A lignin carbon / zinc oxide nanocomposite material and its preparation and application
By using flower-like lignin carbon/zinc oxide nanocomposites in photocatalysts, the problems of narrow light absorption range of zinc oxide and slow photogenerated carrier transfer are solved, which significantly improves the degradation efficiency of organic pollutants and achieves woody High value utilization of the stock.
Patent Information
- Application Number
- CN202310993722.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-08-09
AI Technical Summary
The existing photocatalyst zinc oxide is difficult to efficiently degrade organic dye pollutants due to the narrow light absorption range, slow photogenerated carrier transfer and low recombination rate.
Lignon is used as a surfactant and carbon source to prepare flower-like lignin carbon/zinc oxide nanocomposites through high-temperature calcination to broaden the light absorption range of zinc oxide and improve the photoelectron transfer capability.
It significantly improves the photocatalytic performance, enhances the degradation efficiency of organic pollutants, solves the defect problem of zinc oxide, and promotes the high-value utilization of lignin.
Smart Images

Figure BDA0004383900280000101 
Figure BDA0004383900280000111 
Figure HDA0004383900290000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic / inorganic hybrid composite materials, and specifically relates to a flower-like lignin carbon / zinc oxide nanocomposite material and a preparation method and application thereof. Background Art
[0002] Dye wastewater is a characteristic organic polluted wastewater with the characteristics of high organic concentration, strong toxicity, and difficulty in degradation, which will seriously affect the ecological environment. Therefore, the treatment of organic wastewater is imminent. After research, people have found that methods for degrading organic matter include microbial degradation of organic matter, advanced oxidation technology, etc. However, these methods have disadvantages such as low catalytic efficiency, difficulty in recycling, high cost, and secondary pollution. With the continuous improvement of people's research and treatment methods, advanced oxidation processes (AOPs) have been paid attention to as an alternative to traditional treatment methods. AOPs mainly include: photocatalytic oxidation, electrochemical oxidation, ozone oxidation, Fenton oxidation, and catalytic wet oxidation. Among these methods, photocatalytic oxidation has a good effect on removing difficult-to-degrade organic matter, and has the advantages of mild reaction conditions, no secondary pollution, non-toxic and harmless, low energy consumption, stable catalysts and recyclable utilization, which has attracted the attention of scientists. Photocatalysis is the energy of the charge-carrier pairs generated by photons is equal to or greater than the band gap energy. Due to this change in energy, electrons and holes are formed, hydroxides and other free radicals are generated, which are used to decompose organic pollutants. Among them, nano ZnO material has become a semiconductor photocatalytic material with great research value due to its high quantum efficiency, wide source of raw materials, diverse preparation methods, excellent photocatalytic effect, and non-toxicity.
[0003] As a new II-VI semiconductor material, ZnO has unique photoelectric properties and chemical and thermal stability, but the various defects in ZnO will definitely have an important impact on its properties. There are six main intrinsic defects in ZnO: oxygen vacancies, V O , Zn vacancy V Zn , oxygen interstitial O i , zinc interstitial Zn i , anti-oxygen O Zn , anti-zinc Zn O Among them, V O 、Zn i and Zn O is a donor defect, V Zn , O i and O Zn is an acceptor defect. O 、Zn iThese two defects are considered to be the main reasons why intrinsic zinc oxide is an n-type semiconductor. Therefore, it is often necessary to improve the corresponding performance by other modification methods such as loading with some substances or doping with certain concentrations of specific elements.
[0004] Lignin is the second largest biomass resource in the plant kingdom after cellulose in terms of reserves. There are active groups such as aromatic groups, phenolic hydroxyl groups, alcoholic hydroxyl groups, and carbon-based conjugated double bonds in the molecular structure of lignin. Therefore, it can undergo many chemical reactions such as oxidation, reduction, demethoxylation, carboxylation, sulfonation, alkylation, halogenation, nitration, polycondensation or graft copolymerization, and has broad development prospects. Among them, alkali lignin mainly comes from papermaking black liquor, which is highly alkaline, dark in color, has a strong odor, a lot of foam, and seriously consumes dissolved oxygen in the water. If it is allowed to be discharged, a large amount of organic matter and residual alkali will be discharged into rivers and lakes with wastewater, seriously polluting the environment, wasting the country's precious resources, and causing great harm to industrial, agricultural, fishery production and people's health. The black liquor must be treated and the solids in the black liquor must be recovered at the same time. Therefore, it is very meaningful to utilize the large amount of alkali lignin in the black liquor. Alkali lignin is an anionic organic compound with both hydrophilic and hydrophobic parts, so it has the function of anionic surfactant. Combining the characteristics of alkali lignin with zinc oxide can not only make up for the defects of zinc oxide but also promote its advantages. It can also solve the environmental problems of alkali lignin and make high-value use of lignin. Summary of the invention
[0005] In order to overcome the shortcomings of zinc oxide in the prior art, such as narrow light absorption range of photocatalyst, slow transfer of photogenerated carriers and high recombination rate, the primary purpose of the present invention is to provide a method for preparing a flower-like lignin carbon / zinc oxide nanocomposite material.
[0006] The present invention uses lignin as a surfactant and a carbon source, and prepares lignin carbon / zinc oxide nanocomposites with different morphologies and high catalytic performance by calcining at high temperature in two steps. The process is simple, the raw materials are readily available, and the cost is low.
[0007] Another object of the present invention is to provide a flower-like lignin carbon / zinc oxide nanocomposite material prepared by the above preparation method.
[0008] Another object of the present invention is to provide application of the above-mentioned flower-like lignin carbon / zinc oxide nanocomposite material in the field of photocatalysis.
[0009] The purpose of the present invention is achieved through the following technical solutions:
[0010] A method for preparing a flower-like lignin carbon / zinc oxide nanocomposite material comprises the following steps:
[0011] (1) mixing a lignin alcohol solution and a zinc salt aqueous solution uniformly, adding a precipitant solution dropwise, adding water, heating for reaction, washing, and drying to obtain a lignin carbon / zinc oxide nanocomposite precursor;
[0012] (2) calcining the lignin carbon / zinc oxide nanocomposite material precursor to obtain a flower-shaped lignin carbon / zinc oxide nanocomposite material.
[0013] Preferably, the lignin in step (1) is at least one of alkali lignin, sulfate lignin, lignin sulfonate and enzymatically hydrolyzed lignin.
[0014] Preferably, in step (1), the ratio of lignin to zinc salt is (0.5-2.0) g: (0-10) mmol, and the zinc salt is not 0; more preferably (0.5-2.0) g: 10 mmol; further preferably (1.5-2.0) g: 10 mmol; and most preferably 2.0 g: 10 mmol.
[0015] Preferably, the concentration of the lignin alcohol solution in step (1) is 12.5 to 50 mg / mL; more preferably 37.5 to 50 mg / mL; most preferably 50 mg / mL.
[0016] Preferably, the alcohol solvent in the lignin alcohol solution in step (1) is anhydrous ethanol.
[0017] Preferably, the concentration of the zinc salt aqueous solution in step (1) is 0.5 to 1 mol / L.
[0018] Preferably, the zinc salt in step (1) is at least one of zinc nitrate, zinc acetate, zinc carbonate, zinc chloride and zinc oxalate; more preferably zinc nitrate.
[0019] Preferably, the precipitant solution in step (1) is at least one of aqueous ammonia, potassium hydroxide solution and sodium hydroxide solution; more preferably sodium hydroxide solution; the concentration of the precipitant solution is 4 to 8 mol / L; further preferably 4 to 6 mol / L; most preferably 6 mol / L.
[0020] Preferably, the molar ratio of the precipitant to the zinc salt in step (1) is 4 to 8:1; more preferably 4 to 6:1; most preferably 6:1.
[0021] Preferably, the volume ratio of the water added in step (1) to the precipitant solution is (0-80):10, and the volume of water is not 0.
[0022] Preferably, the temperature of the heating reaction in step (1) is 60-100°C, more preferably 60-80°C, more preferably 60-70°C, and most preferably 70°C; the time is 20-60 min, more preferably 20-40 min, more preferably 30-40 min, and most preferably 30 min.
[0023] Preferably, the washing in step (1) refers to washing the mixed solution of the heated reaction products with deionized water and anhydrous ethanol after centrifugation; more preferably, washing with deionized water and anhydrous ethanol 1 to 5 times each.
[0024] Preferably, the drying in step (1) is conventional drying.
[0025] Preferably, the calcination temperature in step (2) is 450-550°C, more preferably 500-550°C, most preferably 550°C; the calcination time is 1-3h, most preferably 1h.
[0026] Preferably, the calcination atmosphere in step (2) is at least one of nitrogen, ammonia and air; preferably nitrogen.
[0027] The method is used to prepare a flower-like lignin carbon / zinc oxide nanocomposite material.
[0028] The application of the above-mentioned flower-like lignin carbon / zinc oxide nanocomposite material in the field of photocatalysis.
[0029] Preferably, the application is photocatalytic degradation of organic dye pollutants in wastewater.
[0030] The present invention provides a multi-morphological lignin carbon / zinc oxide nanocomposite material prepared by the above method. The composite material has the advantages of multi-morphology, large specific surface area, etc., and is applied to the field of photocatalysis, especially to the photocatalytic degradation of organic dye pollutants in wastewater, and its photocatalytic performance can be significantly improved. The present invention combines the characteristics of lignin with zinc oxide, which can not only make up for the defects of zinc oxide but also promote its advantages, and can also solve the environmental problems of lignin, and make high-value use of lignin, and the process method is simple, the raw materials are easily available and the cost is low.
[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0032] The present invention uses lignin as a carbon source and surfactant to change the interfacial energy of water and anhydrous ethanol, and improves the mutual self-assembly ability of lignin and zinc oxide in liquid; at the same time, the loading of carbon and zinc oxide broadens the light absorption range of zinc oxide and improves the transfer ability of photoelectrons; the unique flower-like morphology increases the specific surface area of the material, enhances its photocatalytic ability, and solves the defects of zinc oxide as a semiconductor photocatalyst, such as narrow light absorption range, slow transfer of photogenerated carriers, and high recombination rate. The material is applied to the field of photocatalysis, especially photocatalytic degradation of organic pollutants, which can significantly improve its degradation efficiency and has potential application value in the field of photocatalytic organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 These are scanning electron microscope images of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 1.
[0034] Figure 2 These are scanning electron microscope images of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 2.
[0035] Figure 3 These are scanning electron microscope images of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 3.
[0036] Figure 4 These are scanning electron microscope images of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 4.
[0037] Figure 5 These are scanning electron microscope images of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 5.
[0038] Figure 6 This is the EDS spectrum of the lignin carbon / zinc oxide nanocomposite prepared by calcining at 550°C in Example 1.
[0039] Figure 7 This is the mapping diagram of the lignin carbon / zinc oxide nanocomposite material prepared by calcination at 550°C in Example 1.
[0040] Figure 8 The thermogravimetric diagram of the lignin carbon / zinc oxide nanocomposite material prepared by calcining at 550° C. in Comparative Example 1 and Example 1.
[0041] Fig. 9 The X-ray diffraction patterns of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 1.
[0042] Fig.10 The X-ray diffraction patterns of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 2 are shown.
[0043] Fig.11 The X-ray diffraction patterns of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 3.
[0044] Fig.12 The X-ray diffraction patterns of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 4 are shown.
[0045] Fig.13 The X-ray diffraction patterns of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 5 are shown.
[0046] Fig.14 These are the experimental results of the concentration variation of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposites prepared in Examples 1 to 5 for the photocatalytic degradation of methylene blue.
[0047] Fig.15 The experimental results of the concentration change of the zinc oxide nanomaterial prepared in Comparative Example 1 and the lignin carbon / zinc oxide nanocomposite material prepared in Example 1-500°C for the photocatalytic degradation of methylene blue. DETAILED DESCRIPTION
[0048] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0049] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially.
[0050] Comparative Example 1
[0051] Prepare 10 ml of 6 mol / L sodium hydroxide solution and 20 ml of 0.5 mol / L zinc nitrate hexahydrate solution, add the prepared sodium hydroxide solution dropwise into the zinc salt solution and then add 80 ml of water, then put the mixture into a water bath and heat it at 70°C for 30 min, then remove the reacted mixture by centrifugation, wash it with deionized water and anhydrous ethanol for 3 times each, dry it overnight to obtain a zinc oxide precursor, then put the precursor into a tubular furnace, calcine it at 550°C for 1 h under a nitrogen atmosphere, and cool it to room temperature to obtain zinc oxide nanomaterials.
[0052] Example 1
[0053] 2.0 g of alkali lignin was added to 40 ml of anhydrous ethanol, and magnetically stirred at room temperature for 2 hours. Then, 10 ml of 6 mol / L sodium hydroxide solution and 20 ml of 0.5 mol / L zinc nitrate hexahydrate solution were prepared. The zinc salt solution was added to the mixture of alkali lignin and ethanol. After stirring for 10 minutes, the prepared sodium hydroxide solution was added dropwise and then 80 ml of water was added. The mixture was placed in a water bath and heated at 70°C for 30 minutes. The reacted mixture was removed by centrifugation, washed with deionized water and anhydrous ethanol for 3 times each, and dried overnight to obtain a lignin carbon / zinc oxide nanocomposite precursor. The precursor was placed in a tubular furnace and calcined at 400°C, 450°C, 500°C, 550°C and 600°C for 1 hour under a nitrogen atmosphere. The mixture was cooled to room temperature to obtain flower-like lignin carbon / zinc oxide nanocomposites obtained at 5 different calcination temperatures.
[0054] Example 2
[0055] 2.0 g of alkali lignin was added to 40 ml of anhydrous ethanol and magnetically stirred at room temperature for 2 h. Then, 10 ml of 4 mol / L, 10 ml of 6 mol / L, 10 ml of 8 mol / L and 10 ml of 10 mol / L sodium hydroxide solution and 20 ml of 0.5 mol / L zinc nitrate hexahydrate solution were prepared respectively. The zinc salt solution was added to the mixture of alkali lignin and ethanol. After stirring for 10 min, the prepared sodium hydroxide solutions of different concentrations were added dropwise and then 80 ml of water was added. The mixture was placed in a water bath and heated at 70 ° C for 30 min. The reacted mixture was removed and centrifuged, washed with deionized water and anhydrous ethanol for 3 times each, and dried overnight to obtain a lignin carbon / zinc oxide nanocomposite precursor. The precursor was placed in a tubular furnace and calcined at 550 ° C for 1 h under a nitrogen atmosphere. It was cooled to room temperature to obtain 4 lignin carbon / zinc oxide nanocomposites with different morphologies.
[0056] Example 3
[0057] 0.5g, 1.0g, 1.5g and 2.0g of alkali lignin were added to 40ml of anhydrous ethanol respectively, and magnetically stirred for 2h at room temperature. Then, 10ml of 6mol / L sodium hydroxide solution and 20ml of 0.5mol / L zinc nitrate hexahydrate solution were prepared. The zinc salt solution was added to the mixed solution of alkali lignin and ethanol in different amounts, stirred for 10min, and then the prepared sodium hydroxide solution was added dropwise, and then 80ml of water was added. The mixture was placed in a water bath and heated at 70℃ for 30min. The reacted mixture was removed and centrifuged, washed with deionized water and anhydrous ethanol for 3 times each, and dried overnight to obtain a lignin carbon / zinc oxide nanocomposite precursor. The precursor was placed in a tubular furnace, calcined at 550℃ for 1h under a nitrogen atmosphere, and cooled to room temperature to obtain 4 lignin carbon / zinc oxide nanocomposites with different morphologies.
[0058] Example 4
[0059] 2.0 g of alkali lignin was added to 40 ml of anhydrous ethanol, and magnetically stirred at room temperature for 2 hours. Then, 10 ml of 6 mol / L sodium hydroxide solution and 20 ml of 0.5 mol / L zinc nitrate hexahydrate solution were prepared. The zinc salt solution was added to the mixture of alkali lignin and ethanol, and after stirring for 10 minutes, the prepared sodium hydroxide solution was added dropwise, and then 80 ml of water was added. The mixture was placed in a water bath and heated in a water bath at 60°C, 70°C, 80°C, 90°C and 100°C for 30 minutes, respectively. The reacted mixture was removed by centrifugation, washed with deionized water and anhydrous ethanol for 3 times each, and dried overnight to obtain a lignin carbon / zinc oxide nanocomposite precursor. The precursor was placed in a tubular furnace, calcined at 550°C for 1 hour under a nitrogen atmosphere, and cooled to room temperature to obtain 5 lignin carbon / zinc oxide nanocomposites with different morphologies.
[0060] Example 5
[0061] 2.0 g of alkali lignin was added to 40 ml of anhydrous ethanol and magnetically stirred at room temperature for 2 h. Then, 10 ml of 6 mol / L sodium hydroxide solution and 20 ml of 0.5 mol / L zinc nitrate hexahydrate solution were prepared. The zinc salt solution was added to the mixture of alkali lignin and ethanol. After stirring for 10 min, the prepared sodium hydroxide solution was added dropwise and then 80 ml of water was added. The mixture was placed in a water bath and heated at 70 ° C for 20 min, 30 min, 40 min, 50 min and 60 min respectively. The reacted mixture was removed by centrifugation, washed with deionized water and anhydrous ethanol for 3 times each, and dried overnight to obtain a lignin carbon / zinc oxide nanocomposite precursor. The precursor was placed in a tubular furnace and calcined at 550 ° C for 1 h in a nitrogen atmosphere. It was cooled to room temperature to obtain 5 lignin carbon / zinc oxide nanocomposites with different morphologies.
[0062] Figure 1 These are SEM images of the materials prepared in comparative example 1 and example 1. Figure a is the material prepared in comparative example 1. It can be seen that the morphology of the nano zinc oxide prepared without adding lignin is in the shape of flower flakes, and the thickness of the flakes is relatively large and unevenly distributed; Figure bf is the material prepared in example 1, which is calcined at different temperatures of 400°C, 450°C, 500°C, 550°C and 600°C. From Figure bf, it can be seen that with the increase of calcination temperature, it can be seen that the lignin carbon / zinc oxide nanocomposite material grows from the previous irregular thick flakes to thin regular petals, especially Figure e. The morphology of the lignin carbon / zinc oxide nanocomposite material prepared in example 1 is the most regular, like a blooming rose; although the lignin carbon / zinc oxide nanocomposite materials prepared at other calcination temperatures are regular, there are still some blocky materials on the surface, and their "blooming" degree is not as good as Figure e.
[0063] Figure 2 These are SEM images of the materials prepared in Comparative Example 1 and Example 2. Figure a is the material prepared in Comparative Example 1, and Figure be is the material prepared in Example 2, which are the materials prepared at 4 mol / L, 6 mol / L, 8 mol / L, and 10 mol / L, respectively. It can be seen that as the amount of precipitant NaOH increases, the catalyst changes from the previous thorn-like shape to the petal-like shape and finally to the agglomerated rod-like shape. It can be seen that the concentration of the precipitant base in the solution has a significant effect on the growth morphology of the material.
[0064] Figure 3 The SEM images of the materials prepared in Comparative Example 1 and Example 3 are shown in Figure a. Figure a is the material prepared in Comparative Example 1, and Figure b is the material prepared in Example 3, which are 0.5g, 1.0g, 1.5g and 2.0g of alkali lignin, respectively. The amount of alkali lignin has a great influence on the morphology of the material. When the amount of alkali lignin is not large, the unique flower-like morphology of the sample cannot be formed. As the amount of alkali lignin increases, the sample begins to form a flower shape, and finally becomes a regular and unique rose-shaped lignin carbon / zinc oxide nanocomposite material.
[0065] Figure 4 These are SEM images of the materials prepared in Comparative Example 1 and Example 4. Figure a is the material prepared in Comparative Example 1, and Figures bf are the materials prepared in Example 4, which are materials prepared at 60°C, 70°C, 80°C, 90°C and 100°C, respectively. As can be seen from the figure, the energy of temperature increase is more direct, resulting in more obvious changes in the material's flake shape. As the temperature increases, the sample grows from a standard flower-like shape (Figure c) to an irregular flake-like shape (Figure de). Figure f shows that some of the material has grown into agglomerated blocks.
[0066] Figure 5The SEM images of the materials prepared in Comparative Example 1 and Example 5 are shown in Figure a. Figure bf is the material prepared in Example 5, and the materials prepared in 20min, 30min, 40min, 50min and 60min, respectively. As the reaction time increases, the material continues to gain energy and gradually grows from the rose-shaped shape of the initial specification to irregular flakes. These features may be due to the excessive surface area of the flakes during the growth process, and the flakes are squeezed against each other, resulting in breakage and irregular flakes and thorns.
[0067] Figure 6 and Figure 7 The following are the EDS scanning analysis and mapping analysis diagrams of the sample calcined at 550°C in Example 1. Figure 6 It can be seen that carbon is distributed on the surface of the sample, and the distribution of Zn and O conforms to the law of ZnO.
[0068] Figure 8 It is the TG characterization diagram of the samples calcined at 550°C in Comparative Example 1 and Example 1. From the figure, it can be seen that the thermal stability of the material is very good, only 9.63% is lost at about 550°C, and the material prepared in Comparative Example 1 only loses 2.71% at about 520°C. Through the TG of alkali lignin AL, it can be seen that the alkali lignin loses a lot during calcination, but the mass loss is reduced after the alkali lignin and the material are composited and fired, which is due to the unique thermal conductivity of ZnO.
[0069] Figures 9 to 13 This is the XRD spectrum of the prepared material. It can be seen from the figure that the zinc oxide in the prepared composite material is a typical hexagonal wurtzite crystal structure, and the crystal peak intensity of the material is relatively high. The results show that in the preparation of the hybrid process, alkali lignin did not change the nanostructure crystal form of zinc oxide.
[0070] Fig.14 It is a photocatalytic performance diagram of the materials of comparative example 1 and examples 1 to 5. The target degradation product of this photocatalysis is a 30mg / L methylene blue solution. Take 50ml of the target degradation product, add 50mg of catalyst, and after 30min of dark reaction to reach adsorption equilibrium, turn on the mercury lamp, take out the solution every 10 minutes to measure its concentration, and at the same time put a group of blank control comparison tests without adding any catalyst. The experimental results show that the lignin carbon / zinc oxide nanocomposite material prepared by calcining at 550℃ in Example 1 has high absorption of ultraviolet light. Combined with Table 1, the lignin carbon / zinc oxide nanocomposite material prepared by calcining at 550℃ in Example 1 can degrade more than 98% of the target product in about 10min, and has excellent adsorption performance for pollutants in the dark reaction stage.
[0071] Fig.15The ultraviolet absorption spectra and concentration change experimental effect diagram of the photocatalytic degradation of methylene blue solution by the materials prepared in comparative example 1 and example 1-550℃. The degradation target in this experiment is a 12mg / L methylene blue solution. The specific operation is: take 100ml of a methylene blue solution with a concentration of 12mg / L, add 50mg of a catalyst; after a dark reaction of 30min to reach adsorption equilibrium, turn on the mercury lamp, and take out the solution every 10 minutes to measure its concentration. It can be seen from the figure that in about 10min, the material prepared in example 1-550℃ degraded 99% of methylene blue, while the material prepared in comparative example 1 only degraded 89% of methylene blue.
[0072] Table 1 Degradation degree of organic matter in water by materials obtained from comparative examples and examples (%)
[0073]
[0074]
[0075] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a lignin carbon / zinc oxide nanocomposite material, characterized in that: The following steps are involved: (1) mixing the lignin alcohol solution and the zinc salt aqueous solution uniformly, adding the precipitant solution dropwise, and then adding water, heating at 60-80° C. for reaction for 20-60 min, washing, and drying to obtain a lignin carbon / zinc oxide nanocomposite material precursor; (2) calcining the lignin carbon / zinc oxide nanocomposite material precursor at 450-550° C. for 1-3 h to obtain a flake-shaped lignin carbon / zinc oxide nanocomposite material; In step (1), the ratio of lignin to zinc salt is (1.5-2.0) g:10 mmol; The molar ratio of the precipitant to the zinc salt in step (1) is 4 to 8:1; The concentration of the precipitant solution in step (1) is 4 to 8 mol / L; The precipitant solution in step (1) is at least one of aqueous ammonia, potassium hydroxide solution and sodium hydroxide solution; The lignin in the lignin alcohol solution in step (1) is at least one of alkali lignin, sulfate lignin, lignin sulfonate and enzymatic lignin; The alcohol solvent in the lignin alcohol solution in step (1) is anhydrous ethanol.
2. The method for preparing a lignin carbon / zinc oxide nanocomposite material according to claim 1, characterized in that: The heating reaction time in step (1) is 20 to 40 minutes; The calcination temperature in step (2) is 500-550°C.
3. The method for preparing a lignin carbon / zinc oxide nanocomposite material according to claim 1, characterized in that: The molar ratio of the precipitant to the zinc salt in step (1) is 4 to 6:
1.
4. The method for preparing a lignin carbon / zinc oxide nanocomposite material according to claim 2, characterized in that: The heating reaction temperature in step (1) is 60-70°C and the reaction time is 30-40 minutes; The calcination temperature in step (2) is 550°C; The calcination time in step (2) is 1 h.
5. The method for preparing a lignin carbon / zinc oxide nanocomposite material according to claim 1, characterized in that: The concentration of the lignin alcohol solution in step (1) is 12.5-50 mg / mL; The concentration of the zinc salt aqueous solution in step (1) is 0.5 to 1 mol / L; The zinc salt in step (1) is at least one of zinc nitrate, zinc acetate, zinc carbonate, zinc chloride and zinc oxalate.
6. The method for preparing a lignin carbon / zinc oxide nanocomposite material according to claim 5, characterized in that: The concentration of the precipitant solution in step (1) is 4 to 6 mol / L; The concentration of the lignin alcohol solution in step (1) is 37.5-50 mg / mL.
7. The method for preparing a lignin carbon / zinc oxide nanocomposite material according to claim 1, characterized in that: The volume ratio of the water added in step (1) to the precipitant solution is (0-80):10, and the volume of water is not 0; The calcination atmosphere in step (2) is at least one of nitrogen, ammonia and air.
8. A lignin carbon / zinc oxide nanocomposite material obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the lignin carbon / zinc oxide nanocomposite material according to claim 8 in the field of photocatalysis.