Biosensor based on bovine serum albumin-polyethyleneimine material

By covalently crosslinking bovine serum albumin and polyethyleneimine to MXene modified glass carbon electrodes and connecting them with DNA aptamers, a stable anti-pollution electrochemical biosensor was constructed, solving BSA at the interface The stability issues on the surface have achieved high sensitivity detection and improvement of anti-pollution performance for CA125.

CN117147654BActive Publication Date: 2024-12-06QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311121531.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-31
Publication Date
2024-12-06
Estimated Expiration
2043-08-31

AI Technical Summary

Technical Problem

In the prior art, bovine serum albumin (BSA) has poor physical adsorption stability at the biosensor interface, hindering charge transfer on the electrode surface and limiting the anti-pollution performance and sensitivity of the interface.

Method used

A stable anti-pollution electrochemical biosensor was constructed by covalently crosslinking bovine serum albumin with polyethyleneimine (PEI) onto a glass carbon electrode modified with MXene and covalently connecting it with DNA aptamers. .

Benefits of technology

The specific, simple and accurate detection of the cancer marker CA125 in real samples is achieved, which significantly improves the anti-pollution performance and sensitivity. It has better anti-pollution performance and higher detection sensitivity than a single BSA modified interface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117147654B_ABST
    Figure CN117147654B_ABST
Patent Text Reader

Abstract

The present invention provides a biosensor based on bovine serum albumin-polyethyleneimine material, which relates to the technical field of electrochemical detection. The biosensor comprises a BSA solution, a PEI solution, a nanomaterial MXene and a DNA aptamer. The BSA solution and the PEI solution are covalently cross-linked to a glassy carbon electrode modified with a conductive nanomaterial MXene, and then covalently linked to the DNA aptamer to prepare a sensor. The excellent conductivity of MXene and the excellent performance of a bovine serum albumin-polyethyleneimine cross-linked coating are integrated. The sensor prepared by the present invention can effectively resist unnecessary biological contamination, and achieve specific, simple, sensitive and accurate detection of a cancer marker CA125 in a real sample. Experimental verification shows that an interface modified by a bovine serum albumin-polyethyleneimine cross-linked coating has more excellent anti-pollution performance and higher sensitivity than an interface modified by a single bovine serum albumin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochemical detection, in particular to a biosensor based on bovine serum albumin-polyethyleneimine material. Background Art

[0002] Electrochemical sensing technology has shown great potential in the detection of disease biomarkers due to its superior properties such as fast response, low cost, simple preparation and sensitive detection. However, in actual use, the contamination problem existing in biological fluids poses a huge threat to its detection accuracy, stability and sensitivity. Therefore, the search for anti-pollution materials with excellent performance to construct effective anti-pollution sensing interfaces has attracted great attention in recent years. Commonly used anti-pollution materials that have been discovered include polyethylene glycol (PEG) and its derivatives, zwitterionic polymers and anti-pollution peptides, but these materials still have problems such as poor stability and complex synthesis.

[0003] In recent years, the anti-fouling properties of protein-based materials have attracted people's attention. Among them, natural bovine serum albumin (BSA) has been widely used in biochemical experiments due to its advantages such as low cost, high abundance and good biocompatibility. For example, natural BSA protein can be anchored on the surface of the material as a blocking agent, and it can also be used as a passivating agent at the sensing interface to block the active sites and prevent the adsorption of nonspecific proteins to a certain extent.

[0004] In the prior art, the BSA protein physically adsorbed on the interface has poor stability and will seriously hinder the charge transfer on the electrode surface, limiting the anti-pollution performance and sensitivity of the interface. The BSA protein-modified interface exhibits strong negative charge and a certain degree of hydrophobicity, which also limits the anti-pollution performance of the interface and is not conducive to the preparation and use of actual biosensors. Summary of the invention

[0005] Technical issues solved

[0006] In view of the shortcomings of the prior art, the present invention provides a biosensor based on bovine serum albumin-polyethyleneimine material, which solves the problems of limited anti-pollution performance of a single protein and hindering interfacial electron transfer.

[0007] Technical Solution

[0008] To achieve the above objectives, the present invention is implemented by the following technical scheme: a biosensor based on bovine serum albumin-polyethyleneimine material, including a BSA solution, a PEI solution, a nanomaterial MXene and a DNA aptamer, wherein the BSA solution and the PEI solution are covalently cross-linked to a glassy carbon electrode modified with a conductive nanomaterial MXene, and then covalently linked to a DNA aptamer to obtain a sensor, and the preparation method of the sensor is as follows:

[0009] Sp1: Electrode pretreatment: After the prepared MXene is evenly mixed with the CS solution, it is drop-coated on the pretreated bare glassy carbon electrode and dried naturally at room temperature to obtain a MXene-CS modified electrode;

[0010] Sp2: Preparation of BSA-PEI / MXene-CS modified electrode, the MXene-CS modified electrode is activated by glutaraldehyde, and then immersed in a mixed solution of BSA and PEI to obtain a BSA-PEI / MXene-CS modified electrode;

[0011] Sp3: Molding preparation of the sensor: the BSA-PEI / MXene-CS modified electrode is immersed in a DNA aptamer solution activated by an EDC / NHS solution to obtain a sensor.

[0012] Preferably, during the electrode pretreatment process, 8 mg of Ti3AlC2 powder is slowly added to a 32 mL hydrofluoric acid solution with a mass fraction of 40%, and continuously stirred at high speed for 48 h at room temperature. The material is then repeatedly washed with secondary water and anhydrous ethanol and centrifuged until the supernatant reaches a pH ≥ 6. The precipitate is then vacuum dried at 60 ° C for 12 h to obtain Ti3C2T x MXene powder was dissolved by ultrasonic treatment in secondary water and then mixed evenly with 0.2% CS solution in a volume ratio of 1:2. Then 20 μL was drop-coated on the pretreated bare glassy carbon electrode and dried naturally at room temperature.

[0013] Preferably, in the preparation of the BSA-PEI / MXene-CS modified electrode, the amino groups on the MXene-CS modified electrode are activated with 5% glutaraldehyde for 50 minutes, and then immersed in a mixed solution of BSA and PEI, and reacted at room temperature for 16 hours. After the reaction, it is rinsed with water twice to remove the BSA-PEI that is not covalently cross-linked, thereby obtaining a BSA-PEI / MXene-CS modified electrode.

[0014] Preferably, in the molding preparation of the sensor, the carboxyl group on the DNA aptamer is first activated with an EDC / NHS solution for 0.5 h, and then the BSA-PEI / MXene-CS modified electrode is immersed in a DNA aptamer solution of not less than 1 μM and reacted at room temperature for 2 h. After the reaction is completed, it is rinsed with secondary water to remove the unfixed DNA aptamer to obtain the sensor.

[0015] Preferably, in the mixed solution of BSA and PEI used in the preparation of the BSA-PEI / MXene-CS modified electrode, the concentration of BSA is 1 mg / mL, and the mass percentage of PEI is 3 wt%.

[0016] Preferably, the BSA solution and the PEI solution are bovine serum albumin solution and polyethyleneimine solution respectively, and the CS solution is a chitosan solution.

[0017] Beneficial Effects

[0018] The present invention provides a biosensor based on bovine serum albumin-polyethyleneimine material. It has the following beneficial effects:

[0019] The present invention adopts the method of covalently cross-linking bovine serum albumin-polyethyleneimine to a glassy carbon electrode modified with MXene, and then covalently linking a DNA aptamer to construct a stable anti-pollution electrochemical biosensor, which integrates the excellent conductivity of MXene and the excellent performance of the bovine serum albumin-polyethyleneimine cross-linked coating. The sensor prepared by the present invention can effectively resist unnecessary biological contamination, and achieve specific, simple, sensitive and accurate detection of the cancer marker CA125 in real samples. It has been verified by experiments that the interface modified by the bovine serum albumin-polyethyleneimine cross-linked coating has better anti-pollution performance and higher sensitivity than the interface modified by a single bovine serum albumin. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The figure is a schematic diagram of the construction process of the biosensor of the present invention and the detection process of the target CA125;

[0021] Figure 2 Scanning electron microscope images of different modified electrodes provided by embodiments of the present invention;

[0022] Figure 3 Full scan X-ray photoelectron spectra of different modified electrodes provided in the embodiments of the present invention;

[0023] Figure 4 The zeta potential data graph of BSA, PEI and BSA-PEI provided in the embodiments of the present invention;

[0024] Figure 5 Water contact angle diagrams of different modified interfaces provided by embodiments of the present invention;

[0025] Figure 6 DPV response curves of different working electrodes provided in the embodiments of the present invention;

[0026] Figure 7 Anti-pollution DPV test diagram of different modified electrodes provided in the embodiments of the present invention in human serum with different concentrations;

[0027] Figure 8 A bar graph comparing the anti-pollution performance of different modified electrodes provided in an embodiment of the present invention in human serum of different concentrations;

[0028] Fig. 9 Laser confocal images of different modified interfaces provided in the embodiments of the present invention after being incubated in 0.2 mg / mL fluorescent protein for 2 hours and co-cultured with cells for 24 hours;

[0029] Fig.10 DPV response diagram (a) and linear curve (b) of the sensor provided in an embodiment of the present invention to different concentrations of CA125;

[0030] Fig.11 A specificity test diagram of a biosensor provided in an embodiment of the present invention;

[0031] Fig.12 A stability test diagram of the biosensor provided in an embodiment of the present invention;

[0032] Fig.13 A reproducibility test diagram of the biosensor provided in an embodiment of the present invention;

[0033] Fig.14 A bar graph comparing the analytical performance of the detection method provided by the embodiment of the present invention and the ELISA detection method;

[0034] Fig.15 PEI concentration optimization diagram provided in an embodiment of the present invention (signal change of the modified electrode immersed in 20% human serum for 30 minutes);

[0035] Fig.16 This is a BSA concentration optimization diagram provided in an embodiment of the present invention (signal change of the modified electrode immersed in 20% human serum for 30 minutes);

[0036] Fig.17 The cross-linking time optimization diagram of the BSA-PEI coating provided in the embodiment of the present invention (the signal change of the modified electrode immersed in 20% human serum for 30 minutes);

[0037] Fig.18 A diagram showing the optimization of DNA aptamer concentration provided by an embodiment of the present invention;

[0038] Fig.19 This is a diagram for optimizing the incubation time of a target object provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Specific embodiment one:

[0041] like Figure 1-19 As shown, a biosensor based on bovine serum albumin-polyethyleneimine material includes a BSA solution, a PEI solution, a nanomaterial MXene and a DNA aptamer. The BSA solution and the PEI solution are covalently cross-linked to a glassy carbon electrode modified with a conductive nanomaterial MXene, and then covalently linked to a DNA aptamer to obtain a sensor. The preparation method of the sensor is as follows:

[0042] Sp1: Electrode pretreatment: Before the interface modification of the glassy carbon electrode, the interface was polished with alumina powder with a particle size of 0.3 μm and 0.05 μm, respectively, and then ultrasonically cleaned with water, anhydrous ethanol, and water for 1-2 minutes respectively;

[0043] Preparation of Sp2: BSA-PEI / MXene-CS modified electrode, 8 mg Ti3AlC2 powder was slowly added into 32 mL of hydrofluoric acid solution with a mass fraction of 40%, and stirred continuously at room temperature for 48 h. After that, the material was repeatedly washed with water and anhydrous ethanol and centrifuged until the supernatant reached pH ≥ 6. Then, the precipitate was vacuum dried at 60 ° C for 12 h to obtain Ti3C2T x MXene powder was ultrasonically dissolved in secondary water and uniformly mixed with 0.2% CS solution in a volume ratio of 1:2. Then 20 μL was drop-coated on the pretreated bare glassy carbon electrode and dried naturally at room temperature. Then, the amino groups on the MXene-CS modified electrode were activated with 5% glutaraldehyde for 50 min, and then immersed in a mixed solution of BSA and PEI for reaction at room temperature for 16 h. After the reaction, it was rinsed with secondary water to remove the non-covalently cross-linked BSA-PEI, thus obtaining a BSA-PEI / MXene-CS modified electrode.

[0044] Sp3: The molding preparation of the sensor, first use EDC / NHS solution to activate the carboxyl group on the DNA aptamer for 0.5h, then immerse the BSA-PEI / MXene-CS modified electrode in a DNA aptamer solution of not less than 1μM, react at room temperature for 2h, after the reaction is completed, rinse with secondary water to remove the unfixed DNA aptamer, and obtain an anti-pollution sensor.

[0045] In the process of sensor preparation, the instruments used were CHI650E electrochemical workstation for electrochemical testing and characterization, a traditional three-electrode system with a glassy carbon electrode as the working electrode, a saturated calomel electrode as the reference electrode and a platinum wire as the counter electrode. A Hitachi S-4800 scanning electron microscope was used to characterize the surface morphology of different modified interfaces, an ESCALAB250Xi spectrometer was used to perform X-ray photoelectron spectroscopy analysis of different modified interfaces, a JC2000D1 water contact angle meter was used to characterize the surface wettability of different modified interfaces, Zeta potential measurements were performed on a ZETASIZERNano-ZS, and nonspecific adsorption tests of fluorescently labeled proteins and cells were performed on a TCSSP5 confocal laser microscope.

[0046] The reagents and materials used and their sources are as follows: Ti3AlC2 powder with a mass fraction of 98% and a particle size of 200 mesh was purchased from Forsman Technology Co., Ltd., hydrofluoric acid with a mass percentage of 40wt% was purchased from Adamas Reagent Co., Ltd., branched polyethyleneimine PEI, with an average Mw of 25,000Da measured by LS and an average Mn of 10,000Da measured by GPC was purchased from Sigma, chitosan (CS), glutaraldehyde (GA), and N-hydroxysuccinimide (NHS) were all from MacLean Biochemical Co., Ltd., and 1-(3-dihydropyridine) was purchased from Sigma. (Methylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) was from Bidex Pharmaceuticals, bovine serum albumin (BSA) and fluorescein isothiocyanate-labeled BSA (FITC-BSA) were purchased from Adamas Reagents, Inc., carbohydrate antigen 125 (CA125), CA125 aptamer and fluorescein diacetate (FDA) were purchased from Sangon Biotechnology, Inc. All reagents were of analytical grade, and ultrapure water was used in all experiments. The water purification system was provided by Milli-Q Water Systems, Bedford, Massachusetts, USA.

[0047] A stable anti-pollution electrochemical biosensor was constructed by covalently cross-linking bovine serum albumin-polyethyleneimine to a glassy carbon electrode modified with MXene, and then covalently linking a DNA aptamer. Integrating the excellent conductivity of MXene and the excellent performance of the bovine serum albumin-polyethyleneimine cross-linked coating, the sensor prepared by the present invention can effectively resist unnecessary biological contamination and achieve specific, simple, sensitive and accurate detection of the cancer marker CA125 in real samples. It has been experimentally verified that the interface modified by the bovine serum albumin-polyethyleneimine cross-linked coating has better anti-pollution performance and higher sensitivity than the interface modified by a single bovine serum albumin.

[0048] The prepared biosensor was used to detect the cancer marker CA125, wherein the biosensor was immersed in a solution containing different concentrations of the target, incubated at a constant temperature for not less than 1.5 h, then rinsed with PBS buffer solution to remove the unspecifically captured CA125, and immersed in a [Fe(CN)6] 3- / 4- In the solution, differential pulse voltammetry was used with a voltage range of -0.2V-0.6V to record the changes in electrical signals before and after identifying the target, thereby achieving specific detection of the target CA125. The linear range of detecting the target CA125 was 0.01-1000U / mL, and the detection limit was 2.6mU / mL. Specific embodiment 2:

[0050] like Figure 1-19 As shown, the characterization experiment of BSA-PEI / MXene-CS modified electrode was carried out, and the specific display content is as follows:

[0051] Scanning electron microscopy characterization of the surface morphology of different modified interfaces, specifically as follows Figure 2 As can be seen from the scanning electron microscope image in A, Ti3AlC2 presents a typical dense bulk structure with no gaps between layers. Figure 2 B. After etching with hydrofluoric acid, the Al layer is removed and MXene presents an accordion-like layered structure with obvious gaps. This interesting structure gives MXene a large specific surface area and excellent conductivity. Figure 2 C, after further mixing with chitosan, MXene is stably attached to the interface due to the film-forming effect of chitosan and the electrostatic interaction between CS and MXene. Figure 2 D. After connecting BSA-PEI, there is no obvious bulk structure on the surface, the cross-linked coating is successfully modified on the interface, and the BSA-PEI / MXene-CS modified electrode is successfully prepared.

[0052] XPS characterization of different modified interfaces, specifically, the chemical composition of different modified interfaces was further analyzed by X-ray photoelectron spectroscopy (XPS), such as Figure 3 As shown in A, there are typical peaks of C1s, O1s, Ti2p, and Al2p on the Ti3AlC2 modified interface. Figure 3 B, The typical peak of F1s appears on the MXene-modified interface, and the typical peak of Al2p disappears, which is due to the successful etching of the Al layer by hydrofluoric acid. Figure 3 The appearance of the typical peaks of C and N1s originates from the amino groups on chitosan, proving the successful modification of MXene-CS. Figure 3D. After further modification with BSA-PEI cross-linking coating, typical characteristic peaks of S2s and S2p appeared, and the typical peak of N1s was significantly enhanced, which originated from the disulfide bonds in BSA and the nitrogen-rich characteristics of BSA and PEI, respectively. Specific embodiment three:

[0054] like Figure 1-19 As shown, experiments were performed to characterize BSA-PEI. Figure 4 As shown in the figure, the zeta potential test shows that BSA has a large negative charge (about -18.9 mV), and due to the cationic nature of PEI (about +30.3 mV), the mixed solution of PEI and BSA is close to neutral charge (about -0.59 mV), indicating that the BSA-PEI modified interface has the potential to resist nonspecific protein adsorption. Next, the water contact angle test was used to evaluate the hydrophilicity of the BSA-PEI modified interface. Figure 5 As shown in the figure, due to the hydrophilicity of MXene, the water contact angle decreased to 46.85° compared with the bare electrode (64.68°). After covalent crosslinking with a single bovine serum albumin, the hydrophilicity of the interface decreased significantly, and the water contact angle increased significantly to 72.72°. After crosslinking with BSA-PEI, the water contact angle of the modified interface decreased significantly to 19.69°, indicating that the interface has excellent hydrophilicity and great potential to resist nonspecific protein adsorption. The BSA-PEI modified interface has a great potential to resist nonspecific protein adsorption at different pH values ​​(2, 4, 6, 8) ( Figure 5 B) and salt strength (1MNaCl, CaCl2, MgCl2, Na2SO4) ( Figure 5 After immersing in the solution of C) for 3 h, the water contact angle did not change significantly and the hydrophilicity was still good, indicating that the modified interface has good acid, alkali and salt resistance. Specific embodiment four:

[0056] like Figure 1-19 As shown in the figure, the electrochemical characterization of the anti-fouling electrochemical biosensor based on BSA-PEI cross-linked conductive nanomaterials was carried out. The construction process of the sensor was characterized by electrochemical DPV test. The test was carried out in the presence of a negatively charged probe [Fe(CN)6] 3- / 4- In an iron standard solution, Figure 6As shown, after incubation with MXene-CS, the electrical signal increased significantly due to the large specific surface area and excellent conductivity of MXene. After cross-linking with BSA-PEI coating, the insulating properties of proteins and polymers hindered the electron transfer on the electrode surface to a certain extent, and the electrical signal decreased. It is worth noting that compared with the interface of physically adsorbed BSA and only cross-linked BSA, due to the cross-linking with conductive nanomaterials and the close electrical neutrality of the modified interface, the BSA-PEI cross-linked coating can better maintain the electron transfer to the underlying electrode and has a relatively high electrical signal. After the DNA aptamer and the target are connected in turn, the electron transfer on the electrode surface will be further hindered, and the electrical signal will decrease in turn. The change in the DPV signal illustrates the successful construction of the sensor and the successful detection of the target. Specific embodiment five:

[0058] like Figure 1-19 As shown, the prepared biosensor was subjected to an anti-pollution test as follows:

[0059] The modified interfaces were immersed in human serum of different dilution concentrations for 30 min and in [Fe(CN)6] 3- / 4- DPV test was carried out in the solution, and the changes of electrical signals before and after immersion were recorded, such as Figure 7 As shown, compared with the bare, MXene-CS and BSA / MXene-CS modified interfaces, the BSA-PEI / MXene-CS modified interface can maintain most of the original signals to the greatest extent in different concentrations of human serum. More importantly, as Figure 8 As shown, after immersion in 100% human serum, the signal inhibition rate (signal inhibition rate (%) = (I0-I) / I0, where I0 and I represent the electrical signal values ​​before and after immersion, respectively) was only 10.24%, indicating that the BSA-PEI modified interface can effectively resist nonspecific adsorption and has better anti-fouling performance than a single BSA coating.

[0060] The bare, MXene-CS, BSA / MXene-CS and BSA-PEI / MXene-CS modified interfaces were placed in 0.2 mg / mL FITC-BSA solution and incubated for 2 h in the dark. The adsorption of nonspecific proteins on the different modified interfaces was evaluated using a TCS-SP5 confocal laser microscope. It can be seen that the bare ( Fig. 9 A) MXene-CS Fig. 9 B) and BSA / MXene-CS modified interface ( Fig. 9 C) have obvious green fluorescence, while the BSA-PEI / MXene-CS modified interface ( Fig. 9D) showed almost no fluorescence. Similarly, similar results were obtained by co-culturing with HeLa cells for 24 h and then staining with 50 μg / mL FDA for 5 min. Fig. 9 E) MXene-CS ( Fig. 9 F) and BSA / MXene-CS modified interface ( Fig. 9 G) showed obvious cell adsorption, while the BSA-PEI / MXene-CS modified interface ( Fig. 9 H), indicating that the BSA-PEI modified interface has an excellent ability to resist nonspecific adsorption. Specific embodiment six:

[0062] like Figure 1-19 As shown in the test of the anti-fouling electrochemical biosensor analytical performance based on BSA-PEI cross-linked conductive nanomaterials, the biosensor was immersed in a solution containing different concentrations of the target, incubated at a constant temperature for not less than 1.5 h, and then rinsed with PBS buffer solution to remove the unspecifically captured CA125, and the above electrode was placed in [Fe(CN)6] containing 0.1M KCl 3- / 4- In the solution, differential pulse voltammetry (voltage range -0.2V-0.6V) was used to record the changes in electrical signals before and after identifying the target object, such as Fig.10 As shown in A (ag represents the target CA125 concentration of 0, 0.01, 0.1, 1, 10, 100, 1000 U / mL respectively), as the CA125 concentration increases, the electrical signal gradually decreases, such as Fig.10 As shown in Figure B, within the target detection range of 0.01-1000U / mL, the signal change value (ΔI=I0-I, where I0 and I are the DPV current values ​​before and after identifying the target, respectively) and the logarithm of the target concentration (LgC) show a good linear relationship, and the linear equation is ΔI(μA)=4.28LgC(U / mL)+12.36, with a correlation coefficient R 2 The detection limit (LOD) was 0.999 and 2.6 mU / mL. Specific embodiment seven:

[0064] like Figure 1-19 As shown in the figure, the selectivity test of the anti-fouling electrochemical biosensor based on BSA-PEI cross-linked conductive nanomaterials was performed. The sensor was immersed in solutions containing 10U / mL CA125, 1μg / mL IgG, CEA, HSA, NSE and their mixed solutions for 1.5h, and then the electrode was placed in [Fe(CN)6] 3- / 4- In the solution, the electrical signal changes before and after identification of each protein were recorded by differential pulse voltammetry, such as Fig.11As shown, even when the concentration of the interfering protein is much greater than that of the target protein, only a negligible electrical signal response is generated, indicating that the sensor of the present invention has good selectivity. Specific embodiment eight:

[0066] like Figure 1-19 As shown, the stability test of the anti-fouling electrochemical biosensor based on BSA-PEI cross-linked conductive nanomaterials: the sensor was placed in [Fe(CN)6] 3- / 4- 100 consecutive CV scans were performed in a solution of Fig.12 As shown in A, the electrical signal has no obvious change and has good stability. Specific embodiment nine:

[0068] like Figure 1-19 As shown in the figure, the reproducibility test of the anti-fouling electrochemical biosensor based on BSA-PEI cross-linked conductive nanomaterials was performed. Seven sensors prepared under the same conditions were immersed in a solution containing 10 U / mL CA125, incubated at a constant temperature for no less than 1.5 h, and then rinsed with PBS buffer solution to remove the unspecifically captured CA125. The above electrodes were placed in a [Fe(CN)6] 3- / 4- In the solution, differential pulse voltammetry (voltage range -0.2V-0.6V) was used to record the changes in electrical signals before and after identifying the target. The results are as follows Fig.13 As shown, the relative standard deviation is 3.82%, indicating that the sensor prepared by the present invention has good reproducibility. Specific embodiment ten:

[0070] like Figure 1-19 As shown, the analytical performance of the provided detection method is compared with that of the ELISA detection method, and the sensor prepared by the present invention is used to detect CA125 in actual human serum samples, and the test results are compared with those of the ELISA method, as shown in FIG. Fig.14 As shown, in the detection of five human serum samples, the sensor prepared by the present invention and the ELISA method have basically consistent detection results, and the difference rate is less than 10%, indicating that the sensor prepared by the present invention has great practical application potential. Specific embodiment eleven:

[0072] like Figure 1-19As shown in the figure, in order to obtain the best anti-fouling performance and sensing performance, we optimized some parameters in the sensor construction process (such as PEI concentration, BSA concentration, BSA-PEI cross-linking time, DNA aptamer concentration and target incubation time). We optimized the anti-fouling performance of the sensor based on the change in electrical signal of the BSA-PEI modified interface before and after immersion in 20% human serum for 30 minutes (ΔI=I0-I, I0 and I represent the DPV electrical signal values ​​before and after immersion in 20% human serum, respectively). The smaller the change in electrical signal, the better the anti-fouling performance of the modified interface. Fig.15 As shown in Figure 2, when the PEI concentration increases from 0.5wt% to 3wt%, the change in the electrical signal decreases. When the concentration increases further, the change in the electrical signal increases. Therefore, 3wt% is selected as the optimal PEI concentration. Similarly, Fig.16 As shown, 1 mg / mL was selected as the optimal BSA concentration; Fig.17 As shown, 16 h was selected as the optimal BSA-PEI cross-linking time. Next, in order to obtain the best sensing performance, the concentration of DNA aptamers and the target incubation time were optimized, as shown in Fig.18 As shown in the figure, when the aptamer concentration reaches 1 μM, the decrease value of the electrical signal no longer increases with the increase of the aptamer concentration, and the interface binding amount reaches saturation. Therefore, 1 μM is selected as the optimal aptamer concentration. Similarly, 90 min is selected as the optimal target incubation time.

[0073] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "comprising a reference structure" do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A biosensor based on bovine serum albumin-polyethyleneimine material, comprising a BSA solution, a PEI solution, a nanomaterial MXene and a DNA aptamer, characterized in that: The BSA solution and the PEI solution are covalently cross-linked to a glassy carbon electrode modified with a conductive nanomaterial MXene, and then covalently linked to a DNA aptamer to prepare a sensor. The preparation method of the sensor is as follows: Sp1: Electrode pretreatment, after the prepared MXene is evenly mixed with the CS solution, it is drop-coated on the pretreated bare glassy carbon electrode and dried naturally at room temperature to obtain a MXene-CS modified electrode, wherein the prepared MXene is Ti 3C2Tx MXene powder, the mass fraction of the CS solution is 0.2%, and the mixing ratio of the prepared MXene and CS solution is 1:2; Sp2: Preparation of BSA-PEI / MXene-CS modified electrode, the MXene-CS modified electrode is activated by glutaraldehyde, and then immersed in a mixed solution of BSA and PEI to obtain a BSA-PEI / MXene-CS modified electrode, wherein the BSA solution and the PEI solution are bovine serum albumin solution and polyethyleneimine solution, respectively, and the CS solution is a chitosan solution; Sp3: Molding preparation of the sensor, the BSA-PEI / MXene-CS modified electrode is immersed in a DNA aptamer solution activated by EDC and NHS solution to obtain a sensor, wherein the EDC solution is a 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride solution, and the NHS solution is an N-hydroxysuccinimide solution.

2. The biosensor based on bovine serum albumin-polyethyleneimine material according to claim 1, characterized in that: During the electrode pretreatment process, 8 mg Ti3AlC2 powder was slowly added to a 32 mL hydrofluoric acid solution with a mass fraction of 40%, and stirred continuously at high speed for 48 h at room temperature. The material was then repeatedly washed with secondary water and anhydrous ethanol and centrifuged until the supernatant reached a pH ≥ 6. The precipitate was then vacuum dried at 60 ° C for 12 h to obtain Ti3C2T x MXene powder was dissolved by ultrasonic treatment in secondary water and then mixed evenly with 0.2% CS solution in a volume ratio of 1:

2. Then 20 μL was drop-coated on the pretreated bare glassy carbon electrode and dried naturally at room temperature.

3. The biosensor based on bovine serum albumin-polyethyleneimine material according to claim 1, characterized in that: In the preparation of the BSA-PEI / MXene-CS modified electrode, the amino groups on the MXene-CS modified electrode were activated with 5% glutaraldehyde for 50 minutes, and then immersed in a mixed solution of BSA and PEI to react at room temperature for 16 hours. After the reaction was completed, it was rinsed with water twice to remove the BSA-PEI that was not covalently cross-linked, thereby obtaining a BSA-PEI / MXene-CS modified electrode.

4. The biosensor based on bovine serum albumin-polyethyleneimine material according to claim 1, characterized in that: In the molding preparation of the sensor, the carboxyl group on the DNA aptamer is first activated with an EDC / NHS solution for 0.5 h, and then the BSA-PEI / MXene-CS modified electrode is immersed in a DNA aptamer solution of not less than 1 μM and reacted at room temperature for 2 h. After the reaction is completed, it is rinsed with secondary water to remove the unfixed DNA aptamer to obtain the sensor.

5. The biosensor based on bovine serum albumin-polyethyleneimine material according to claim 3, characterized in that: In the mixed solution of BSA and PEI used in the preparation of the BSA-PEI / MXene-CS modified electrode, the concentration of BSA was 1 mg / mL, and the mass percentage of PEI was 3 wt%.