

Using the preparation process of high air permeability aramid pulp/molecular sieve adsorption paper, the aramid pulp liquid is prepared through closed stirring of alkali solution, aramid fiber and dimethyl sulfoxide, and the molecular sieve is added under magnetic stirring conditions. Sub-homogenization and vacuum suction dehydration molding, combined with roll drying, form an adsorption paper with high air permeability and excellent adsorption performance.

Benefits of technology

It achieves high air permeability and efficient adsorption of toxic and harmful gases and fine particles, reduces air flow resistance, expands the application scope of the material, and improves engineering feasibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117127435B_ABST
    Figure CN117127435B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of gas separation material preparation, and in particular to a high-permeability aramid pulp / molecular sieve adsorption paper and a preparation process thereof, comprising the following steps: step 1: stirring, deflaking and washing alkali solution, aramid fiber and dimethyl sulfoxide to obtain aramid pulp dispersion A; step 2: adding molecular sieve to obtain mixed pulp suspension B under magnetic stirring conditions; step 3: dehydration and forming to obtain wet paper web D1 and wet paper web D2; step 4: pre-drying to obtain semi-finished paper web F1 and semi-finished paper web F2; step 5: mixing the semi-finished paper web F1 and semi-finished paper web F2 by rolling with a crouching roller in a manner of yellow surface contact and overlap, and then drying to obtain aramid pulp / molecular sieve adsorption paper. The invention uses the deprotonation effect of the DMSO / KOH / H2O system to pre-treat the surface of aramid pulp fiber, and the aramid pulp solution obtained after the treatment generates a negatively charged polymer solution due to deprotonation, so that the molecular sieve is more easily adsorbed around the aramid pulp.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gas separation material preparation, in particular to a high-permeability aramid pulp / molecular sieve adsorption paper and a preparation process thereof. Background Art

[0002] A large amount of pollutants emitted from industry, transportation and daily life will enter the air, gradually harming the human respiratory tract, lungs and blood, and because people have higher and higher requirements for indoor environment and comfort. In order to ensure the quality of indoor environment, it is usually necessary to treat indoor air. In addition to adjusting the temperature and humidity of indoor air, it is also necessary to treat air pollutants and carbon dioxide concentration. With the rapid development of the national economy, the market for interior decoration is becoming more and more prosperous. Some building materials used for interior decoration will continue to emit a certain concentration of volatile organic pollutants (such as benzene and formaldehyde), affecting people's health. In addition, in some confined spaces, such as underground shopping malls, meeting rooms with concentrated personnel, cabins, etc., the indoor carbon dioxide concentration continues to increase due to human breathing. When the carbon dioxide concentration reaches a certain value, it will also pose a threat to human health. Air pollutants also have a very complex composition, including harmful gases, fine droplets and solid particles, which will cause harm to human health. Therefore, to reduce the harm of gaseous pollutants to the human body, the most suitable solution is to prepare a highly permeable molecular sieve adsorption material to remove toxic and harmful gases directly during the air circulation process. This is also one of the simple and low-cost methods to reduce related risks.

[0003] At present, there are two main typical air filter materials. One is a porous material that is screened by size, including activated carbon, porous ceramics, etc.; the other is a fiber-based air filter material. Air filtration is a method for removing particulate matter from an airflow. An ideal air filter should be able to efficiently capture foreign particles while allowing air to pass easily. The filtration mechanism determines the retention of pollutants on the filter. The filtration mechanism of fiber-based filter materials mainly includes diffusion, interception, inertial collision, gravity, electrostatic adsorption, and intermolecular interaction. Because the fiber's slip effect on air can significantly reduce its resistance to air flow, fiber-based filter materials have higher porosity and lower pressure drop. Molecular sieve is a hydrated aluminosilicate that has the function of screening molecules. Due to the action of molecular gravity, surface forces are generated on the solid surface. When fluids such as air flow through, irregular motion causes molecular concentration on the surface, which reduces the number of such molecules in the fluid and achieves the purpose of separation and removal. For water, NH 3 , H 2 S, sulfur dioxide, carbon dioxide, C 2 H 5 OH, C 2 H6, C 2 H4 etc. have strong adsorption and removal effects. However, the current fiber-based air filter materials have high resistance and low dust holding capacity; the air volume is relatively small, and the filtering effect on fine particles or toxic and harmful gases is poor. Therefore, there is an urgent need for separation paper with high dust holding capacity and adsorption effect on toxic and harmful gases and fine particles. Based on this, the present invention provides a high-permeability aramid pulp / molecular sieve adsorption paper and its preparation process. Summary of the invention

[0004] Aiming at the problem that separation paper in the prior art cannot have both dust holding capacity and adsorption of fine particles and toxic and harmful gases, the present invention provides a preparation process of high-permeability aramid pulp / molecular sieve adsorption paper.

[0005] The present invention is achieved through the following technical solutions:

[0006] A process for preparing high-permeability aramid pulp / molecular sieve adsorption paper comprises the following steps:

[0007] Step 1: preparing aramid pulp liquid by mixing alkali solution, aramid fiber and dimethyl sulfoxide in a closed manner, and then adding deionized water to decompose, wash and activate, to obtain aramid pulp dispersion A;

[0008] Step 2: adding the molecular sieve into the aramid fiber dispersion A, and obtaining a mixed slurry suspension B under magnetic stirring conditions;

[0009] Step 3: the mixed pulp suspension B is evenly divided into suspension B1 and suspension B2, and the suspensions are dehydrated and formed in paper formers to obtain wet paper webs D1 and D2;

[0010] Step 4: pre-drying the wet paper webs D1 and D2 to obtain semi-finished paper webs F1 and F2 with one side being yellow and the other side being white;

[0011] Step 5: The semi-finished product F1 and the semi-finished paper web F2 are mixed by rolling with a couch roll in a manner that the yellow surfaces are in contact and overlapped, and then dried to obtain aramid pulp / molecular sieve adsorption paper.

[0012] Preferably, in step 1, the alkali solution is potassium hydroxide, and the concentration of the alkali solution is 0.40 mol / L to 0.45 mol / L; the aramid fiber is para-aramid fiber; and the ratio of the alkali solution, dimethyl sulfoxide, and aramid fiber is (50-55) mL: (300-350) mL: (3.0-3.5) g.

[0013] Preferably, in step 2, the molecular sieve is 4A molecular sieve, and the amount of molecular sieve added is (6.2~8.2) g.

[0014] Preferably, in step 3, the molecular sieve contents in suspension B1 and suspension B2 are both (3.1-4.1) g.

[0015] Preferably, in step 3, the preparation steps of the wet paper web D1 are as follows:

[0016] Step 31: firstly add water to the pulp storage chamber of the paper sheet former, and then pour the mixed pulp suspension B1 into the pulp storage chamber to form a pulp suspension C1 containing aramid pulp fibers and molecular sieves;

[0017] Step 32, the slurry suspension C1 in the slurry storage chamber is homogenized multiple times by a homogenizing roller, and then drained by a forming wire under vacuum suction, and after the slurry is drained, vacuum suction dehydration is performed to obtain a molecular sieve-aramid fiber wet paper web D1;

[0018] The steps for preparing the wet paper web D2 are the same as those for preparing the wet paper web D2.

[0019] Preferably, in step 31, the water supply volume of the slurry storage chamber is (3.5-4.5) L, and the total mass-volume concentration of aramid fibrils and molecular sieves obtained by mixing water with the mixed slurry suspension C is (1.69-1.74) g / L.

[0020] Preferably, in step 32, the number of homogenization is (10-20) times, and the homogenization time is (8-15) s; the mesh size of the filter during water filtration is (2300-2400) mesh, the vacuum drainage time is (20-25) min, and the vacuum suction dehydration time is (10-15) s.

[0021] Preferably, in step 4, the pre-drying temperature is (60-65)°C and the time is (10-15) min.

[0022] Preferably, in step 5, the couch roll rolls back and forth without applying any external pressure; the temperature during drying is (60-65)°C and the time is (1-2) h.

[0023] Aramid pulp / molecular sieve adsorption paper obtained by a high-permeability aramid pulp / molecular sieve adsorption paper preparation process.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The invention discloses a high-permeability aramid pulp / molecular sieve adsorption paper preparation process using DMSO / KOH / H 2 The deprotonation of the O system pre-treats the surface of aramid pulp fibers. The aramid pulp solution obtained after the treatment generates a negatively charged polymer solution due to the deprotonation, which is easier to react with the metal Al in the molecular sieve. 3+ 、Na +The reaction occurs, making the molecular sieve easier to adsorb around the aramid pulp, and the DMSO / KOH / H 2 O system is alkaline, with strong dissolving ability, wide dissolving range and good stability. It is an excellent solvent for aramid pulp, which opens the hydrogen bonds between aramid pulp molecular chains, making it easier for molecular sieves to be fixed on the fiber surface, and not easy to dissolve in the solution, thus improving the stability and further improving the retention rate of molecular sieves in paper-based materials.

[0026] At the same time, molecular sieves have a higher adsorption effect on toxic and harmful substances. Compared with pure paper-based filtration separation materials based on physical and mechanical retention, molecular sieves are a type of crystalline microporous material with a skeleton structure composed of silicon oxygen tetrahedrons and aluminum oxygen tetrahedrons connected to each other through shared oxygen atoms and having uniform intracrystalline pores. They have excellent ion exchange, catalytic and adsorption properties.

[0027] Furthermore, the reagents used in the present invention are all conventional pharmaceutical reagents, which are low-toxic, cheap and easily available, and the equipment used are all conventional instruments and equipment, which lays a good foundation for the engineering of high-permeability aramid pulp / molecular sieve adsorption paper and improves the feasibility of process engineering.

[0028] Furthermore, the present invention utilizes microporous mesh filtration. Since a general paper machine uses a (200-600) mesh forming mesh, the (2300-2400) mesh forming mesh used in the present invention is more compatible with the diameter of the 4A type molecular sieve used in the present invention, thereby reducing the problem of serious molecular sieve loss during the paper sheet forming process.

[0029] Furthermore, pressureless vacuum drying is adopted during drying, and aramid pulp fiber is used as the skeleton structure of the paper-based material, which has excellent heat resistance and flame retardancy, and can give the prepared paper-based material stable operation in high-temperature gas, thus broadening the application range of the paper-based material. Therefore, the fiber pore structure is ensured, and the air permeability of the paper sheet is improved, thereby further improving the adsorption effect of the patent of the present invention and expanding the application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of a process for preparing a high-permeability aramid pulp / molecular sieve adsorption paper according to the present invention;

[0031] Figure 2 SEM image of paper-based material of Example 1 of the present invention;

[0032] Figure 3 SEM image of the molecular sieve attachment in the paper-based material of Example 3 of the present invention;

[0033] Figure 4 The average thickness of the paper-based material and its error in the examples of the present invention;

[0034] Figure 5 The air permeability of the examples of the present invention;

[0035] Figure 6 XRD comparison diagram of paper-based materials in the examples of the present invention;

[0036] Figure 7 Formaldehyde filtration efficiency of paper-based materials in the examples of the present invention;

[0037] Figure 8 PM2.5 filtration efficiency of the paper-based material of the present invention;

[0038] Fig. 9 Cumulative void area of ​​the inventive examples as a function of void size. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.

[0040] A large amount of pollutants will enter the air, and fiber-based filter materials have higher porosity and lower pressure drop than other filter materials. Molecular sieves have a strong adsorption and removal effect on water, acetylene and carbon dioxide. The present invention provides a high-permeability aramid pulp / molecular sieve adsorption paper and a preparation process thereof.

[0041] Reference Figure 1 The present invention provides a process for preparing high-permeability aramid pulp / molecular sieve adsorption paper, comprising the following steps:

[0042] Step 1: Alkali solution, aramid fiber and dimethyl sulfoxide are stirred in a closed manner to prepare aramid pulp liquid, and then deionized water is added for decomposition and washing for activation to obtain aramid pulp dispersion A. Among them, "closed" means that the three raw materials are placed in a bottle with a bottle cap for stirring, and they are not in contact with the outside air during stirring. The alkali solution is potassium hydroxide, and the concentration of the alkali solution is 0.40mol / L~0.45mol / L; the aramid fiber is para-aramid fiber; the ratio of alkali solution, dimethyl sulfoxide, and aramid fiber is (50~55)mL: (300~350)mL: (3.0~3.5)g. The decomposition speed is (15000~25000) revolutions, which is used to give the optimal process range of dispersion and separation, and is not limited to this parameter.

[0043] Step 2: Add (6.2-8.2) g of molecular sieve to the aramid fiber dispersion A, and obtain a mixed slurry suspension B under magnetic stirring conditions; the molecular sieve is 4A molecular sieve, the main component of which is Na 2 O.Al 2 O 3 ·2SiO 2 9 / 2H 2 O, with an effective pore size of about 4A, can adsorb water and NH3 , H 2 S, sulfur dioxide, carbon dioxide, C 2 H 5 OH, C 2 H 6 , C 2 H 4 Molecules with critical diameter no greater than 4A.

[0044] Step 3: The mixed slurry suspension B is evenly divided into suspension B1 and suspension B2, and the suspensions are dehydrated and formed in a paper former to obtain wet paper webs D1 and D2. The molecular sieve content in the suspensions B1 and B2 is (3.1-4.1) g.

[0045] The steps for preparing the wet paper web D1 are as follows:

[0046] Step 31: First, add (3.5-4.5) L of water to the pulp storage chamber of the paper sheet former, and then pour the mixed pulp suspension B1 into the pulp storage chamber to form a pulp suspension C1 containing aramid pulp fibers and molecular sieves; the total mass-volume concentration of aramid precipitated fibers and molecular sieves in the pulp suspension C1 is (1.36-1.58) g / L.

[0047] Step 32, homogenizing the slurry suspension C1 in the slurry storage chamber with a homogenizing roller (10 to 20) times, and the homogenizing time is (8 to 15) seconds;

[0048] Then, the slurry is drained through a forming net with a mesh size of (2300-2400) for (20-25) minutes under vacuum suction. After the slurry is drained, vacuum suction dehydration is performed for (10-15) seconds to obtain a molecular sieve-aramid fiber wet paper web D1.

[0049] The steps for preparing the wet paper web D2 are the same as those for preparing the wet paper web D2.

[0050] Step 4: Pre-dry the wet paper webs D1 and D2 to obtain semi-finished paper webs F1 and F2 with one side yellow and the other side white. The white side has a higher molecular sieve content, mainly because the relative density of aramid pulp is generally 1.41~1.5g / cm 3 The relative density of molecular sieve is generally 2~2.8g / cm 3 Therefore, in the dehydration and forming stage, the molecular sieve is more likely to settle and aggregate than the aramid pulp, thus forming a side with more white molecular sieve and a side with more yellow aramid pulp; among them, the pre-drying temperature is (60~65)℃, and the time is (10~15)min.

[0051] Step 5: The semi-finished product F1 and the semi-finished paper web F2 are mixed by rolling with a couch roll in a manner that the yellow surfaces are in contact and overlapped, and then dried to obtain aramid pulp / molecular sieve adsorption paper. During operation, the couch roll rolls back and forth without any external pressure; the drying temperature is (60-65)°C and the drying time is (1-2) h.

[0052] Example 1

[0053] Step 1, weigh 1g KOH, 50ml water, 300ml DMSO and 3g para-aramid pulp, seal and stir for 6h, then add deionized water for decomposition and filtration. The ratio of aramid fiber solution to deionized water is 200mL:1000mL. The decomposition speed is 20000 rpm, and the decomposition time is 4min. Aramid fiber dispersion A is obtained;

[0054] Step 2, weigh 0g of molecular sieve and add it to the aramid fiber dispersion A, and obtain a mixed slurry suspension B under magnetic stirring conditions. The bottle mouth is sealed during magnetic stirring, the stirring reaction time is 15min, and the rotation speed is (400-600) r / min.

[0055] Step 3, dividing the mixed pulp suspension B into two parts B1 and B2 with equal molecular sieve contents, and dehydrating and forming them in the same way to obtain wet paper webs D1 and D2.

[0056] Step 31, in the cross-sectional area of ​​0.0314m 2 First, 3.5 L of water is added to the pulp storage chamber of the paper sheet former, and then the mixed pulp suspension B1 of step 2 is poured into the pulp storage chamber to form a pulp suspension C1 with a concentration of 0.86 g / L, that is, the total mass-volume concentration of aramid pulp fiber and molecular sieve in the pulp suspension C1 is 0.86 g / L, and the mixture is diluted;

[0057] Step 32, homogenizing the diluted slurry suspension C1 in the slurry storage chamber with a homogenizing roller, the homogenization times are 10 times, and the homogenization time is 8 seconds; the diluted slurry suspension B is drained and formed under vacuum suction through a forming screen with a diameter of 200 mm and a mesh number of 2300 meshes, and after the slurry is filtered, vacuum suction dehydration is performed for 10 seconds to obtain a molecular sieve-aramid fiber wet paper web D1;

[0058] Step 4, pad the formed molecular sieve-aramid fiber wet paper webs D1 and D2 with felt on both sides and put them into a precision air drying oven for pre-drying at 60°C for 15 minutes to obtain semi-finished paper webs F1 and F2 with one side yellow and the other side white.

[0059] Step 5, the semi-finished product F1 and the semi-finished paper web F2 are mixed by rolling with a couch roller in a manner that the yellow surfaces are in contact and overlapped, and the couch roller is rolled back and forth for 2 seconds without applying any external force, and the mixed molecular sieve-aramid fiber wet paper web is placed in a precision blast drying oven for final drying at a temperature of 65° C. for 1.5 hours, to obtain a high-permeability aramid pulp / molecular sieve adsorption paper;

[0060] The molecular sieve aramid fiber paper prepared in Example 1 has an actual weight of 2.78 g and a specific surface area of ​​0.0114 m 2 / g air permeability 26.276 (μm / Pa·s), average thickness 0.527mm, average tightness 0.095g / cm 3 , thickness standard deviation 0.076mm, breaking stress 21.33MPa, elongation 7.06%, formaldehyde filtration efficiency 93.73%, PM2.5 filtration efficiency is 90.80%. Figure 2 The SEM image shown shows that there are a large number of aramid pulp fibers on the paper base material, and there are large gaps between them that can be filled with fillers.

[0061] Example 2

[0062] Step 1, weigh 1g KOH, 50ml water, 300ml DMSO and 3g para-aramid pulp, seal and stir for 6h, then add deionized water for decomposition and filtration. The ratio of aramid fiber solution to deionized water is 200mL:1000mL. The decomposition speed is 20000 rpm, and the decomposition time is 4min. Aramid fiber dispersion A is obtained;

[0063] Step 2, weighing 2g of molecular sieve and adding it to the aramid fiber dispersion A, and obtaining a mixed slurry suspension B under magnetic stirring conditions, the bottle mouth is sealed during magnetic stirring, the stirring reaction time is 15min, and the rotation speed is (400-600) r / min;

[0064] Step 3, dividing the mixed pulp suspension B into two parts B1 and B2 with equal molecular sieve contents, and dehydrating and forming them successively by the same process to obtain wet paper webs D1 and D2.

[0065] Step 31, in the cross-sectional area of ​​0.0314m 2 First, 3.5 L of water is added to the pulp storage chamber of the paper sheet former, and then the mixed pulp suspension B1 of step 2 is poured into the pulp storage chamber to form a pulp suspension C1 with a concentration of 1.14 g / L, that is, the total mass-volume concentration of aramid pulp fibers and molecular sieves in the pulp suspension C1 is 1.14 g / L;

[0066] Step 32, homogenize the diluted slurry suspension C1 in the slurry storage chamber with a homogenizing roller, the homogenization times are 10 times, and the homogenization time is 8 seconds; the diluted slurry suspension B is drained and formed under the action of vacuum suction through a forming screen with a diameter of 200 mm and a mesh size of 2300. After the slurry is filtered, it is vacuum-dehydrated for 10 seconds to obtain a molecular sieve-aramid fiber wet paper web D1.

[0067] Step 4, pad the formed molecular sieve-aramid fiber wet paper webs D1 and D2 with felt on both sides and put them into a precision air drying oven for pre-drying at 60°C for 15 minutes to obtain semi-finished paper webs F1 and F2 with one side yellow and the other side white.

[0068] Step 5, the semi-finished product F1 and the semi-finished paper web F2 are mixed by rolling with a couch roller in a manner that the yellow surfaces are in contact and overlapped, and the couch roller is used to reciprocate for 2 seconds without applying any external force, and the mixed molecular sieve-aramid fiber wet paper web is placed in a precision blast drying oven for final drying at a temperature of 65° C. for 1.5 hours to obtain a high-permeability aramid pulp / molecular sieve adsorption paper;

[0069] The molecular sieve aramid fiber paper prepared in Example 2 has an actual weight of 4.43 g and a specific surface area of ​​0.0072 m 2 / g, air permeability 20.1 (μm / Pa·s), average thickness 0.620mm, average tightness 0.081g / cm 3 The standard deviation of thickness is 0.129mm, the breaking stress is 7.65MPa, the elongation is 5.76%, the filtration efficiency for formaldehyde is 93.17%, and the filtration efficiency for PM2.5 is 96.63%.

[0070] Example 3

[0071] Step 1, weigh 1g KOH, 50ml water, 300ml DMSO and 3g para-aramid pulp, seal and stir for 6h, then add deionized water for decomposition and filtration. The ratio of aramid fiber solution to deionized water is 200mL:1000mL. The decomposition speed is 20000 rpm, and the decomposition time is 4min. Aramid fiber dispersion A is obtained;

[0072] Step 2, weighing 4 g of molecular sieve and adding it to the aramid fiber dispersion A, and obtaining a mixed slurry suspension B under magnetic stirring conditions, the bottle mouth is sealed during magnetic stirring, the stirring reaction time is 15 min, and the rotation speed is (400-600) r / min;

[0073] Step 3, dividing the mixed slurry suspension B into two parts B1 and B2 with equal molecular sieve content, and dehydrating and forming them successively.

[0074] Step 31, in the cross-sectional area of ​​0.0314m2 First, 3.5 L of water is added to the pulp storage chamber of the paper sheet former, and then the mixed pulp suspension B1 of step 2 is poured into the pulp storage chamber to form a pulp suspension C1 with a concentration of 1.43 g / L, that is, the total mass-volume concentration of aramid pulp fibers and molecular sieves in the pulp suspension C1 is 1.43 g / L;

[0075] Step 32, homogenizing the diluted slurry suspension C1 in the slurry storage chamber with a homogenizing roller, the homogenization times are 10 times, and the homogenization time is 8 seconds; the diluted slurry suspension B is drained and formed under vacuum suction through a forming screen with a diameter of 200 mm and a mesh number of 2300 meshes, and after the slurry is filtered, vacuum suction dehydration is performed for 10 seconds to obtain a molecular sieve-aramid fiber wet paper web D1;

[0076] Step 4, pad the formed molecular sieve-aramid fiber wet paper webs D1 and D2 with felt on both sides and put them into a precision air drying oven for pre-drying at 60°C for 15 minutes to obtain semi-finished paper webs F1 and F2 with one side yellow and the other side white.

[0077] Step 5, the semi-finished product F1 and the semi-finished paper web F2 are mixed by rolling with a couch roller in a manner that the yellow surfaces are in contact and overlapped, and the couch roller is used to reciprocate for 2 seconds without applying any external force, and the mixed molecular sieve-aramid fiber wet paper web is placed in a precision blast drying oven for final drying at a temperature of 65° C. for 1.5 hours to obtain a high-permeability aramid pulp / molecular sieve adsorption paper;

[0078] The molecular sieve aramid fiber paper prepared in Example 3 has an actual weight of 6.04 g and a specific surface area of ​​0.0052 m 2 / g, air permeability 7.697 (μm / Pa·s), average thickness 0.705mm, average tightness 0.071g / cm 3 , thickness standard deviation 0.127mm, breaking stress 7.15MPa, elongation 4.85%, formaldehyde filtration efficiency 71.97%, PM2.5 filtration efficiency is 97.39%. Figure 3 It can be seen that when the molecular sieve content is 4g, the gaps in the aramid pulp fiber have been filled with a large number of molecular sieve particles.

[0079] Example 4

[0080] Step 1, weigh 1g KOH, 50ml water, 300ml DMSO and 3g para-aramid pulp, seal and stir for 6h, then add deionized water for decomposition and filtration. The ratio of aramid fiber solution to deionized water is 200mL:1000mL. The decomposition speed is 20000 rpm, and the decomposition time is 4min. Aramid fiber dispersion A is obtained;

[0081] Step 2, weighing 6 g of molecular sieve and adding it to the aramid fiber dispersion A, and obtaining a mixed slurry suspension B under magnetic stirring conditions, the bottle mouth is sealed during magnetic stirring, the stirring reaction time is 15 min, and the rotation speed is (400-600) r / min;

[0082] Step 3, dividing the mixed pulp suspension B into two parts B1 and B2 with equal molecular sieve contents, and successively dehydrating and forming them to obtain wet paper webs D1 and D2.

[0083] Step 31, in the cross-sectional area of ​​0.0314m 2 First, 3.5 L of water is added to the pulp storage chamber of the paper sheet former, and then the mixed pulp suspension B1 of step 2 is poured into the pulp storage chamber to form a pulp suspension C1 with a concentration of 1.71 g / L, that is, the total mass-volume concentration of aramid pulp fibers and molecular sieves in the pulp suspension C1 is 1.71 g / L;

[0084] Step 32, homogenizing the diluted slurry suspension C1 in the slurry storage chamber with a homogenizing roller, the homogenization times are 10 times, and the homogenization time is 8 seconds; the diluted slurry suspension B is drained and formed under vacuum suction through a forming screen with a diameter of 200 mm and a mesh number of 2300 meshes, and after the slurry is filtered, vacuum suction dehydration is performed for 10 seconds to obtain a molecular sieve-aramid fiber wet paper web D1;

[0085] Step 4, pad the formed molecular sieve-aramid fiber wet paper webs D1 and D2 with felt on both sides and put them into a precision air drying oven for pre-drying at 60°C for 15 minutes to obtain semi-finished paper webs F1 and F2 with one side yellow and the other side white.

[0086] Step 5, the semi-finished product F1 and the semi-finished paper web F2 are mixed by rolling with a couch roller in a manner that the yellow surfaces are in contact and overlapped, and the couch roller is rolled back and forth for 2 seconds without applying any external force, and the mixed molecular sieve-aramid fiber wet paper web is placed in a precision blast drying oven for final drying at a temperature of 65° C. for 1.5 hours, to obtain a high-permeability aramid pulp / molecular sieve adsorption paper;

[0087] The molecular sieve aramid fiber paper prepared in Example 4 has an actual weight of 8.01 g and a specific surface area of ​​0.0040 m 2 / g, air permeability 12.700 (μm / Pa·s), average thickness 1.036mm, average tightness 0.048g / cm 3 The standard deviation of thickness is 0.275mm, the breaking stress is 3.34MPa, the elongation is 5.15%, the filtration efficiency for formaldehyde is 68.17%, and the filtration efficiency for PM2.5 is 97.91%.

[0088] Example 5

[0089] Step 1, weigh 1g KOH, 50ml water, 300ml DMSO and 3g para-aramid pulp, seal and stir for 6h, then add deionized water for decomposition and filtration. The ratio of aramid fiber solution to deionized water is 200mL:1000mL. The decomposition speed is 20000 rpm, and the decomposition time is 4min. Aramid fiber dispersion A is obtained;

[0090] Step 2, weighing 8g of molecular sieve and adding it to the aramid fiber dispersion A, and obtaining a mixed slurry suspension B under magnetic stirring conditions, the bottle mouth is sealed during magnetic stirring, the stirring reaction time is 15min, and the rotation speed is (400-600) r / min;

[0091] Step 3, dividing the mixed pulp suspension B into two parts B1 and B2 with equal molecular sieve contents, and successively dehydrating and forming them to obtain wet paper webs D1 and D2.

[0092] Step 31, in the cross-sectional area of ​​0.0314m 2 First, 3.5 L of water is added to the pulp storage chamber of the paper sheet former, and then the mixed pulp suspension B1 of step 2 is poured into the pulp storage chamber to form a pulp suspension C1 with a concentration of 2.00 g / L, that is, the total mass-volume concentration of aramid pulp fibers and molecular sieves in the pulp suspension C1 is 2.00 g / L;

[0093] Step 32, homogenizing the diluted slurry suspension C1 in the slurry storage chamber with a homogenizing roller, the homogenization times are 10 times, and the homogenization time is 8 seconds; the diluted slurry suspension B is drained and formed under vacuum suction through a forming screen with a diameter of 200 mm and a mesh number of 2300 meshes, and after the slurry is filtered, vacuum suction dehydration is performed for 10 seconds to obtain a molecular sieve-aramid fiber wet paper web D1;

[0094] Step 4, pad the formed molecular sieve-aramid fiber wet paper web D1 with felt on both sides and put it into a precision air drying oven for pre-drying at 60° C. for 15 minutes to obtain semi-finished paper webs F1 and F2 with one side being yellow and the other side being white.

[0095] Step 5, the semi-finished product F1 and the semi-finished paper web F2 are mixed by rolling with a couch roller in a manner that the yellow surfaces are in contact and overlapped, and the couch roller is used to reciprocate for 2 seconds without applying any external force, and the mixed molecular sieve-aramid fiber wet paper web is placed in a precision blast drying oven for final drying at a temperature of 65° C. for 1.5 hours to obtain a high-permeability aramid pulp / molecular sieve adsorption paper;

[0096] The molecular sieve aramid fiber paper prepared in Example 5 has an actual weight of 9.55 g and a specific surface area of ​​0.0033 m 2 / g, air permeability 18 (μm / Pa·s), average thickness 0.817mm, average tightness 0.061g / cm3 The standard deviation of thickness is 0.118mm, the breaking stress is 2.19MPa, the elongation is 4.11%, the filtration efficiency for formaldehyde is 55.70%, and the filtration efficiency for PM2.5 is 98.10%.

[0097] Table 1 Mass and proportion of each component in the examples

[0098]

[0099] The invention also discloses aramid pulp / molecular sieve adsorption paper obtained by the high-permeability aramid pulp / molecular sieve adsorption paper preparation process.

[0100] Figure 4 The average thickness of the paper base material and its error in each embodiment. As the molecular sieve content increases, the thickness of the paper also increases, indicating that most of the added molecular sieves are retained in the paper. However, it can be seen from the figure that when the molecular sieve addition amount is 6g, the amount retained in the paper is the largest; when the added molecular sieve content reaches 8g, the amount of molecular sieve that can be retained in the paper will decrease. This shows that the retention rate of a certain amount of aramid pulp for the molecular sieve is certain, and the amount of molecular sieve added should not be too much.

[0101] Reference Figure 5 It can be seen that with the increase of molecular sieve content in the paper base, when the molecular sieve addition amount is 4g, the corresponding air permeability of the paper is better. Figure 6 It can be seen that as the molecular sieve content in the paper base of each example increases, the relatively gentle peak representing the aramid fiber will gradually be replaced by a sharp peak representing the molecular sieve.

[0102] Reference Figure 7 The filtration efficiency of formaldehyde decreases with the increase of molecular sieve content. In comparison, the paper base with 2g molecular sieve added has better filtration effect on formaldehyde, followed by the paper base with 4g molecular sieve added.

[0103] Reference Figure 8 It can be seen that with the increase of molecular sieve addition content, the filtering effect for PM2.5 gradually increases. Fig. 9 It can be seen that the cumulative void area changes with the void, rising relatively slowly in the initial stage, rising rapidly in the middle stage, and then becoming more stable in the final stage.

[0104] The above description is only a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and substitutions, and these modifications and substitutions are also within the scope of protection covered by the claims.

Claims

1. A process for preparing high-permeability aramid pulp / molecular sieve adsorption paper, It is characterized in that The following steps are involved: Step 1: preparing aramid pulp liquid by stirring alkali solution, aramid fiber and dimethyl sulfoxide in a closed manner, and then adding deionized water for decomposition, washing and activation to obtain aramid pulp dispersion A; wherein the alkali solution is potassium hydroxide, and the concentration of the alkali solution is 0.40 mol / L to 0.45 mol / L; the aramid fiber is para-aramid fiber; the ratio of alkali solution, dimethyl sulfoxide and aramid fiber is (50-55) mL: (300-350) mL: (3.0-3.5) g; Step 2: adding molecular sieve to the aramid fiber dispersion A, and obtaining a mixed slurry suspension B under magnetic stirring conditions; wherein the molecular sieve is 4A molecular sieve, and the addition amount of the molecular sieve is (6.2-8.2) g; Step 3: The mixed slurry suspension B is evenly divided into suspension B1 and suspension B2, and the two are dehydrated and formed in a paper former to obtain wet paper web D1 and wet paper web D2; wherein the molecular sieve content in suspension B1 and suspension B2 is (3.1-4.1) g; the preparation steps of wet paper web D1 are as follows: Step 31: first add water to the pulp storage chamber of the paper sheet former, and then pour the mixed pulp suspension B1 into the pulp storage chamber to form a pulp suspension C1 containing aramid pulp fibers and molecular sieves; the amount of water added to the pulp storage chamber is (3.5-4.5) L, and the water and the mixed pulp suspension C are mixed to obtain a total mass-volume concentration of aramid fibrils and molecular sieves of (1.69-1.74) g / L; Step 32, the slurry suspension C1 in the slurry storage chamber is homogenized multiple times by a homogenizing roller, and then drained by a forming net under vacuum suction, and vacuum suction dehydration is performed after the slurry is filtered to obtain a molecular sieve-aramid fiber wet paper web D1; the number of homogenization is (10-20) times, and the homogenization time is (8-15) s; the mesh number of the filter screen during the drainage is (2300-2400) mesh, the vacuum drainage time is (20-25) min, and the vacuum suction dehydration time is (10-15) s; The preparation steps of wet paper web D2 are the same as those of wet paper web D1; Step 4: pre-drying the wet paper webs D1 and D2 to obtain semi-finished paper webs F1 and F2 with one side being yellow and the other side being white; wherein the pre-drying temperature is (60-65)°C and the time is (10-15) min; Step 5: Mix the semi-finished product F1 and the semi-finished paper web F2 by rolling them with the yellow surfaces in contact and overlapping manner, and then dry them to obtain aramid pulp / molecular sieve adsorption paper; wherein the couch roller rolls back and forth without applying any external pressure; the temperature during drying is (60-65)°C and the time is (1-2) h.

2. Aramid pulp / molecular sieve adsorption paper obtained by the high permeability aramid pulp / molecular sieve adsorption paper preparation process according to claim 1.