Carbon fiber recycling method and recycling device

By soaking and washing the carbon fiber reinforced composite material with a composite strong alkali solution, the problem of poor carbon fiber recycling effect is solved, efficient recycling and fat removal rate are achieved, and the mechanical properties of carbon fiber are improved.

CN117143392BActive Publication Date: 2024-11-05SHENZHEN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310970941.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-03
Publication Date
2024-11-05
Estimated Expiration
2043-08-03

AI Technical Summary

Technical Problem

In the prior art, carbon fiber recycle effect is poor, low fat removal rate and low recovery rate, and carbon fiber reinforced composite materials are difficult to effectively recycle and process, resulting in environmental pollution and waste of resources.

Method used

The carbon fiber reinforced composite material is soaked and washed by using a composite strong alkali solution. The carbon fiber reinforced composite material is combined with aprotic polar solvent, and combined with proton additives to form a super-strong alkali system to achieve efficient recycling of carbon fibers.

Benefits of technology

It realizes efficient recycling of carbon fibers, with a fat removal rate of 100%, solving the problems of poor recycling effect and low recovery rate, and improving the tensile strength and interface shear performance of carbon fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117143392B_ABST
    Figure CN117143392B_ABST
Patent Text Reader

Abstract

The present invention discloses a carbon fiber recycling method and a recycling device, wherein the recycling method specifically comprises the following steps: S1, immersing a carbon fiber reinforced composite material (CFRP) in a composite strong alkali solution and reacting for 20 to 180 minutes to obtain a carbon fiber crude product and a reaction solution; S2, washing and drying the carbon fiber crude product obtained in S1 to obtain recycled carbon fiber. The present invention not only achieves the purpose of a degreasing rate of up to 100% by selecting a composite strong alkali solution to recycle the carbon fiber reinforced composite material, but also solves the problems of poor performance and low recovery rate of the recycled carbon fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon fiber recovery, and in particular relates to a carbon fiber recovery method and a recovery device. Background Art

[0002] Carbon fiber reinforced plastics (CFRP) have high strength (2-10Gpa), high stiffness (200-700Gpa), low specific gravity (1.5-2g / cm 3 ) and corrosion resistance (acid, alkali, salt), it is widely used in aerospace, construction and civil engineering, wind power generation, sports and leisure, rail transit and pressure vessel industries. Its global demand will reach 199,000 tons in 2022.

[0003] The consumption of carbon fiber reinforced composite materials has accumulated over the years, resulting in a huge amount of CFRP waste. The resin in carbon fiber reinforced composite materials is a three-dimensional cross-linked network structure with insoluble and infusible properties, while carbon fiber is inorganic and inert, so carbon fiber reinforced composite materials are extremely difficult to degrade. The traditional methods of CFRP waste treatment are mainly landfill and incineration. Landfill not only occupies a large amount of precious land resources, but also slowly releases toxic gases such as CO2 and SO2; incinerating one ton of carbon fiber reinforced composite materials will produce 2011kg CO2, which is not conducive to the sustainable development of society. Realizing efficient and environmentally friendly recycling and treatment of carbon fiber reinforced composite waste is an urgent frontier topic. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a carbon fiber recycling method, which solves the problems of poor carbon fiber recycling effect, low fat removal rate and low recovery rate in the prior art.

[0005] The present invention also aims to provide a recovery device using the above recovery method.

[0006] In order to solve the above problems, the technical solution adopted by the present invention is: a carbon fiber recycling method, characterized in that the method specifically comprises the following steps:

[0007] S1. Soaking the carbon fiber reinforced composite material in a composite strong alkali solution, and allowing it to react or magnetically stir or mechanically stir for 20 to 180 minutes to obtain a crude carbon fiber product and a reaction solution;

[0008] S2. Washing and drying the crude carbon fiber obtained in S1 to obtain recycled carbon fiber.

[0009] In S1, the carbon fiber reinforced composite material is immersed in the composite strong alkali solution at normal pressure and 25-180°C.

[0010] Preferably, in S1, the carbon fiber reinforced composite material includes carbon fiber prepreg, bisphenol A type epoxy resin carbon fiber reinforced composite material, unsaturated polyester resin carbon fiber reinforced composite material, epoxy vinyl ester resin carbon fiber reinforced composite material, phenolic resin carbon fiber reinforced composite material, bismaleimide resin carbon fiber reinforced composite material.

[0011] Preferably, in S1, the composite strong alkali solution is a mixture of a strong ionic alkali solution and a non-protonic polar solvent; the mass ratio of the strong ionic alkali solution to the non-protonic polar solvent is 0.05-0.2, and the concentration of the strong ionic alkali solution is 1-120wt.%.

[0012] Preferably, the composite strong alkali solution further contains a proton auxiliary agent, and the mass ratio of the strong ionic alkali solution to the proton auxiliary agent is 0.01 to 1.2; the mass ratio of the proton auxiliary agent to the aprotic polar solvent is 1 to 25 wt.%.

[0013] Preferably, the strong ionic base solution is at least one of EtONa, EtOK, NaOBu-t, KOBu-t, NaOH, and KOH; and the aprotic polar solvent is at least one of DMF, THF, and DMSO.

[0014] Preferably, the proton auxiliary agent is at least one of water, methanol and ethanol.

[0015] Preferably, in S2, the crude carbon fiber product is washed with a cleaning liquid; wherein the cleaning liquid is at least one of deionized water, DMSO, ethanol, and chloroform.

[0016] Preferably, the drying temperature is 20 to 80° C., and the drying time is 5 to 40 hours.

[0017] Another technical solution of the present invention is achieved as follows: a recovery device using the above-mentioned carbon fiber recovery method, which includes a composite strong alkali solution preparation kettle, a carbon fiber reinforced composite material (CFRP) soaker and a first connecting pipeline, the composite strong alkali solution preparation kettle is connected to the carbon fiber reinforced composite material (CFRP) soaker through the first connecting pipeline, and the first connecting pipeline is provided with a control valve capable of controlling the material flow rate and feeding time.

[0018] Preferably, the recovery device also includes a strong ion base solution container, a water container, a non-protonic polar solvent container and a second connecting pipeline. The strong ion base solution container, water container and non-protonic polar solvent container are connected to the composite strong alkali solution preparation kettle through the second connecting pipeline. The pipelines on the second connecting pipeline that are respectively connected to the ion base solution container, water container and non-protonic polar solvent container are all provided with control valves.

[0019] Preferably, the composite strong alkali solution preparation kettle is also provided with a proton additive addition port.

[0020] Preferably, a stirring component is also provided in the composite strong alkali solution preparation kettle.

[0021] Preferably, an opening for placing the carbon fiber reinforced composite material (CFRP) infuser is also provided above the carbon fiber reinforced composite material (CFRP) infuser.

[0022] Compared with the prior art, the present invention recovers the carbon fiber in the carbon fiber reinforced composite material by selecting a composite strong alkali solution, which not only achieves the purpose of a degreasing rate of up to 100%, but also solves the problems of poor carbon fiber recovery effect and low recovery rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG1 is a schematic diagram showing the results of recycling carbon fibers in a thermosetting prepreg using the composite strong alkali solution of the present invention; wherein:

[0024] Figure 1a Schematic diagram of a thermosetting carbon fiber prepreg in an embodiment of the present invention;

[0025] Figure 1b A schematic diagram of carbon fiber recovered from an embodiment of the present invention;

[0026] Figure 1c This is a schematic diagram of the reaction solution after the recovery is completed in the embodiment of the present invention;

[0027] FIG2 is a schematic diagram showing the results of using the composite strong alkali solution of the present invention to recover carbon fibers from bisphenol A epoxy resin CFRP; wherein:

[0028] Figure 2a Schematic diagram of bisphenol A epoxy resin CFRP in an embodiment of the present invention;

[0029] Figure 2b A schematic diagram of carbon fiber recovered from an embodiment of the present invention;

[0030] FIG3 is a schematic diagram showing the results of using the composite strong alkali solution of the present invention to recover carbon fibers from unsaturated polyester resin CFRP; wherein:

[0031] Figure 3a Schematic diagram of unsaturated polyester resin CFRP in an embodiment of the present invention;

[0032] Figure 3b A schematic diagram of carbon fiber recovered from an embodiment of the present invention;

[0033] FIG4 is a schematic diagram showing the results of recycling carbon fibers in epoxy vinyl ester resin CFRP using the composite strong alkali solution of the present invention; wherein:

[0034] Figure 4a Schematic diagram of epoxy vinyl ester resin CFRP in an embodiment of the present invention;

[0035] Figure 4b A schematic diagram of carbon fiber recovered from an embodiment of the present invention;

[0036] FIG5 is a schematic diagram showing the results of using the composite strong alkali solution of the present invention to recover carbon fibers from phenolic resin CFRP; wherein:

[0037] Figure 5a Schematic diagram of phenolic resin CFRP in an embodiment of the present invention;

[0038] Figure 5b A schematic diagram of carbon fiber recovered from an embodiment of the present invention;

[0039] FIG6 is a schematic diagram showing the results of using the composite strong alkali solution of the present invention to recover carbon fibers from bismaleimide resin CFRP; wherein:

[0040] Figure 6a Schematic diagram of bismaleimide resin CFRP in an embodiment of the present invention;

[0041] Figure 6b A schematic diagram of carbon fiber recovered from an embodiment of the present invention;

[0042] Figure 7 TGA-DTG curves of CFRP and carbon fiber recovered from the embodiment of the present invention;

[0043] Figure 8 This is a graph showing the tensile strength of carbon fibers recovered from an embodiment of the present invention;

[0044] Fig. 9 This is a SEM image of the carbon fiber recovered from the embodiment of the present invention;

[0045] Fig.10 This is an AFM image of the carbon fiber recovered from an embodiment of the present invention;

[0046] Fig.11 and Fig.12 This is the XPS graph of carbon fiber recovered from the embodiment of the present invention;

[0047] Fig.13 A recycling device for recycling carbon fiber provided in an embodiment of the present invention

[0048] In the figure, 1. composite strong alkali solution preparation kettle, 11. proton additive addition port, 12. stirring assembly, 2. CFRP soaker, 21. opening, 3. first connecting pipeline, 4. strong ion alkali solution container, 5. water container, 6. non-protonic polar solvent container, 7. control valve, 8. second connecting pipeline, 9. CFRP. DETAILED DESCRIPTION

[0049] An embodiment of the present invention provides a carbon fiber recycling method, which specifically includes the following steps:

[0050] S1. Immerse the carbon fiber reinforced composite material (CFRP) in a composite strong alkali solution at normal pressure and 25-180° C., and allow to react for 20-180 minutes to obtain a crude carbon fiber product and a reaction solution;

[0051] S2. Wash the crude carbon fiber obtained in S1 with deionized water, and then dry it at a temperature of 20 to 80° C. for 5 to 40 hours to obtain recycled carbon fiber.

[0052] In addition, the composite strong base solution described in S1 above is a mixture of a strong ionic base solution and a non-protonic polar solvent; the mass ratio of the strong ionic base solution to the non-protonic polar solvent is 0.05-0.2, and the concentration of the strong ionic base solution is 0.01-1.1.

[0053] Furthermore, the mass ratio of the strong ionic alkali solution to the aprotic polar solvent is 0.05 to 0.1, and the concentration of the strong ionic alkali solution is 1 to 110 wt.%.

[0054] Furthermore, the composite strong alkali solution also contains a proton auxiliary agent, and the mass ratio of the strong ionic alkali solution to the proton auxiliary agent is 0.01-1.1; the mass ratio of the proton auxiliary agent to the non-protonic polar solvent is 0.05-0.2.

[0055] Furthermore, the mass ratio of the strong ionic base solution to the proton auxiliary agent is 0.01 to 0.8; the mass ratio of the proton auxiliary agent to the aprotic polar solvent is 1 to 20 wt.%.

[0056] The strong ion base solution is at least one of EtONa, EtOK, NaOBu-t, KOBu-t, NaOH, and KOH; the aprotic polar solvent is at least one of DMF, THF, and DMSO; the aprotic polar solvent is at least one of DMSO, DMF, and THF; the proton auxiliary agent is at least one of water, methanol, and ethanol; the pK of the composite strong base solution is a The value is 30~40.

[0057] Table 1 Typical super base systems

[0058]

[0059]

[0060] In view of the infusibility and insolubility of epoxy resin, a non-protonic solvent / strong ionic base / proton auxiliary composite strong superbase system is designed. A small amount of composite superbase formed in the system exists in the solution near the solid-liquid interface; when the superbase is consumed in the reaction, it is continuously replenished from the solid phase to the liquid phase near the interface to form phase transfer catalysis; the proton auxiliary in the system can continuously transport protons to convert the anions formed during the reaction into new stable molecules, thereby maintaining the strong alkalinity of the system; in addition, the non-protonic polar solvent plays a dual role as a reaction solvent and a reaction reagent in the recovery reaction, and has an accelerating and catalytic effect. For example, in the KOBu-t / DMSO system, double bond rearrangement can be produced, so that the reaction can proceed homogeneously at a lower temperature, significantly improving the recovery efficiency. Therefore, the combination of superbase phase transfer catalytic performance and chemical swelling performance can achieve efficient recovery of carbon fiber reinforced composites (CFRP) at room temperature and pressure.

[0061] In addition, refer to Figure 8 The embodiment of the present invention also provides a recovery device using the above-mentioned carbon fiber recovery method, which includes a composite strong alkali solution preparation kettle 1, a CFRP soaker 2 and a first connecting pipeline 3. The composite strong alkali solution preparation kettle 1 is connected to the preform soaker 2 through the first connecting pipeline 3. The first connecting pipeline 3 is provided with a control valve 7 capable of controlling the material flow rate and feeding time.

[0062] In the specific implementation process, the recovery device also includes a strong ion base solution container 4, a water container 5, a non-protonic polar solvent container 6 and a second connecting pipeline 8. The strong ion base solution container 4, the water container 5 and the non-protonic polar solvent container 6 are connected to the composite strong alkali solution preparation kettle 1 through the second connecting pipeline 8. The second connecting pipeline 8 is respectively connected to the ion base solution container 4, the water container 5, and the non-protonic polar solvent container 6. The pipelines are provided with control valves 7.

[0063] In the specific implementation process, the composite strong alkali solution preparation kettle 1 is also provided with a proton auxiliary agent addition port 11 .

[0064] In the specific implementation process, a stirring component 12 is also provided in the composite strong alkali solution preparation kettle 1 .

[0065] In a specific implementation process, an opening 21 for placing the CFRP 9 is further provided above the CFRP soaker 2 .

[0066] The following are specific embodiments

[0067] 1. Example of preparing a composite strong alkali solution

[0068] Example 1

[0069] The composite strong alkali solution for recycling carbon fiber provided in Example 1 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.2 g, the mass of ethanol is 1 g, and the mass of DMSO is 200 g.

[0070] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system composite strong alkaline solution;

[0071] Example 2

[0072] The composite strong alkali solution for recycling carbon fiber provided in Example 2 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.2 g, the mass of ethanol is 1 g, and the mass of DMSO is 100 g.

[0073] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system composite strong alkaline solution;

[0074] Example 3

[0075] The composite strong alkali solution for recycling carbon fiber provided in Example 3 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.2 g, the mass of ethanol is 1 g, and the mass of DMSO is 50 g.

[0076] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system composite strong alkaline solution;

[0077] Example 4

[0078] The composite strong alkali solution for recycling carbon fiber provided in Example 4 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.1 g, the mass of ethanol is 1 g, and the mass of DMSO is 200 g.

[0079] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system composite strong alkaline solution;

[0080] Example 5

[0081] The composite strong alkali solution for recycling carbon fiber provided in Example 5 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.1 g, the mass of ethanol is 1 g, and the mass of DMSO is 100 g.

[0082] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0083] Example 6

[0084] The composite strong alkali solution for recycling carbon fiber provided in Example 6 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.1 g, the mass of ethanol is 1 g, and the mass of DMSO is 50 g.

[0085] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0086] Example 7

[0087] The composite strong alkali solution for recycling carbon fiber provided in Example 7 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically: the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.04g, the mass of ethanol is 1g, and the mass of DMSO is 200g.

[0088] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0089] Example 8

[0090] The composite strong alkali solution for recycling carbon fiber provided in Example 8 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.04g, the mass of ethanol is 1g, and the mass of DMSO is 100g.

[0091] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0092] Example 9

[0093] The composite strong alkali solution for recycling carbon fiber provided in Example 9 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically: the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.04g, the mass of ethanol is 1g, and the mass of DMSO is 50g.

[0094] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0095] Example 10

[0096] The composite strong alkali solution for recycling carbon fiber provided in Example 10 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.01 g, the mass of ethanol is 1 g, and the mass of DMSO is 200 g.

[0097] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0098] Embodiment 11

[0099] The composite strong alkali solution for recycling carbon fiber provided in Example 11 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.01 g, the mass of ethanol is 1 g, and the mass of DMSO is 100 g.

[0100] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0101] Example 12

[0102] The composite strong alkali solution for recycling carbon fiber provided in Example 12 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C2H5ONa in the composite strong alkali solution is 0.01 g, the mass of ethanol is 1 g, and the mass of DMSO is 50 g.

[0103] The specific preparation method is: inject the corresponding mass of DMSO and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form a C2H5ONa (sodium ethoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0104] Example 13

[0105] The composite strong alkali solution for recycling carbon fiber provided in Example 13 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.1 g, the mass of ethanol is 1 g, and the mass of DMSO is 500 g.

[0106] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0107] Embodiment 14

[0108] The composite strong alkali solution for recycling carbon fiber provided in Example 14 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.1 g, the mass of ethanol is 1 g, and the mass of DMSO is 200 g.

[0109] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0110] Embodiment 15

[0111] The composite strong alkali solution for recycling carbon fiber provided in Example 15 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.1 g, the mass of ethanol is 1 g, and the mass of DMSO is 100 g.

[0112] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0113] Example 16

[0114] The composite strong alkali solution for recycling carbon fiber provided in Example 16 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.01 g, the mass of ethanol is 1 g, and the mass of DMSO is 500 g.

[0115] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0116] Embodiment 17

[0117] The composite strong alkali solution for recycling carbon fiber provided in Example 17 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.01 g, the mass of ethanol is 1 g, and the mass of DMSO is 800 g.

[0118] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0119] Embodiment 18

[0120] The composite strong alkali solution for recycling carbon fiber provided in Example 18 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.01 g, the mass of ethanol is 1 g, and the mass of DMSO is 1000 g.

[0121] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0122] Embodiment 19

[0123] The composite strong alkali solution for recycling carbon fiber provided in Example 19 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.25 g, the mass of ethanol is 1 g, and the mass of DMSO is 500 g.

[0124] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0125] Embodiment 20

[0126] The composite strong alkali solution for recycling carbon fiber provided in Example 20 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.25 g, the mass of ethanol is 1 g, and the mass of DMSO is 800 g.

[0127] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0128] Embodiment 21

[0129] The composite strong alkali solution for recycling carbon fiber provided in Example 21 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.25 g, the mass of ethanol is 1 g, and the mass of DMSO is 1000 g.

[0130] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / C2H5OH (ethanol) system reaction solution.

[0131] Embodiment 22

[0132] The composite strong alkali solution for recycling carbon fiber provided in Example 22 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a protonic auxiliary agent CH3OH (methanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.01 g, the mass of methanol is 1 g, and the mass of DMSO is 500 g.

[0133] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / methanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / CH3OH (methanol) system reaction solution.

[0134] Embodiment 23

[0135] The composite strong alkali solution for recycling carbon fiber provided in Example 23 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a protonic auxiliary agent CH3OH (methanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.1 g, the mass of methanol is 1 g, and the mass of DMSO is 200 g.

[0136] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / methanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / CH3OH (methanol) system reaction solution.

[0137] Embodiment 24

[0138] The composite strong alkali solution for recycling carbon fiber provided in Example 24 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMSO and a proton auxiliary compound alcohol; specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.1g, the mass of the compound alcohol is 1g (methanol:ethanol = 0.1~10), and the mass of DMSO is 200g.

[0139] The specific preparation method is: inject the corresponding mass of DMSO and potassium tert-butoxide / complex alcohol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMSO / complex alcohol system reaction solution.

[0140] Embodiment 25

[0141] The composite strong alkali solution for recycling carbon fiber provided in Example 25 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMF and a proton auxiliary agent CH3OH (methanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.1 g, the mass of methanol is 1 g, and the mass of DMF is 200 g.

[0142] The specific preparation method is: inject the corresponding mass of DMF and potassium tert-butoxide / methanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMF / CH3OH (methanol) system reaction solution.

[0143] Embodiment 26

[0144] The composite strong alkali solution for recycling carbon fiber provided in Example 26 of the present invention is composed of a mixture of a strong ionic base C4H9OK (potassium tert-butoxide), a non-protonic polar solvent DMF and a proton auxiliary agent C2H5OH (ethanol); specifically, the mass of the strong ionic base C4H9OK in the composite strong alkali solution is 0.01 g, the mass of ethanol is 1 g, and the mass of DMF is 200 g.

[0145] The specific preparation method is: inject the corresponding mass of DMF and potassium tert-butoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form a C4H9OK (potassium tert-butoxide) / DMF / C2H5OH (ethanol) system reaction solution.

[0146] Embodiment 27

[0147] The composite strong alkaline solution for recycling carbon fiber provided in Example 27 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMF and a protonic auxiliary agent C2H5OH (ethanol); specifically, a 20% EtONa solution (20gEtONa+100gEtOH) is mixed with a non-protonic polar solvent DMF organic solvent in a mass ratio of 1:50.

[0148] The specific preparation method is: inject the corresponding mass of DMF and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form the corresponding C2H5ONa (sodium ethoxide) / DMF / C2H5OH (ethanol) system reaction solution.

[0149] Embodiment 28

[0150] The composite strong alkaline solution for recycling carbon fiber provided in Example 28 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent DMF and a protonic auxiliary agent C2H5OH (ethanol); specifically, a 1% EtONa solution (1gEtONa+100gEtOH) is mixed with a non-protonic polar solvent DMF organic solvent in a mass ratio of 1:100.

[0151] The specific preparation method is: inject the corresponding mass of DMF and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let it stand for 1 minute to form the corresponding C2H5ONa (sodium ethoxide) / DMF / C2H5OH (ethanol) system reaction solution.

[0152] Embodiment 29

[0153] The composite strong alkaline solution for recycling carbon fiber provided in Example 29 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent NMP and a proton auxiliary agent C2H5OH (ethanol); specifically, a 20% EtONa solution (20gEtONa+100gEtOH) is mixed with a non-protonic polar solvent NMP organic solvent in a mass ratio of 1:50.

[0154] The specific preparation method is: inject the corresponding mass of NMP and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form the corresponding C2H5ONa (sodium ethoxide) / NMP / C2H5OH (ethanol) system reaction solution.

[0155] Embodiment 30

[0156] The composite strong alkaline solution for recycling carbon fiber provided in Example 30 of the present invention is composed of a mixture of a strong ionic base C2H5ONa (sodium ethoxide), a non-protonic polar solvent NMP and a proton auxiliary agent C2H5OH (ethanol); specifically, a 1% EtONa solution (1gEtONa+100gEtOH) is mixed with a non-protonic polar solvent DMF organic solvent in a mass ratio of 1:100.

[0157] The specific preparation method is: inject the corresponding mass of NMP and sodium ethoxide / ethanol solution into a glass reaction container in sequence, stir for 30 seconds to fully mix the two, and let stand for 1 minute to form the corresponding C2H5ONa (sodium ethoxide) / NMP / C2H5OH (ethanol) system reaction solution.

[0158] Embodiment 31

[0159] The composite strong alkali solution for recycling carbon fiber provided in Example 31 of the present invention is a mixture of a strong ion KOH alkali solution and a non-protonic polar DMSO solvent; the mass ratio of the strong ion KOH alkali solution to the non-protonic polar DMSO solvent is 0.05, and the concentration of the strong ion alkali solution is 0.01; specifically, the mass of the strong ion KOH alkali in the composite strong alkali solution is 0.03g, the mass of water is 2.97g, and the mass of the non-protonic polar DMSO is 60g.

[0160] Embodiment 32

[0161] The composite strong alkali solution for recovering carbon fiber provided in Example 32 of the present invention is a mixture of a strong ion KOH alkali solution and a non-protonic polar DMSO solvent; the mass ratio of the strong ion KOH alkali solution to the non-protonic polar DMSO solvent is 0.05, and the concentration of the strong ion alkali solution is 0.05; specifically, the mass of the strong ion KOH alkali in the composite strong alkali solution is 0.14g, the mass of water is 2.86g, and the mass of the non-protonic polar DMSO is 60g.

[0162] Embodiment 33

[0163] The composite strong alkali solution for recovering carbon fiber provided in Example 33 of the present invention is a mixture of a strong ion KOH alkali solution and a non-protonic polar DMSO solvent; the mass ratio of the strong ion KOH alkali solution to the non-protonic polar DMSO solvent is 0.05, and the concentration of the strong ion alkali solution is 0.1; specifically, the mass of the strong ion KOH alkali in the composite strong alkali solution is 0.27 g, the mass of water is 2.73 g, and the mass of the non-protonic polar DMSO is 60 g.

[0164] Embodiment 34

[0165] The composite strong alkali solution for recovering carbon fiber provided in Example 34 of the present invention is a mixture of a strong ion KOH alkali solution and a non-protonic polar DMSO solvent; the mass ratio of the strong ion KOH alkali solution to the non-protonic polar DMSO solvent is 0.05, and the concentration of the strong ion alkali solution is 0.3; specifically, the mass of the strong ion KOH alkali in the composite strong alkali solution is 0.69 g, the mass of water is 2.31 g, and the mass of the non-protonic polar DMSO is 60 g.

[0166] Embodiment 35

[0167] The composite strong alkali solution for recovering carbon fiber provided in Example 35 of the present invention is a mixture of a strong ion KOH alkali solution and a non-protonic polar DMSO solvent; the mass ratio of the strong ion KOH alkali solution to the non-protonic polar DMSO solvent is 0.05, and the concentration of the strong ion alkali solution is 0.5; specifically, the mass of the strong ion KOH alkali in the composite strong alkali solution is 1.00 g, the mass of water is 2.00 g, and the mass of the non-protonic polar DMSO is 60 g.

[0168] Embodiment 36

[0169] The composite strong alkali solution for recovering carbon fiber provided in Example 36 of the present invention is a mixture of a strong ion KOH alkali solution and a non-protonic polar DMSO solvent; the mass ratio of the strong ion KOH alkali solution to the non-protonic polar DMSO solvent is 0.05, and the concentration of the strong ion alkali solution is 0.8; specifically, the mass of the strong ion KOH alkali in the composite strong alkali solution is 1.33 g, the mass of water is 1.67 g, and the mass of the non-protonic polar DMSO is 60 g.

[0170] Embodiment 37

[0171] The composite strong alkali solution for recovering carbon fiber provided in Example 37 of the present invention is a mixture of a strong ion KOH alkali solution and a non-protonic polar DMSO solvent; the mass ratio of the strong ion KOH alkali solution to the non-protonic polar DMSO solvent is 0.05, and the concentration of the strong ion alkali solution is 1.1; specifically, the mass of the strong ion KOH alkali in the composite strong alkali solution is 1.57 g, the mass of water is 1.43 g, and the mass of the non-protonic polar DMSO is 60 g.

[0172] 2. Examples of CFRP recycling

[0173] The composite strong alkali solutions obtained in Examples 1, 2, 8, 14, 19, 20, 28, 33, 34, 35, 36 and 37 were respectively used to treat the specified carbon fiber reinforced composite materials (such as Figure 1a As shown) for dissolution recovery, the specific embodiments are described as follows.

[0174] Embodiment 38

[0175] The method for recycling a specified thermosetting carbon fiber prepreg provided in this embodiment 38 comprises the following specific steps:

[0176] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 1 of the present invention, and were allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1 L) deionized water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 38-1, 38-2, and 38-3.

[0177] Embodiment 39

[0178] The method for recycling a specified thermosetting carbon fiber prepreg provided in Example 39 comprises the following specific steps:

[0179] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 2 of the present invention, and were allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction was completed, the carbon fiber was taken out and soaked and washed with sufficient (1 L) deionized water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 39-1, 39-2, and 39-3.

[0180] Embodiment 40

[0181] The method for recycling a specified carbon fiber prepreg provided in this embodiment 40 comprises the following specific steps:

[0182] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 8 of the present invention, and were allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1 L) deionized water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 40-1, 40-2, and 40-3.

[0183] Embodiment 41

[0184] The method for recycling a specified thermosetting carbon fiber prepreg provided in this embodiment 41 comprises the following specific steps:

[0185] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 14 of the present invention, and were allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1L) deionized water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 41-1, 41-2, and 41-3.

[0186] Embodiment 42

[0187] The method for recycling a specified thermosetting carbon fiber prepreg provided in this embodiment 42 comprises the following specific steps:

[0188] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 19 of the present invention, and were allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1L) deionized water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 42-1, 42-2, and 42-3.

[0189] Embodiment 43

[0190] The method for recycling a specified thermosetting carbon fiber prepreg provided in Example 43 comprises the following specific steps:

[0191] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 20 of the present invention, and allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1L) water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recovered carbon fiber samples, which were respectively recorded as: 43-1, 43-2, and 43-3.

[0192] Embodiment 44

[0193] The method for recycling a specified thermosetting carbon fiber prepreg provided in Example 44 comprises the following specific steps:

[0194] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 28 of the present invention, and were allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction was completed, the carbon fiber was taken out and soaked and washed with sufficient (1L) deionized water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 44-1, 44-2, and 44-3.

[0195] Embodiment 45

[0196] The method for recycling a specified thermosetting carbon fiber prepreg provided in Example 45 comprises the following specific steps:

[0197] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 33 of the present invention, and allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1L) deionized water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 45-1, 45-2, and 45-3.

[0198] Embodiment 46

[0199] The method for recycling a specified thermosetting carbon fiber prepreg provided in Example 46 comprises the following specific steps:

[0200] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 34 of the present invention, and allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1L) water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 46-1, 46-2, and 46-3.

[0201] Embodiment 47

[0202] The method for recycling a specified carbon fiber prepreg provided in Example 47 comprises the following specific steps:

[0203] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 35 of the present invention, and allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1L) deionized water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 47-1, 47-2, and 47-3.

[0204] Embodiment 48

[0205] The method for recycling a specified thermosetting carbon fiber prepreg provided in Example 48 comprises the following specific steps:

[0206] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 36 of the present invention, and allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1L) water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 48-1, 48-2, and 48-3.

[0207] Embodiment 49

[0208] The method for recycling a specified thermosetting carbon fiber prepreg provided in Example 49 comprises the following specific steps:

[0209] At normal pressure and room temperature (25°C), three groups of carbon fiber prepregs were placed in the composite strong alkali solution obtained in Example 37 of the present invention, and allowed to react for 20 min, 30 min, and 40 min, respectively. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient (1L) deionized water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 49-1, 49-2, and 49-3.

[0210] In addition, during the recycling process, the resin is degraded in the reaction solution, the carbon fiber and the resin are separated, and the carbon fiber is taken out after reaching the set reaction time to obtain the carbon fiber (such as Figure 1b ) and a reaction solution containing resin degradation products (such as Figure 1c shown).

[0211] The composite strong alkali solutions obtained in Examples 1, 2, 8, 14, 19, 20, 28, 33, 34, 35, 36 and 37 were respectively used to treat bisphenol A epoxy resin CFRP (such as Figure 2a As shown) for dissolution recovery, the specific embodiments are described as follows.

[0212] Embodiment 50

[0213] The method for recovering bisphenol A epoxy resin CFRP provided in this embodiment 50 comprises the following specific steps:

[0214] Three groups of bisphenol A epoxy resin CFRP were placed in the composite strong alkali solution obtained in Example 1 of the present invention at normal pressure and 140°C, 160°C and 180°C, respectively, and reacted for 3 hours under magnetic stirring. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient amount (1L) of water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 50-1, 50-2, 50-3.

[0215] Embodiment 51

[0216] The method for recycling bisphenol A epoxy resin CFRP provided in Example 51 comprises the following specific steps:

[0217] Three groups of bisphenol A epoxy resin CFRP were placed in the composite strong alkali solution obtained in Example 2 of the present invention at normal pressure and 140°C, 160°C and 180°C, respectively, and reacted for 3 hours under magnetic stirring. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient amount (1L) of water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 51-1, 51-2, 51-3.

[0218] Examples 52-61 are all for recycling bisphenol A epoxy resin CFRP. The difference from Example 50 is that different composite strong alkali solutions are used. The specific differences are:

[0219] The composite strong alkali solution used in Example 52 is the composite strong alkali solution obtained in Example 8, and the recovered carbon fiber samples are respectively recorded as: 52-1, 52-2, 52-3;

[0220] The composite strong alkali solution used in Example 53 is the composite strong alkali solution obtained in Example 14, and the recovered carbon fiber samples are respectively recorded as: 53-1, 53-2, 53-3;

[0221] The composite strong alkali solution used in Example 54 is the composite strong alkali solution obtained in Example 19, and the recovered carbon fiber samples are respectively recorded as: 54-1, 54-2, 54-3;

[0222] The composite strong alkali solution used in Example 55 is the composite strong alkali solution obtained in Example 20, and the recovered carbon fiber samples are respectively recorded as: 55-1, 55-2, 55-3;

[0223] The composite strong alkali solution used in Example 56 is the composite strong alkali solution obtained in Example 28, and the recovered carbon fiber samples are respectively recorded as: 56-1, 56-2, 56-3;

[0224] The composite strong alkali solution used in Example 57 is the composite strong alkali solution obtained in Example 33, and the recovered carbon fiber samples are respectively recorded as: 57-1, 57-2, 57-3;

[0225] The composite strong alkali solution used in Example 58 is the composite strong alkali solution obtained in Example 34, and the recovered carbon fiber samples are respectively recorded as: 58-1, 58-2, 58-3;

[0226] The composite strong alkali solution used in Example 59 is the composite strong alkali solution obtained in Example 35, and the recovered carbon fiber samples are respectively recorded as: 59-1, 59-2, 59-3;

[0227] The composite strong alkali solution used in Example 60 is the composite strong alkali solution obtained in Example 36, and the recovered carbon fiber samples are respectively recorded as: 60-1, 60-2, 60-3;

[0228] The composite strong alkali solution used in Example 61 is the composite strong alkali solution obtained in Example 37, and the recovered carbon fiber samples are respectively recorded as: 61-1, 61-2, 61-3;

[0229] In addition, during the recycling process, the resin is degraded in the reaction solution, the carbon fiber and the resin are separated, and the carbon fiber is taken out after reaching the set reaction time to obtain the carbon fiber (such as Figure 2b ) and a reaction solution containing resin degradation products.

[0230] The composite strong alkali solutions obtained in Examples 1, 2, 8, 14, 19, 20, 28, 33, 34, 35, 36 and 37 were respectively used to treat unsaturated polyester resin CFRP (such as Figure 3a As shown) for dissolution recovery, the specific embodiments are described as follows.

[0231] Embodiment 62

[0232] The method for recovering unsaturated polyester resin CFRP provided in Example 62 comprises the following specific steps:

[0233] Three groups of unsaturated polyester resin CFRP were placed in the composite strong alkali solution obtained in Example 1 of the present invention at normal pressure and 140°C, 160°C and 180°C, respectively, and reacted for 3 hours under magnetic stirring. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient amount (1L) of water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 62-1, 62-2, 62-3.

[0234] Examples 63-73 are all about recycling unsaturated polyester resin CFRP. The difference from Example 62 is that different composite strong alkali solutions are used. The specific differences are:

[0235] The composite strong alkali solution used in Example 63 is the composite strong alkali solution obtained in Example 2, and the recovered carbon fiber samples are respectively recorded as: 63-1, 63-2, 63-3;

[0236] The composite strong alkali solution used in Example 64 is the composite strong alkali solution obtained in Example 8, and the recovered carbon fiber samples are respectively recorded as: 64-1, 64-2, 64-3;

[0237] The composite strong alkali solution used in Example 65 is the composite strong alkali solution obtained in Example 14, and the recovered carbon fiber samples are respectively recorded as: 65-1, 65-2, 65-3;

[0238] The composite strong alkali solution used in Example 66 is the composite strong alkali solution obtained in Example 19, and the recovered carbon fiber samples are respectively recorded as: 66-1, 66-2, 66-3;

[0239] The composite strong alkali solution used in Example 67 is the composite strong alkali solution obtained in Example 20, and the recovered carbon fiber samples are respectively recorded as: 67-1, 67-2, 67-3;

[0240] The composite strong alkali solution used in Example 68 is the composite strong alkali solution obtained in Example 28, and the recovered carbon fiber samples are respectively recorded as: 68-1, 68-2, 68-3;

[0241] The composite strong alkali solution used in Example 69 is the composite strong alkali solution obtained in Example 33, and the recovered carbon fiber samples are respectively recorded as: 69-1, 69-2, 69-3;

[0242] The composite strong alkali solution used in Example 70 is the composite strong alkali solution obtained in Example 34, and the recovered carbon fiber samples are respectively recorded as: 70-1, 70-2, 70-3;

[0243] The composite strong alkali solution used in Example 71 is the composite strong alkali solution obtained in Example 35, and the recovered carbon fiber samples are respectively recorded as: 71-1, 71-2, 71-3;

[0244] The composite strong alkali solution used in Example 72 is the composite strong alkali solution obtained in Example 36, and the recovered carbon fiber samples are respectively recorded as: 72-1, 72-2, 73-3;

[0245] The composite strong alkali solution used in Example 73 is the composite strong alkali solution obtained in Example 37, and the recovered carbon fiber samples are respectively recorded as: 73-1, 73-2, 73-3;

[0246] In addition, during the recycling process, the resin is degraded in the reaction solution, the carbon fiber and the resin are separated, and the carbon fiber is taken out after reaching the set reaction time to obtain the carbon fiber (such as Figure 3b ) and a reaction solution containing resin degradation products.

[0247] The composite strong alkali solutions obtained in Examples 1, 2, 8, 14, 19, 20, 28, 33, 34, 35, 36 and 37 were respectively used to treat epoxy vinyl ester resin CFRP (such as Figure 4a As shown) for dissolution recovery, the specific embodiments are described as follows.

[0248] Embodiment 74

[0249] The method for recycling epoxy vinyl ester resin CFRP provided in Example 74 comprises the following specific steps:

[0250] Three groups of epoxy vinyl ester resin CFRP were placed in the composite strong alkali solution obtained in Example 1 of the present invention at normal pressure and 140°C, 160°C and 180°C, respectively, and reacted for 3 hours under magnetic stirring. After the reaction was completed, the carbon fiber was taken out and soaked and washed with sufficient amount (1L) of water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 74-1, 74-2, 74-3.

[0251] Examples 75-85 are all for recycling epoxy vinyl ester resin CFRP, and the difference from Example 74 is that different composite strong alkali solutions are used. The specific differences are:

[0252] The composite strong alkali solution used in Example 75 is the composite strong alkali solution obtained in Example 2, and the recovered carbon fiber samples are respectively recorded as: 75-1, 75-2, 75-3;

[0253] The composite strong alkali solution used in Example 76 is the composite strong alkali solution obtained in Example 8, and the recovered carbon fiber samples are respectively recorded as: 76-1, 76-2, 76-3;

[0254] The composite strong alkali solution used in Example 77 is the composite strong alkali solution obtained in Example 14, and the recovered carbon fiber samples are respectively recorded as: 77-1, 77-2, 77-3;

[0255] The composite strong alkali solution used in Example 78 is the composite strong alkali solution obtained in Example 19, and the recovered carbon fiber samples are respectively recorded as: 78-1, 78-2, 78-3;

[0256] The composite strong alkali solution used in Example 79 is the composite strong alkali solution obtained in Example 20, and the recovered carbon fiber samples are respectively recorded as: 79-1, 79-2, 79-3;

[0257] The composite strong alkali solution used in Example 80 is the composite strong alkali solution obtained in Example 28, and the recovered carbon fiber samples are respectively recorded as: 80-1, 80-2, 80-3;

[0258] The composite strong alkali solution used in Example 69 is the composite strong alkali solution obtained in Example 33, and the recovered carbon fiber samples are respectively recorded as: 81-1, 81-2, 81-3;

[0259] The composite strong alkali solution used in Example 70 is the composite strong alkali solution obtained in Example 34, and the recovered carbon fiber samples are respectively recorded as: 82-1, 82-2, 83-3;

[0260] The composite strong alkali solution used in Example 71 is the composite strong alkali solution obtained in Example 35, and the recovered carbon fiber samples are respectively recorded as: 83-1, 83-2, 83-3;

[0261] The composite strong alkali solution used in Example 72 is the composite strong alkali solution obtained in Example 36, and the recovered carbon fiber samples are respectively recorded as: 84-1, 84-2, 84-3;

[0262] The composite strong alkali solution used in Example 73 is the composite strong alkali solution obtained in Example 37, and the recovered carbon fiber samples are respectively recorded as: 85-1, 85-2, 85-3;

[0263] In addition, during the recycling process, the resin is degraded in the reaction solution, the carbon fiber and the resin are separated, and the carbon fiber is taken out after reaching the set reaction time to obtain the carbon fiber (such as Figure 4b ) and a reaction solution containing resin degradation products.

[0264] The composite strong alkali solutions obtained in Examples 1, 2, 8, 14, 19, 20, 28, 33, 34, 35, 36 and 37 were respectively used to treat phenolic resin CFRP (such as Figure 5a As shown) for dissolution recovery, the specific embodiments are described as follows.

[0265] Embodiment 86

[0266] The method for recovering phenolic resin CFRP provided in Example 80 comprises the following specific steps:

[0267] Three groups of phenolic resin CFRP were placed in the composite strong alkali solution obtained in Example 1 of the present invention at normal pressure and 140°C, 160°C and 180°C, respectively, and reacted for 3 hours under magnetic stirring. After the reaction, the carbon fiber was taken out and soaked and washed with sufficient amount (1L) of water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 86-1, 86-2, 86-3.

[0268] Examples 87-97 are all about recycling phenolic resin CFRP. The difference from Example 86 is that different composite strong alkali solutions are used. The specific differences are:

[0269] The composite strong alkali solution used in Example 87 is the composite strong alkali solution obtained in Example 2, and the recovered carbon fiber samples are respectively recorded as: 87-1, 87-2, 87-3;

[0270] The composite strong alkali solution used in Example 88 is the composite strong alkali solution obtained in Example 8, and the recovered carbon fiber samples are respectively recorded as: 88-1, 88-2, 88-3;

[0271] The composite strong alkali solution used in Example 89 is the composite strong alkali solution obtained in Example 14, and the recovered carbon fiber samples are respectively recorded as: 89-1, 89-2, 89-3;

[0272] The composite strong alkali solution used in Example 90 is the composite strong alkali solution obtained in Example 19, and the recovered carbon fiber samples are respectively recorded as: 90-1, 90-2, 90-3;

[0273] The composite strong alkali solution used in Example 91 is the composite strong alkali solution obtained in Example 20, and the recovered carbon fiber samples are respectively recorded as: 91-1, 91-2, 91-3;

[0274] The composite strong alkali solution used in Example 92 is the composite strong alkali solution obtained in Example 28, and the recovered carbon fiber samples are respectively recorded as: 92-1, 92-2, 92-3;

[0275] The composite strong alkali solution used in Example 93 is the composite strong alkali solution obtained in Example 33, and the recovered carbon fiber samples are respectively recorded as: 93-1, 93-2, 93-3;

[0276] The composite strong alkali solution used in Example 94 is the composite strong alkali solution obtained in Example 34, and the recovered carbon fiber samples are respectively recorded as: 94-1, 94-2, 94-3;

[0277] The composite strong alkali solution used in Example 95 is the composite strong alkali solution obtained in Example 35, and the recovered carbon fiber samples are respectively recorded as: 95-1, 95-2, 95-3;

[0278] The composite strong alkali solution used in Example 96 is the composite strong alkali solution obtained in Example 36, and the recovered carbon fiber samples are respectively recorded as: 96-1, 96-2, 96-3;

[0279] The composite strong alkali solution used in Example 97 is the composite strong alkali solution obtained in Example 37, and the recovered carbon fiber samples are respectively recorded as: 97-1, 97-2, 97-3;

[0280] In addition, during the recycling process, the resin is degraded in the reaction solution, the carbon fiber and the resin are separated, and the carbon fiber is taken out after reaching the set reaction time to obtain the carbon fiber (such as Figure 5b ) and a reaction solution containing resin degradation products.

[0281] The composite strong alkali solutions obtained in Examples 1, 2, 8, 14, 19, 20, 28, 33, 34, 35, 36 and 37 were respectively used to treat bismaleimide resin CFRP (such as Figure 6aAs shown) for dissolution recovery, the specific embodiments are described as follows.

[0282] Embodiment 98

[0283] The method for recycling bismaleimide resin CFRP provided in Example 98 comprises the following specific steps:

[0284] Three groups of phenolic resin CFRP were placed in the composite strong alkali solution obtained in Example 1 of the present invention at normal pressure and 140°C, 160°C and 180°C, respectively, and reacted for 3 hours under magnetic stirring. After the reaction was completed, the carbon fiber was taken out and soaked and washed with sufficient amount (1L) of water for 5 times. After washing, it was dried in an oven at 30°C for 48 hours to obtain recycled carbon fiber samples, which were respectively recorded as: 98-1, 98-2, 98-3.

[0285] Examples 99-109 are all about recycling bismaleimide resin CFRP. The difference from Example 98 is that different composite strong alkali solutions are used. The specific differences are:

[0286] The composite strong alkali solution used in Example 99 is the composite strong alkali solution obtained in Example 2, and the recovered carbon fiber samples are respectively recorded as: 99-1, 99-2, and 99-3;

[0287] The composite strong alkali solution used in Example 100 is the composite strong alkali solution obtained in Example 8, and the recovered carbon fiber samples are respectively recorded as: 100-1, 100-2, 100-3;

[0288] The composite strong alkali solution used in Example 101 is the composite strong alkali solution obtained in Example 14, and the recovered carbon fiber samples are respectively recorded as: 101-1, 101-2, 101-3;

[0289] The composite strong alkali solution used in Example 102 is the composite strong alkali solution obtained in Example 19, and the recovered carbon fiber samples are respectively recorded as: 102-1, 102-2, 102-3;

[0290] The composite strong alkali solution used in Example 103 is the composite strong alkali solution obtained in Example 20, and the recovered carbon fiber samples are respectively recorded as: 103-1, 103-2, 103-3;

[0291] The composite strong alkali solution used in Example 104 is the composite strong alkali solution obtained in Example 28, and the recovered carbon fiber samples are respectively recorded as: 104-1, 104-2, 104-3;

[0292] The composite strong alkali solution used in Example 105 is the composite strong alkali solution obtained in Example 33, and the recovered carbon fiber samples are respectively recorded as: 105-1, 105-2, 105-3;

[0293] The composite strong alkali solution used in Example 106 is the composite strong alkali solution obtained in Example 34, and the recovered carbon fiber samples are respectively recorded as: 106-1, 106-2, 106-3;

[0294] The composite strong alkali solution used in Example 107 is the composite strong alkali solution obtained in Example 35, and the recovered carbon fiber samples are respectively recorded as: 107-1, 107-2, 107-3;

[0295] The composite strong alkali solution used in Example 108 is the composite strong alkali solution obtained in Example 36, and the recovered carbon fiber samples are respectively recorded as: 108-1, 108-2, 108-3;

[0296] The composite strong alkali solution used in Example 109 is the composite strong alkali solution obtained in Example 37, and the recovered carbon fiber samples are respectively recorded as: 109-1, 109-2, 109-3;

[0297] In addition, during the recycling process, the resin is degraded in the reaction solution, the carbon fiber and the resin are separated, and the carbon fiber is taken out after reaching the set reaction time to obtain the carbon fiber (such as Figure 6b ) and a reaction solution containing resin degradation products.

[0298] 3. Experimental example on performance testing of recycled carbon fiber

[0299] In order to verify the recovery effect of the composite strong alkali solution obtained in the present invention on CFRP, the carbon fiber samples recovered in Examples 38-99 were subjected to a TGA test for fat removal rate analysis, and the tensile strength and shear strength of the recycled carbon fiber were tested. The specific data are shown in Table 3 below.

[0300] Table 3 shows the performance results of the carbon fiber samples obtained in Examples 38-99

[0301]

[0302]

[0303]

[0304]

[0305]

[0306]

[0307]

[0308] According to the standard ISO 14127:2008 Carbon-fibre-reinforced composites—Determination of the resin, fiber and void contents, the carbon fiber degreasing rate obtained in Examples 38 to 99 was tested, with 3 effective parallel test pieces for each working condition.

[0309] According to ISO 11566:1996 Carbon fibre—Determination of the tensile properties of single-filament specimens, the tensile strength of the carbon fiber single filaments obtained in Examples 38 to 109 was tested, with 20 effective parallel specimens for each working condition.

[0310] According to the single fiber droplet embedding and pulling method, for the carbon fiber interfacial shear strength obtained in Examples 38 to 109, there were 5 valid parallel specimens for each working condition.

[0311] In addition, the internal structure, surface microstructure and chemical composition of the recycled carbon fibers were characterized. Scanning electron microscopy (SEM) analysis results showed that the surface of the recycled carbon fibers was uniform; atomic force microscopy (AFM) analysis results showed that the nanoscale microstructure on the surface of the recycled carbon fibers increased and the surface roughness improved; X-ray diffraction (XRD) analysis results showed that the internal crystal structure of the recycled carbon fibers was refined; X-ray photoelectron spectroscopy (XPS) analysis results showed that the content of oxygen-containing functional groups on the surface of the recycled carbon fibers increased and the surface hydrophilicity was enhanced; based on the above multiple effects, the mechanical properties of the recycled carbon fibers, such as tensile properties and interface shear properties, are improved compared with the original fibers.

[0312] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A carbon fiber recycling method, characterized in that: The method specifically comprises the following steps: S1. Immerse the carbon fiber reinforced composite material in a composite strong alkali solution and react for 20 to 180 minutes to obtain a crude carbon fiber product and a reaction solution; the composite strong alkali solution is a mixture of a strong ionic alkali solution, a non-protonic polar solvent and a protonic additive; the mass ratio of the strong ionic alkali solution to the non-protonic polar solvent is 0.05 to 0.2, and the concentration of the strong ionic alkali solution is 1 to 120 wt.%; the mass ratio of the strong ionic alkali solution to the protonic additive is 0.01 to 1.2; the mass ratio of the protonic additive to the non-protonic polar solvent is 1 to 25 wt.%; S2. Washing and drying the crude carbon fiber obtained in S1 to obtain recycled carbon fiber.

2. The carbon fiber recycling method according to claim 1, characterized in that: In S1, the carbon fiber reinforced composite material is immersed in the composite strong alkali solution at normal pressure and 25-180°C.

3. The carbon fiber recovery method according to claim 1 or 2, characterized in that: In S1, the carbon fiber reinforced composite material includes thermosetting carbon fiber prepreg, bisphenol A epoxy resin carbon fiber reinforced composite material, unsaturated polyester resin carbon fiber reinforced composite material, epoxy vinyl ester resin carbon fiber reinforced composite material, phenolic resin carbon fiber reinforced composite material, bismaleimide resin carbon fiber reinforced composite material.

4. The carbon fiber recycling method according to claim 3, characterized in that: The strong ionic alkaline solution is at least one of EtONa, EtOK, NaOBu-t, KOBu-t, NaOH, and KOH; and the aprotic polar solvent is at least one of DMF, THF, and DMSO.

5. The carbon fiber recycling method according to claim 4, characterized in that: The proton auxiliary agent is at least one of water, methanol and ethanol.

6. The carbon fiber recycling method according to claim 3, characterized in that: In S2, the crude carbon fiber product is washed with a cleaning liquid.

7. The carbon fiber recovery method according to claim 6, characterized in that: In S2, the drying temperature is 20 to 80°C, and the drying time is 5 to 40 hours.

Citation Information

Cited By

  • Degradation method of amine cured epoxy resin

    CN122356576A